Composite multi-dimensional high-performance zinc ion battery negative electrode material and preparation method thereof

Through the hydrothermal reaction and electrochemical deposition method of chondroitin sulfate and graphene oxide, a composite multi-dimensional high-performance zinc ion battery negative electrode material with three-dimensional structure was constructed, which solved the problems of dendrites growth and side reaction of zinc ion battery negative electrode material, significantly improved the The electrochemical performance and cycle stability of the battery are obtained.

CN118983429APending Publication Date: 2024-11-19SOUTHEAST UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411039989.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The negative electrode materials of zinc ion batteries have problems with dendrite growth and side reactions, resulting in a decrease in capacity and efficiency, hindering its large-scale application.

Method used

Chondroitin sulfate and graphene oxide are used as raw materials to construct a three-dimensional structure through hydrothermal reaction of ethylenediamine, and zinc is deposited by electrochemical deposition to form a composite multi-dimensional high-performance zinc ion battery negative electrode material to inhibit the growth and sub-gauge of zinc dendrites reaction.

Benefits of technology

The electrochemical performance of zinc ion batteries has been improved, the preparation method is simple and the raw materials are easy to obtain, and a stable interface layer is effectively built, which improves the cycling performance and application prospects of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983429A_ABST
    Figure CN118983429A_ABST
Patent Text Reader

Abstract

The invention discloses a composite multi-dimensional high-performance zinc ion battery negative electrode material and a preparation method thereof. Chondroitin sulfate (CS) powder is added into a graphene oxide (GO) solution, stirring and dissolving are performed to prepare a precursor solution, an ethylenediamine (EDA) solution is added into the precursor solution, and CS (at) rGO-EDA is obtained through a hydrothermal reaction. And taking out the product, washing with deionized water, and freeze-drying. And depositing Zn on the CS (at) rGO-EDA substrate by an electrochemical deposition method to obtain the composite multi-dimensional high-performance zinc ion battery negative electrode material Zn / CS (at) rGO-EDA. The composite multi-dimensional high-performance zinc ion battery negative electrode material disclosed by the invention shows relatively good conductivity and relatively long cycle life, and has excellent performance under high current density. The invention provides a simple scheme and idea for the preparation of the zinc ion battery negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite multi-dimensional high-performance zinc ion battery negative electrode material and a preparation method thereof, belonging to the technical field of energy storage materials. Background Art

[0002] Due to the development of society, the energy demand of modern society is constantly increasing, which puts higher requirements on energy storage devices. Batteries are efficient, convenient and environmentally friendly electrochemical energy storage systems, which have been widely used in large-scale grid-connected energy storage systems, portable electronic devices and electric vehicles. At present, lithium-ion batteries are the dominant energy storage devices on the market. However, they have their own shortcomings such as shortage of metallic lithium resources, high cost, harsh preparation conditions, toxic organic electrolytes, and potential safety hazards, which seriously hinder their further application. Therefore, zinc-ion batteries with mild aqueous electrolyte solutions have attracted widespread attention due to their simple preparation technology, high energy density, intrinsic safety and economic feasibility. Therefore, they are expected to replace lithium-ion batteries as large-scale energy storage devices.

[0003] Zn metal is used as the negative electrode material of zinc ion batteries because of its high conductivity (resistivity is 5.91μΩ·cm), low redox potential (-0.76V vsSHE), large hydrogen evolution overpotential, high theoretical specific capacity (820mAh / g, 5851mAh / cm), low ion radius (0.075nm), low cost, and abundant availability. Zn anode is an important component of aqueous zinc ion batteries. During the charge and discharge process, Zn 2+ Rapidly and reversibly dissolves and precipitates on the surface of Zn metal anode to achieve energy conversion. 2+ The fast and reversible plating / stripping behavior of Zn anode directly affects the overall performance of the battery. Commercial Zn foil is usually used as Zn anode by most researchers.

[0004] However, the specific surface area of ​​zinc foil is limited and the contact with the electrolyte is insufficient. 2+ The deposition of Zn on the surface of Zn metal anode is uneven, causing dendrite growth and passivation. These side reactions lead to a decrease in the capacity and coulombic efficiency of zinc ion batteries, which seriously hinders the large-scale application of zinc ion batteries. Carbon-based materials have good conductivity, and modifying the Zn negative electrode interface is conducive to stabilizing Zn 2+The plating / stripping behavior of Zn is improved. In carbon materials, graphene acts as a protective layer to inhibit the growth of dendrites on the Zn negative electrode. At the same time, graphene has a lower lattice mismatch and can effectively drive Zn deposition with a locked crystal orientation relationship. The conductive network and porous structure of the three-dimensional carbon composite material enable rapid electron / ion transmission and abundant deposition space, thereby hindering the formation of Zn dendrites and reducing the nucleation potential. High-performance zinc-ion battery negative electrode materials based on three-dimensional carbon composites can be effectively constructed, which has better application prospects. Summary of the invention

[0005] Purpose of the invention: The first purpose of the present invention is to provide a composite multidimensional high-performance zinc ion battery negative electrode material; the second purpose of the present invention is to provide a method for preparing the composite multidimensional high-performance zinc ion battery negative electrode material.

[0006] Technical solution: The composite multi-dimensional high-performance zinc ion battery negative electrode material described in the present invention comprises chondroitin sulfate (CS) and graphene oxide (GO) as raw materials, ethylenediamine (EDA) as a cross-linking agent for hydrothermal reaction, and then Zn is deposited by electrochemical deposition.

[0007] Furthermore, zinc foil is used as a zinc source when depositing Zn.

[0008] Furthermore, the thickness of the zinc foil is 100-200 μm, and the diameter of the zinc foil is 12-19 mm.

[0009] The method for preparing the composite multi-dimensional high-performance zinc ion battery negative electrode material of the present invention comprises the following steps:

[0010] (1) adding chondroitin sulfate (CS) powder into graphene oxide (GO) solution, stirring and dissolving to prepare a precursor CS@rGO solution;

[0011] (2) adding ethylenediamine (EDA) solution to the precursor CS@rGO solution, hydrothermal reaction, washing, freeze drying, and obtaining CS@rGO-EDA;

[0012] (3) Through electrochemical deposition, zinc foil was used as the zinc source and negative electrode to deposit Zn on CS@rGO-EDA to obtain Zn / CS@rGO-EDA.

[0013] Furthermore, in step (1), the mass concentration of the graphene oxide solution is 1-5 mg / mL, preferably 2 mg / mL.

[0014] Furthermore, in step (1), the mass ratio of chondroitin sulfate to graphene oxide is 1-2:6.

[0015] Furthermore, in step (1), the temperature for stirring and dissolving is 80-100° C., preferably 90° C., and the time for stirring and dissolving is 1-3 h.

[0016] Furthermore, in step (2), the concentration of the ethylenediamine solution is 1-2 mg / L.

[0017] Furthermore, in step (2), the volume ratio of the ethylenediamine solution to the precursor CS-rGO solution is 0.8-1.6:30.

[0018] Furthermore, in step (2), the temperature of the hydrothermal reaction is 160-180° C., and the time of the hydrothermal reaction is 8-10 h.

[0019] Furthermore, in step (2), the freeze-drying temperature is below -50°C and the freeze-drying time is 10-12 hours.

[0020] Furthermore, in step (3), the current density of the electrochemical deposition is 1-10 mA / cm 2 .

[0021] Furthermore, in step (3), the electrochemical deposition time is 1-3 hours.

[0022] Principle of the invention: The CS of the present invention is cross-linked with reduced graphene oxide (rGO) through ester groups, and the cross-linking agent EDA constructs a three-dimensional CS@rGO-EDA structure through a hydrothermal reaction. The biomacromolecule CS is rich in carboxyl (-COOH), sulfonic acid (-SO3H), acylamino (-NH─C(O)-), hydroxyl (-OH), and ether (-C─O─C-) groups, and exhibits a special affinity for the zinc surface, which leads to their initial strong attachment through favorable potential energy interactions. The process ultimately establishes a stable interface layer, effectively preventing uncontrolled chemical corrosion of the electrolyte and maintaining the surface uniformity of the electrode. The three-dimensional structure has good conductivity, effectively inhibits the growth of zinc dendrites and the generation of side reactions, and effectively improves the electrochemical performance of zinc ion batteries.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0024] (1) The preparation method of the present invention is simple, the raw materials are easily available, and CS is a biological macromolecule in the human body and is harmless to the human body;

[0025] (2) The composite multidimensional zinc ion battery negative electrode of the present invention has excellent electrochemical properties;

[0026] (3) The present invention effectively inhibits the growth of zinc dendrites and the generation of side reactions, and constructs a stable zinc negative electrode interface layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the structure of CS@rGO prepared in Example 1;

[0028] Figure 2 This is a SEM image of the composite multi-dimensional high-performance zinc ion battery negative electrode material obtained in Example 1;

[0029] Figure 3 This is a SEM image of the composite multi-dimensional high-performance zinc ion battery negative electrode material obtained in Example 2;

[0030] Figure 4 This is a SEM image of the composite multi-dimensional high-performance zinc ion battery negative electrode material obtained in Example 3;

[0031] Figure 5 This is the cycle performance diagram of the Zn / CS@rGO-EDA / / Zn / CS@rGO-EDA symmetric battery obtained in Example 4;

[0032] Figure 6 This is a cycle performance diagram of the all-electric button cell assembled in Example 5;

[0033] Figure 7 This is a diagram showing a lighted thermometer for a soft-pack pouch battery assembled in Example 5;

[0034] Figure 8 This is a SEM image of the negative electrode material of the zinc ion battery negative electrode comparison sample obtained in Comparative Example 1;

[0035] Fig. 9 This is a full battery cycle performance diagram of the zinc ion battery negative electrode comparison sample material obtained in Comparative Example 1. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0037] Example 1

[0038] (1) Add 10 mg CS powder into 30 mL 2 mg / mL GO solution and stir in a water bath at 90 °C for 1 h to dissolve into the precursor CS@rGO solution. The schematic diagram of the CS@rGO structure is shown in Figure 1 shown.

[0039] (2) The precursor CS@rGO solution was added into the reactor and 800 μL 1 mg / mL EDA solution was added dropwise, and the product CS@rGO-EDA was obtained by hydrothermal reaction at 180 °C for 10 h. The product CS@rGO-EDA was taken out and washed with deionized water, and freeze-dried at -50 °C for 12 h. Subsequently, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode by electrochemical deposition. 160 mg of CS@rGO-EDA was taken and mixed with 80% CS@rGO-EDA, 10% polyvinylidene fluoride (PVDF), 10% conductive carbon black and a small amount of N-methylpyrrolidone (NMP) in a mass ratio and then coated on a stainless steel foil (thickness of 80 μm, length × width of 9 cm × 9 cm) and cut into a disc (diameter of 14 mm) as the positive electrode. 100 μL of 2 mol / L zinc sulfate (ZnSO4) solution was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CS@rGO-EDA matrix, and take it out to obtain a composite multi-dimensional high-performance zinc ion battery negative electrode material.

[0040] The composite multi-dimensional high-performance zinc ion battery negative electrode material prepared in this example was subjected to scanning electron microscopy analysis, and the results are as follows: Figure 2 shown. Figure 2 This is a scanning electron microscope (SEM) image of the composite multi-dimensional high-performance zinc ion battery negative electrode material obtained in Example 1. Figure 2 It can be seen that due to the cross-linking effect of CS and EDA, reduced graphene oxide (rGO) presents a layered structure, but rGO tends to stack, which hinders the rapid transport of ions.

[0041] Example 2

[0042] The experimental process was the same as in Example 1. 10 mg of CS powder was added to 30 mL of 2 mg / mL GO solution and stirred in a water bath at 90 ° C for 1 h to dissolve and prepare a precursor CS@rGO solution. The precursor CS@rGO solution was added to the reactor and 1.6 mL of 1 mg / mL LEDA solution was added dropwise. The CS@rGO-EDA was obtained by hydrothermal reaction at 180 ° C for 10 h. The product CS@rGO-EDA was taken out and washed with deionized water, and freeze-dried at -50 ° C for 12 h. Subsequently, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode by electrochemical deposition. 160 mg of CS@rGO-EDA was taken and mixed with 80% CS@rGO-EDA, 10% PVDF, 10% conductive carbon black and a small amount of NMP in a mass ratio. The mixture was evenly coated on a stainless steel foil (thickness of 80 μm, length × width of 9 cm × 9 cm) and cut into a disc (diameter of 14 mm) as the positive electrode. 100 μL 2 mol / L ZnSO4 was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CS@rGO-EDA matrix, and take out the electrode to obtain a composite multi-dimensional high-performance zinc ion battery negative electrode material.

[0043] The composite multi-dimensional high-performance zinc ion battery negative electrode material prepared in this example was subjected to scanning electron microscopy analysis, and the results are as follows: Figure 3 shown. Figure 3 This is a SEM image of the composite multi-dimensional high-performance zinc ion battery negative electrode material obtained in Example 2. Figure 3 It can be seen that due to the increase in EDA content, the sheet-like rGO is gradually connected into a piece, becoming a rapid ion transmission channel and a conductive skeleton.

[0044] Example 3

[0045] The experimental process was the same as in Example 1. 20 mg of CS powder was added to 30 mL of 2 mg / mL GO solution and stirred in a water bath at 90 ° C for 1 h to dissolve and prepare a precursor CS@rGO solution. The precursor CS@rGO solution was added to the reactor and 800 μL of 1 mg / mL LEDA solution was added dropwise. The CS@rGO-EDA was obtained by hydrothermal reaction at 180 ° C for 10 h. After the product was taken out, the CS@rGO-EDA was washed with deionized water and freeze-dried at -50 ° C for 12 h. Subsequently, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode by electrochemical deposition. 160 mg of CS@rGO-EDA was taken and mixed with 80% CS@rGO-EDA, 10% PVDF, 10% conductive carbon black and a small amount of NMP in a mass ratio. The mixture was evenly coated on a stainless steel foil (thickness of 80 μm, length × width of 9 cm × 9 cm) and cut into a disc (diameter of 14 mm) as the positive electrode. 100 μL 2 mol / L ZnSO4 was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CS@rGO-EDA matrix, and take out the electrode to obtain a composite multi-dimensional high-performance zinc ion battery negative electrode material.

[0046] The composite multi-dimensional high-performance zinc ion battery negative electrode material prepared in this example was subjected to scanning electron microscopy analysis, and the results are as follows: Figure 4 shown. Figure 4 This is a SEM image of the composite multi-dimensional high-performance zinc ion battery negative electrode material matrix obtained in Example 3. Figure 4 It can be seen that due to the increase in CS content, the rGO sheet diameter is larger, the folds are more, and the layers are thinner, which is conducive to the rapid transmission of ions and electrons.

[0047] From the SEM images of comparative examples 1-3, it can be seen that due to the increase in the content of EDA and CS crosslinking agents, the crosslinking effect is enhanced, and the formed CS@rGO-EDA structure has a larger sheet diameter, more wrinkles, and thinner layers, which is conducive to the rapid transmission of ions and electrons, thereby improving the electrochemical performance of zinc ion batteries.

[0048] Example 4

[0049] The experimental process was the same as in Example 1. 20 mg of CS powder was added to 30 mL of 2 mg / mL GO solution and stirred in a water bath at 90 ° C for 1 h to dissolve and prepare a precursor CS@rGO solution. The precursor CS@rGO solution was added to the reactor and 1.6 mL of 1 mg / mL LEDA solution was added dropwise. The CS@rGO-EDA was obtained by hydrothermal reaction at 180 ° C for 10 h. The product CS@rGO-EDA was taken out and washed with deionized water and freeze-dried at -50 ° C for 12 h. Subsequently, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode by electrochemical deposition. 160 mg of CS@rGO-EDA was taken and mixed with 80% CS@rGO-EDA, 10% PVDF, 10% conductive carbon black and a small amount of NMP in a mass ratio. The mixture was evenly coated on a stainless steel foil (thickness of 80 μm, length × width of 9 cm × 9 cm) and cut into a disc (diameter of 14 mm) as the positive electrode. 100 μL 2 mol / L ZnSO4 was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CS@rGO-EDA matrix, and take out the electrode piece to obtain the composite multi-dimensional high-performance zinc ion battery negative electrode material Zn / CS@rGO-EDA.

[0050] The composite multidimensional high-performance zinc ion battery negative electrode material prepared in this example was cut into electrode sheets with a length × width of 8.5 cm × 6 cm, and two identical electrolyte sheets were used as the positive electrode and the negative electrode, respectively, and 100 μL 2mol / L ZnSO4 was used as the electrolyte to assemble a Zn / CS@rGO-EDA / / Zn / CS@rGO-EDA symmetrical battery.

[0051] The electrochemical cycle performance of the Zn / CS@rGO-EDA / / Zn / CS@rGO-EDA symmetrical battery prepared in this example was analyzed. Figure 5 shown. Figure 5 This is the cycle performance diagram of the Zn / CS@rGO-EDA / / Zn / CS@rGO-EDA symmetric battery obtained in Example 4. Figure 5 It can be seen that the obtained composite multidimensional high-performance zinc-ion battery negative electrode can be stably cycled for 1000 hours, which reflects the good stability of the battery cycle performance.

[0052] Example 5

[0053] 80 mg of CS powder was added to 120 mL of 2 mg / mL GO solution and stirred in a water bath at 90 °C for 1 h to dissolve and prepare the precursor CS@rGO solution. The precursor CS@rGO solution was added to the reactor and 6.4 mL of 1 mg / mL EDA solution was added dropwise, and CS@rGO-EDA was obtained by hydrothermal reaction at 180 °C for 10 h. The product CS@rGO-EDA was taken out and washed with deionized water and freeze-dried at -50 °C for 12 h. Subsequently, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode by electrochemical deposition. 160 mg of CS@rGO-EDA was taken and mixed with 80% CS@rGO-EDA, 10% PVDF, 10% conductive carbon black and a small amount of NMP in a mass ratio. The mixture was evenly coated on a stainless steel foil (thickness of 80 μm, length × width of 9 cm × 9 cm) and cut into a disc (diameter of 14 mm) as the positive electrode. 100 μL of 2 mol / L ZnSO4 solution was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CS@rGO-EDA matrix, and take out the electrode to obtain a composite multi-dimensional high-performance zinc ion battery negative electrode material.

[0054] The composite multi-dimensional high-performance zinc ion battery negative electrode material was cut into a disc with a diameter of 19 mm as the Zn / CS@rGO-EDA negative electrode. 160 mg of NH4V4O 10 , and in accordance with the mass ratio of 80% NH4V4O 10 , 10% PVDF, 10% conductive carbon black and a small amount of NMP were mixed and coated on a stainless steel foil (thickness 80 μm, length × width 9 cm × 9 cm) and cut into 14 mm discs as NH4V4O 10 The positive electrode and 100 μL 2 mol / L ZnSO4 solution were used as the electrolyte to assemble a fully electric button cell.

[0055] Composed of 3 8×5.5cm 2 NH4V4O 10 Positive electrode, 3 pieces 8.5×6cm 2 Zn / CS@rGO-EDA negative electrode sheet (thickness: 80 μm) and five 9×6.5 cm 2 The glass fiber separators are separated in sequence, and 100 μL 2 mol / L ZnSO4 solution is used as the electrolyte to assemble into a soft-pack pouch battery.

[0056] The fully electric button cell and soft-pack pouch cell prepared in this example were subjected to cycle performance tests. Figure 6-7 As shown, Figure 6 This is the cycle performance diagram of the all-electric button cell obtained in Example 5. Figure 6It can be seen that the obtained full battery has a high current density of 10A. -1 After 800 stable cycles, there is still 150mAh g -1 capacity.

[0057] Figure 7 This is a diagram showing the lighting thermometer of the soft-pack pouch battery obtained in Example 5. Figure 7 It can be seen that the prepared soft-pack pouch battery successfully allowed the thermometer to operate, which reflects the commercial potential application of the obtained composite multidimensional high-performance zinc-ion battery negative electrode material.

[0058] Comparative Example 1

[0059] The preparation process is the same as that in Example 5, except that chitosan is used instead of chondroitin sulfate. 80 mg of chitosan (CSA) powder is added to 120 mL of 2 mg / mL graphene oxide (GO) solution, and the solution is dissolved in a water bath at 90 ° C for 1 h to prepare a precursor CSA@rGO solution. The precursor CSA@rGO solution is added to the reactor and 6.4 mL of EDA solution is added dropwise, and the hydrothermal reaction is carried out at 180 ° C for 10 h to obtain CSA@rGO-EDA. The product CSA@rGO-EDA is taken out and washed with deionized water and freeze-dried at -50 ° C for 12 h. Then, by electrochemical deposition, a zinc foil with a thickness of 150 μm and a diameter of 19 mm was used as the zinc source and negative electrode. 160 mg of CSA@rGO-EDA was taken and mixed with 80% CSA@rGO-EDA, 10% PVDF, 10% conductive carbon black and a small amount of NMP in a mass ratio and then coated on a stainless steel foil as the positive electrode. 100 μL 2 mol / L ZnSO4 was used as the electrolyte to assemble a button cell with a current density of 10 mA cm -2 , deposit for 1h, deposit Zn on the CSA@rGO-EDA matrix, and take out the electrode piece to obtain the comparison sample material of the zinc ion battery negative electrode.

[0060] The preparation of the full battery is the same as in Example 5, except that the negative electrode material of the zinc ion battery is used instead of the composite multi-dimensional high-performance zinc ion battery negative electrode material as the negative electrode, and the NH4V4O 10 Assemble the full battery with positive electrode.

[0061] The negative electrode material of the zinc ion battery negative electrode comparison sample prepared in this comparative example was analyzed by scanning electron microscope. The results Figure 8 As shown, Figure 8 This is a SEM image of the negative electrode material of the zinc ion battery negative electrode comparison sample obtained in Comparative Example 1. Figure 8 It can be seen that compared with CS@rGO-EDA, the structure of CSA@rGO-EDA is more disordered, the flakes are smaller and tend to be stacked, which hinders the rapid transmission of electrons and ions.

[0062] The full battery prepared in this comparative example was subjected to a cycle performance test, and the results Fig. 9 As shown, Fig. 9 This is a full battery cycle performance diagram of the zinc ion battery negative electrode comparison sample material obtained in Comparative Example 1. Fig. 9 It can be seen that the obtained full battery is 10Ag -1 A short circuit occurred after only a few cycles, and the performance was far lower than that of the composite multi-dimensional high-performance zinc ion battery negative electrode material in Example 5.

Claims

1. A composite multi-dimensional high-performance zinc ion battery negative electrode material, characterized in that: The method comprises taking chondroitin sulfate and graphene oxide as raw materials, carrying out a hydrothermal reaction with ethylenediamine as a cross-linking agent, and then utilizing an electrochemical deposition method to deposit Zn.

2. The composite multidimensional high performance zinc ion battery negative electrode material according to claim 1, characterized in that: Zinc foil was used as the zinc source for Zn deposition.

3. The composite multidimensional high performance zinc ion battery negative electrode material according to claim 2, characterized in that: The thickness of the zinc foil is 100-200 μm, and the diameter of the zinc foil is 12-19 mm.

4. The method for preparing the composite multidimensional high-performance zinc ion battery negative electrode material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) adding chondroitin sulfate powder to graphene oxide solution, stirring and dissolving, and preparing a precursor CS@rGO solution; (2) adding ethylenediamine solution to the precursor CS@rGO solution, hydrothermally reacting, washing, and freeze-drying to obtain CS@rGO-EDA; (3) Through electrochemical deposition, zinc foil was used as the zinc source and negative electrode to deposit Zn on CS@rGO-EDA to obtain Zn / CS@rGO-EDA.

5. The method for preparing the composite multidimensional high performance zinc ion battery negative electrode material according to claim 4, characterized in that: In step (1), the mass concentration of the graphene oxide solution is 1-5 mg / mL, and the mass ratio of chondroitin sulfate to graphene oxide is 1-2:

6.

6. The method for preparing the composite multidimensional high performance zinc ion battery negative electrode material according to claim 4, characterized in that: In step (1), the temperature for stirring and dissolving is 80-100° C., and the time for stirring and dissolving is 1-3 h.

7. The method for preparing the composite multidimensional high performance zinc ion battery negative electrode material according to claim 4, characterized in that: In step (2), the concentration of the ethylenediamine solution is 1-2 g / mL, and the volume ratio of the ethylenediamine solution to the precursor CS-rGO solution is 0.8-1.6:

30.

8. The method for preparing the composite multidimensional high performance zinc ion battery negative electrode material according to claim 4, characterized in that: In step (2), the temperature of the hydrothermal reaction is 160-180° C., and the time of the hydrothermal reaction is 8-10 h.

9. The method for preparing the composite multidimensional high performance zinc ion battery negative electrode material according to claim 4, characterized in that: In step (2), the freeze-drying temperature is below -50°C and the freeze-drying time is 10-12 hours.