WS2 / h-BN field effect transistor based on interface defect charge long-term storage and preparation method thereof

By introducing ultraviolet light processing and mechanical peeling technology into WS2/h-BN field effect transistors, the problem of unclear interface of two-dimensional materials is solved, long-term storage of charge and multi-state distinction are realized, and the photoelectric performance of the device is improved. Next-generation memory provides application pathways.

CN118983344APending Publication Date: 2024-11-19NORTHEAST NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411214577.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing two-dimensional material field effect transistors have challenges in material preparation, device construction processes and performance development, especially the unclear interface between traditional oxide semiconductors and two-dimensional materials, which affects their performance indicators and is difficult to achieve long-term storage of charges. .

Method used

Using WS2/h-BN field effect transistors based on interface defects, the ability of two-dimensional interface to store charges is enhanced through ultraviolet light treatment, and the devices are prepared in combination with mechanical peeling and thermal evaporation technology to ensure silicon/silica substrate and hexagonal nitriding. The tight bond between boron and molybdenum disulfide and the metal electrodes achieve long-term storage of charge.

Benefits of technology

It realizes the efficient charge storage and memory function of the two-dimensional material interface. By adjusting the power and electrical processing of ultraviolet light processing, the device's photoelectric performance and multi-state distinction capabilities are significantly improved, and is suitable for image encryption and memory applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983344A_ABST
    Figure CN118983344A_ABST
Patent Text Reader

Abstract

The invention discloses a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges and a preparation method of the WS2 / h-BN field effect transistor. The invention discloses a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges. The WS2 / h-BN field effect transistor comprises a silicon / silicon dioxide substrate, a WS2 / h-BN heterojunction, a metal electrode and a device channel, the silicon / silicon dioxide substrate is used as a carrier of the lowermost layer, and the commercial two-dimensional WS2 and h-BN body materials are subjected to previous stripping and transferring by utilizing PDMS (Polydimethylsiloxane). Wherein ultraviolet light treatment is introduced and is used for enhancing the charge storage capacity of a two-dimensional interface and the defect density of a unit area. According to the method, the long-term efficient memory of the two-dimensional image is realized by changing the ultraviolet light processing power and combining later electrical processing and characterization, and the method can be used for functional development of image encryption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of field effect transistors, and specifically relates to a WS2 / h-BN field effect transistor based on interface defects that can realize long-term charge storage and a preparation process thereof. Background Art

[0002] As a hot research direction for next-generation electronic devices, two-dimensional material field-effect transistors have made significant progress in the fields of integrated circuits and electrical storage in recent years. Two-dimensional materials such as graphene, molybdenum disulfide, tungsten disulfide (WS2), boron nitride (h-BN), etc., have shown great potential in building high-performance transistors due to their unique mechanical and optoelectronic properties. These materials have advantages such as atomic thinness and high carrier mobility, which help to reduce short channel effects and comprehensively improve the optoelectronic performance of devices. At present, the research on two-dimensional material field-effect transistors mainly revolves around the following aspects. 1. Material preparation and property regulation, such as preparing large-area single-layer graphene by chemical vapor deposition, and obtaining high-quality molybdenum disulfide and tungsten disulfide by mechanical exfoliation; 2. Optimization of device construction process, including miniaturization of gate length to sub-nanometer level, optimization of electrode contact to quantum limit, etc.; 3. Development of high-quality dielectric layer to solve key technical problems such as unclear interface between traditional oxide semiconductors and two-dimensional materials, such as the atomically thin single-crystalline aluminum oxide prepared recently as top gate dielectric, which significantly improves the performance indicators of two-dimensional material field effect transistors; 4. Exploration of new architectures and integration methods, such as heterogeneous integration technology, combining two-dimensional materials with traditional silicon-based circuits to achieve higher-performance electronic devices. In addition, the band gap size of two-dimensional materials has an important influence on the performance of transistors: by regulating the band gap of the material, the key performance parameters of the device such as the switching ratio, conductivity, energy consumption and operating frequency can be optimized. For example, methods such as introducing defects or external fields can effectively regulate the band gap of two-dimensional materials to improve the performance of FETs. It can be seen that the research on two-dimensional material field effect transistors is in a rapid development stage, and it is expected to be widely used in high-performance electronic devices, flexible electronics, photoelectric sensors and other fields in the future. However, to realize the commercial application of integrated circuits based on 2D semiconductors, continuous efforts are needed in material preparation, device construction process, performance and function development, and continuous exploration of new materials and architectures. Summary of the invention

[0003] The purpose of the present invention is to effectively solve the above-mentioned scientific and technological problems currently faced, and to provide a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges and a preparation method thereof.

[0004] The WS2 / h-BN field effect transistor based on long-term storage of interface defect charges comprises, from bottom to top, a silicon / silicon dioxide substrate, a hexagonal boron nitride two-dimensional thin layer, a WS2 two-dimensional thin layer, and two metal electrodes; the upper surface of the hexagonal boron nitride two-dimensional thin layer and the lower surface of the WS2 two-dimensional thin layer have been subjected to ultraviolet exposure treatment;

[0005] The UV exposure treatment has a power of 0-60 microwatts, a UV wavelength of 265 nm, and a duration of 10 minutes;

[0006] The substrate is 1 cm×1 cm and has a 280nm oxide layer; the overlapping area of ​​the hexagonal boron nitride two-dimensional thin layer and the WS2 two-dimensional thin layer is greater than 4 square microns;

[0007] The metal electrodes are two gold electrodes with a thickness of 50 nm which are deposited by thermal evaporation.

[0008] The invention relates to a method for preparing a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges, which comprises:

[0009] 1) Substrate cutting:

[0010] a. Mark the straight cutting edge of the commercial silicon / silicon dioxide substrate with a plastic plate and divide it into 1 cm×1 cm substrate units;

[0011] b. Use a sapphire glass cutter to cut along a 1 cm × 1 cm straight edge with a force of 100 N.

[0012] c. Keep the substrate horizontal and use vertical force to bend it along the vertical edge with a force of 200 N until the substrate is separated into two pieces along the straight edge.

[0013] d. Repeat the above steps ac for the four edges of the square unit substrate

[0014] 2) Preparation of lower layer h-BN material and UV exposure treatment

[0015] a. Place the commercial h-BN bulk material on the PDMS film, take a piece of PDMS film, stick the two together, and apply a pressure of 50 N to the upper layer so that the two are tightly bonded;

[0016] b. Take the upper PDMS film with the material attached and transfer it to the square unit substrate;

[0017] c. After heating the whole to 120°C and maintaining for 10 minutes, remove the upper PDMS film. At this time, the h-BN adhered to the upper PDMS film has been completely transferred to the unit substrate;

[0018] d. Place the substrate containing h-BN in UV exposure for 10 minutes at a power of 0-60 μW. The wavelength of the UV light used for exposure is 265 nm and the light source type is LED light source.

[0019] 3) Preparation of upper WS2 material and UV exposure treatment

[0020] a. Place the commercial WS2 bulk material on the PDMS film, take a piece of PDMS film, paste the two face to face, and apply a pressure of 100 N to the upper layer so that the two are tightly combined;

[0021] b. Take the PDMS film with WS2 material on the upper layer and expose it to UV light. The exposure power is 10 minutes, the power is 0-60 microwatts, the wavelength of UV light used for exposure is 265 nm, and the light source type is LED light source.

[0022] c. Use a transfer platform (Meita Optoelectronics: 2D material microscopic transfer platform) to transfer and stack the WS2 material and the substrate containing h-BN, ensuring that the materials on both sides have an overlapping area of ​​more than 4 square microns. After heating the entire structure to 120°C and maintaining it for 10 minutes, remove the upper PDMS film. At this time, all the WS2 attached to the upper PDMS film has been transferred to the unit substrate;

[0023] 4) Electrode deposition and device processing

[0024] a. The substrate containing the WS2 / h-BN material is placed inverted in the evaporation chamber;

[0025] b. Use copper wire as a mask to cover the front of the overlapping area and fix it with high temperature tape;

[0026] c. Using the thermal evaporation scheme, the instrument adds a current of 110 A, so that the 50 nm thick gold is completely evaporated on the front of the material;

[0027] d. Take out the sample after evaporation, use laboratory plastic tweezers, touch the copper wire with the tweezers head, and use a force of 50 N to break the copper wire.

[0028] e. The fabricated device was annealed in argon at 120°C for 2 hours to ensure strong coupling of the heterojunction.

[0029] f. Finally, a high voltage of 60 V is applied to the back gate to accumulate charges at the heterojunction interface.

[0030] The present invention provides a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges and a preparation method thereof. The WS2 / h-BN field effect transistor based on long-term storage of interface defect charges includes: a silicon / silicon dioxide substrate, a WS2 / h-BN heterojunction, a metal electrode, and a device channel. The above-mentioned silicon / silicon dioxide substrate is used as the bottom carrier, and PDMS is used to perform pre-stripping and transfer of commercial two-dimensional WS2 and h-BN bulk materials. Among them, ultraviolet light treatment is introduced to enhance the ability of the two-dimensional interface to store charges and the defect density per unit area. The present invention realizes long-term and efficient memory of two-dimensional images by changing the power of ultraviolet light treatment, combined with later electrical processing and characterization, and can be used for the development of image encryption functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a schematic diagram of the WS2 / h-BN field effect transistor based on long-term storage of interface defect charges and its preparation process of the present invention;

[0032] Figure 2 This is a fluorescence microscopy image of a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges;

[0033] Figure 3 This is the Raman spectrum of the WS2 / h-BN field effect transistor based on long-term storage of interface defect charges;

[0034] Figure 4 This is the X-ray photoelectron spectrum of the WS2 / h-BN field effect transistor based on long-term storage of interface defect charges;

[0035] Figure 5 This is a transfer curve scan of the WS2 / h-BN field effect transistor based on long-term storage of interface defect charges. The arrow indicates the scanning direction, and the color is used to distinguish the optoelectronic performance of devices with different treatments.

[0036] Figure 6 It is based on the scan results and status of different devices;

[0037] Figure 7 For imaging demonstration and graphic reproduction based on different preparation schemes. DETAILED DESCRIPTION

[0038] Example 1 Preparation process of WS2 / h-BN field effect transistor

[0039] Please see attached Figure 1 , the preparation process of WS2 / h-BN field effect transistor is divided into the following six steps:

[0040] 1) Substrate cutting and processing: Mark the straight cutting edge of the commercial silicon / silicon dioxide substrate with a plastic plate and divide it into 1 cm×1 cm substrate units; use a sapphire glass knife to cut along the 1 cm×1 cm straight edge with a force of 100 N. Keep the substrate horizontal and use a vertical force to bend it along the vertical edge with a force of 200 N until the substrate is divided into two pieces along the straight edge. Repeat the above operation for the four edges of the square unit substrate.

[0041] 2) Mechanical peeling of hexagonal boron nitride: Place the commercial h-BN bulk material on the PDMS film, take a piece of PDMS film, paste the two face to face, and apply 50 N of pressure to the upper layer to make the two tightly bonded; take the upper PDMS film with material attached, and transfer it to the square unit substrate. After heating the whole to 120℃ and keeping it for 10 minutes, remove the upper PDMS film. At this time, the h-BN attached to the upper PDMS film has been completely transferred to the unit substrate.

[0042] 3) UV exposure treatment: The substrate containing h-BN is placed in UV exposure for 10 minutes at a power of 0-60 microwatts. The wavelength of the UV light used for exposure is 265 nm, and the light source type is LED light source.

[0043] 4) Preparation of WS2 material and UV exposure treatment: Place commercial WS2 bulk material on a PDMS film, take a piece of PDMS film, stick the two together, and apply a pressure of 100 N to the upper layer so that the two are tightly combined; take the PDMS film with WS2 material on the upper layer, and place it in UV exposure. The exposure power is 10 minutes, the power is 0-60 microwatts, the wavelength of the ultraviolet light used for exposure is 265 nm, and the light source type is LED light source.

[0044] 5) Heterojunction construction: Use a transfer platform (Meta Optoelectronics: 2D material microscopic transfer platform) to transfer and stack the WS2 material and the substrate containing h-BN, ensuring that the materials on both sides have an overlapping area of ​​more than 4 square microns. After heating the entire structure to 120°C and maintaining it for 10 minutes, remove the upper PDMS film. At this time, all the WS2 attached to the upper PDMS film has been transferred to the unit substrate.

[0045] 6) Electrode evaporation and device processing: Place the substrate containing the above WS2 / h-BN material upside down in the evaporation chamber; use copper wire as a mask to cover the front of the overlapping area and fix it with high-temperature tape; use a thermal evaporation scheme, add a current of 110 A to the instrument, so that the 50 nm thick gold is completely evaporated on the front of the material; take out the evaporated sample, use laboratory plastic tweezers, touch the copper wire with the tweezer head, and use a force of 50 N to break the copper wire. The prepared device is annealed in argon at 120°C for 2 hours to ensure strong coupling of the heterojunction. Finally, a high voltage of 60 V is applied to the back gate on the back side to accumulate charge at the heterojunction interface.

[0046] At this point, the device preparation and processing process has been completed.

[0047] Example 2 WS2 / h-BN field effect transistor based on long-term storage of interface defect charges

[0048] Please see attached Figure 2 , based on the long-term storage of interface defect charge, the WS2 / h-BN field effect transistor includes: silicon / silicon dioxide substrate, WS2 / h-BN heterojunction, metal electrode, and device channel. The silicon / silicon dioxide substrate is purchased commercially, and then processed and cut using a sapphire glass knife; the WS2 / h-BN heterojunction is a two-dimensional material that has been mechanically peeled off and exposed to ultraviolet light, and then transferred and bonded. The blue channel width is 10 microns. The pink areas on the left and right are 50-nanometer-thick metal electrodes.

[0049] Example 3 Characterization of Materials for WS2 / h-BN Field Effect Transistors

[0050] See also Figure 2-4 The specific characterization method is as follows:

[0051] 1) See attached Figure 2 , the WS2 / h-BN field effect transistor based on long-term storage of interface defect charges was placed in an optical field, a laser with a wavelength of 532 nm was introduced, and the laser power was attenuated to 0.1 mW. The upper layer material WS2 was exposed, and the integration time was 100 milliseconds, and its Raman spectrum intensity was recorded by a spectrometer. The results showed that the upper layer WS2 of the heterojunction prepared by UV exposure and gate treatment still maintained its typical Raman vibration characteristics, corresponding to the in-plane vibration mode (E 2g 1 ) and out-of-plane vibration modes (A 1g ).

[0052] 2) See attached Figure 3, the WS2 / h-BN field effect transistor based on long-term storage of interface defect charge was placed in an X-ray radiation field, and the change in its scattered light intensity was monitored. Figure 3 The binding energy spectrum shown corresponds to the atomic orbital energies of W and S atoms, respectively, and is consistent with the typical WS2 material energy spectrum.

[0053] Example 4 Application of WS2 / h-BN field effect transistor based on long-term storage of interface defect charges

[0054] Its application specifically involves the following parts:

[0055] 1) Please see the attached Figure 5 :The transfer curve scanning diagram of WS2 / h-BN field effect transistor based on long-term storage of interface defect charge, in which the arrow indicates the scanning direction, and the color is used to distinguish the optoelectronic performance of devices after different treatments. Connect the three-terminal electrodes, use the gate as the scanning voltage, keep the bias at 5V, the starting point is -45V, and the voltages on the left and right ends are -45V and 45V respectively. Here, the end points are artificially defined as four states, I, II, III, and IV, which can be distinguished by current. The specific differences between different states are marked in the table. That is, there are four states with or without UV treatment, and with or without cycle of scanning voltage. The four states correspond to different storage densities of charge on the heterojunction interface of the device.

[0056] 2) Please see the attached Figure 6 , using four states and a special mask, on the one hand, two-dimensional scanning can be used to control whether the device is treated with UV light; on the other hand, combined with the gate voltage cycle of the device, the resistance level at the end of the scan can be controlled. Here, we use the color of the mask and its hollowed-out position in the schematic diagram to define its state: I, II, III, and IV correspond to dark blue, dark red, orange, and light blue, respectively.

[0057] Specifically:

[0058] State I: no UV exposure and no scanning cycle;

[0059] State II: with UV exposure and without scanning cycle;

[0060] State III: no UV exposure and with scanning cycle;

[0061] State IV: UV exposure and scanning cycle.

[0062] 3) Please see the attached Figure 7 We used the above pattern as the input image, selected 10×10 pixels as the writing module of a single Chinese character, and performed multiple writing on a single device with or without UV exposure and with or without scanning cycles, and kept the written device under natural conditions for 48 hours. Finally, the device current was read out using a two-terminal circuit, as shown in the attached figure. Figure 7 As shown on the right, the device imaging shows good distinguishability and the content of the Chinese characters can be clearly distinguished.

[0063] The present invention effectively modulates the interface charge, and the device has multi-state distinction and adjustability, thereby realizing long-term complex image memory. It not only provides a potential method for modulating the interface charge of the field effect transistor, but also opens up a path for the application of the next generation of memory.

Claims

1. WS2 / h-BN field effect transistor based on long-term storage of interface defect charges, characterized by: From bottom to top, there are a silicon / silicon dioxide substrate, a hexagonal boron nitride two-dimensional thin layer, a WS2 two-dimensional thin layer, and two metal electrodes; the upper surface of the hexagonal boron nitride two-dimensional thin layer and the lower surface of the WS2 two-dimensional thin layer have been subjected to ultraviolet exposure treatment.

2. The WS2 / h-BN field effect transistor based on long-term storage of interface defect charges according to claim 1, characterized in that: The ultraviolet exposure treatment has a power of 0-60 microwatts, an ultraviolet light wavelength of 265 nm, and a duration of 10 minutes.

3. The WS2 / h-BN field effect transistor based on long-term storage of interface defect charges according to claim 2, characterized in that: The substrate is 1 cm×1 cm and has a 280nm oxide layer; the overlapping area of ​​the hexagonal boron nitride two-dimensional thin layer and the WS2 two-dimensional thin layer is greater than 4 square microns.

4. The WS2 / h-BN field effect transistor based on long-term storage of interface defect charges according to claim 3, characterized in that: The metal electrodes are two gold electrodes with a thickness of 50 nm which are deposited by thermal evaporation.

5. A method for preparing a WS2 / h-BN field effect transistor based on long-term storage of interface defect charges, comprising: 1) Substrate cutting: a. Mark the straight cutting edge of the commercial silicon / silicon dioxide substrate with a plastic plate and divide it into 1 cm×1 cm substrate units; b. Use a sapphire glass knife to cut along a 1 cm × 1 cm straight edge with a force of 100 N; c. Keep the substrate horizontal, use vertical force, bend along the vertical edge direction with a force of 200 N, until the substrate is divided into two pieces along the straight edge; d. Repeat the above steps ac for the four edges of the square unit substrate 2) Preparation of lower layer h-BN material and UV exposure treatment a. Place the commercial h-BN bulk material on the PDMS film, take a piece of PDMS film, stick the two together, and apply a pressure of 50 N to the upper layer so that the two are tightly bonded; b. Take the upper PDMS film with the material attached and transfer it to the square unit substrate; c. After heating the whole to 120°C and maintaining for 10 minutes, remove the upper PDMS film. At this time, the h-BN adhered to the upper PDMS film has been completely transferred to the unit substrate; d. Place the substrate containing h-BN in UV exposure for 10 minutes at a power of 0-60 microwatts. The wavelength of the UV light used for exposure is 265 nm and the light source type is LED light source; 3) Preparation of upper WS2 material and UV exposure treatment a. Place the commercial WS2 bulk material on the PDMS film, take a piece of PDMS film, paste the two face to face, and apply a pressure of 100 N to the upper layer so that the two are tightly combined; b. Take the upper PDMS film with WS2 material and place it in UV exposure. The exposure power is 10 minutes, the power is 0-60 microwatts, the wavelength of UV light used for exposure is 265 nm, and the light source type is LED light source; c. Use a transfer table to transfer and stack the WS2 material and the substrate containing h-BN, ensuring that the materials on both sides have an overlapping area of ​​more than 4 square microns; heat the entire structure to 120°C and keep it for 10 minutes, then remove the upper PDMS film. At this time, the WS2 adhered to the upper PDMS film has been completely transferred to the unit substrate; 4) Electrode deposition and device processing a. The substrate containing the WS2 / h-BN material is placed inverted in the evaporation chamber; b. Use copper wire as a mask to cover the front of the overlapping area and fix it with high temperature tape; c. Using the thermal evaporation scheme, the instrument adds a current of 110 A, so that the 50 nm thick gold is completely evaporated on the front of the material; d. Take out the sample after evaporation, use laboratory plastic tweezers, touch the copper wire with the tweezers head, and use a force of 50 N to break the copper wire; e. The prepared device was annealed in argon at 120 ° C for 2 hours to ensure strong coupling of the heterojunction; f. Finally, a high voltage of 60 V is applied to the back gate to accumulate charges at the heterojunction interface.