Method for preparing iron-chromium liquid flow primary battery and energy storage battery by taking ferrochrome as raw material
By optimizing the fabrication process of iron-chromium red red batteries and using ferrochrome alloys to prepare iron oxide red and divalent chromium ion solutions, the problems of electrolyte stability and hydrogen evolution were solved, improving battery performance and safety, and making the batteries suitable for large-scale energy storage applications.
Patent Information
- Application Number
- CN202411225798.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
AI Technical Summary
Existing iron-chromium redox flow batteries suffer from poor electrolyte stability, impurity accumulation, hydrogen evolution, and mixing of positive and negative electrode liquids during long-term use, which affect battery efficiency and safety.
Using ferrochrome alloy as raw material, by preparing iron oxide red and divalent chromium ion solutions, optimizing electrode materials and structure, designing fuel cell stack flow channels, and combining ion membrane replacement and solution recovery treatment, the problems of hydrogen evolution and mixing of positive and negative electrode liquids are solved.
It improves the coulombic efficiency and cycle life of the battery, reduces production costs, and achieves long-term stable operation and safety of the battery, meeting the needs of large-scale energy storage.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of iron-chromium liquid flow batteries, and in particular relates to a method for preparing an iron-chromium liquid flow primary battery and an energy storage battery by using chromium-iron alloy as a raw material. Background Art
[0002] The iron-chromium flow battery is a redox-based flow battery that uses the reversible electrochemical reaction of iron and chromium ions to store and release energy. Its basic components include:
[0003] Electrolyte: The positive and negative electrolytes contain compounds of iron and chromium respectively.
[0004] Battery stack: It is composed of multiple battery cells, including electrodes and ion exchange membranes.
[0005] Liquid storage tank: stores positive and negative electrolyte.
[0006] Liquid flow pump: used to circulate electrolyte and realize electrochemical reaction through the battery stack.
[0007] Iron-chromium flow batteries have the following advantages:
[0008] High safety: Compared with other batteries, iron-chromium flow batteries have a lower risk of thermal runaway.
[0009] Flexibility: Battery capacity can be flexibly adjusted by increasing the size of the storage tank.
[0010] Application Areas
[0011] Suitable for energy storage of renewable energy sources (such as wind power and solar power).
[0012] It can be used as grid peak load regulation and backup power supply.
[0013] Problems to be solved
[0014] The long-term stability of the electrolyte needs to be improved to prevent impurity accumulation and degradation.
[0015] Existing ion exchange membranes are easily cross-contaminated, affecting battery efficiency and life.
[0016] Electrode materials and structures need to be optimized to improve the efficiency of electrochemical reactions.
[0017] Negative electrode reactions may lead to hydrogen evolution, reducing energy efficiency and increasing safety risks.
[0018] Recovery and treatment of electrode liquid. Summary of the invention
[0019] Technical problem: The present invention aims to provide a set of implementation processes for iron-chromium liquid flow batteries, which can solve the problem of the decrease of storage capacity with the increase of charge and discharge cycles by recycling the positive and negative electrode liquids after a relatively low number of charge and discharge cycles. At the same time, it can effectively solve the problems of hydrogen evolution and the mixed liquid of the positive and negative electrode flows.
[0020] Technical solution, a method for preparing iron-chromium liquid flow primary battery and energy storage battery using chromium-iron alloy as raw material, characterized in that it includes the following steps:
[0021] S1: Produce red iron oxide using ferrochrome as raw material;
[0022] S2: adding the red iron oxide obtained in S1 to one or more of sulfuric acid, nitric acid or hydrochloric acid to form a cathode solution;
[0023] Reactants: ferric ions (Fe 3+ )
[0024] Reaction process: During discharge, trivalent iron ions accept electrons at the positive electrode and are reduced to divalent iron ions.
[0025] Chemical equation:
[0026] Fe 3+ +e − →Fe 2+
[0027] The reverse reaction during charging: the divalent iron ions lose electrons and are reoxidized to trivalent iron ions.
[0028] S3: acid dissolving the ferrochrome alloy under inert gas protection and separating ferrous oxalate to obtain a cathode solution;
[0029] Reactants: divalent chromium ions (Cr 2+ )
[0030] Reaction process: During discharge, divalent chromium ions lose electrons at the negative electrode and oxidize to trivalent chromium ions.
[0031] Chemical equation:
[0032] Cr 2+ →Cr 3+ +e −
[0033] The reverse reaction during charging: trivalent chromium ions accept electrons and are reduced to divalent chromium ions.
[0034] S4: adding the positive electrode liquid and the negative electrode liquid produced above into the positive and negative electrode solution storage tanks of the iron-chromium liquid flow battery respectively; starting the liquid flow pump of the iron-chromium liquid flow battery; when the two liquid flows enter the battery stack, a redox reaction occurs and the external circuit generates current discharge, that is, a primary battery is formed;
[0035] When connected to an external power source, the positive electrode liquid of the discharged primary battery is reduced from trivalent to divalent, and the negative electrode liquid is oxidized from divalent to trivalent by itself, and then transformed into an energy storage battery;
[0036] S5: When the number of charge and discharge times of the positive and negative solutions of the iron-chromium flow battery reaches more than 1,000 times, the isolation capacity of the ion membrane decays, which will cause the positive and negative solutions to mix and penetrate and hydrogen evolution. At this time, the solution is recovered and processed to prepare chromic anhydride and ferrous oxalate, and the ion membrane is replaced as needed to effectively solve the problems of hydrogen evolution and the mixing and penetration of the positive and negative solutions.
[0037] Furthermore, S1 includes the following steps:
[0038] S11. preparing a low melting point eutectic oxide;
[0039] S12. Preparation of low melting point eutectic super oxide;
[0040] S13. Prepare sodium chromate solution and red iron oxide.
[0041] Further, in S11, a low melting point eutectic oxide is prepared: sodium nitrate and sodium chromate are used as raw materials, and the temperature is raised to 630° C. to 640° C. and maintained until all the materials form a molten liquid, thereby obtaining a low melting point eutectic oxide;
[0042] In S12, a low-melting point eutectic superoxide is prepared: the heating of the low-melting point eutectic oxide is stopped to cool the material to 590°C~610°C and maintain the temperature, and air is blown into the low-melting point eutectic oxide to enter a super-strong oxidation state. At this time, sodium nitrate decomposes to release nitric oxide to form sodium superoxide, until the molten liquid is completely converted into an aqueous solution state and no nitric oxide gas is discharged, thereby forming a low-melting point eutectic superoxide composed of sodium superoxide and sodium chromate.
[0043] (1) Adding ferrochrome powder to low-melting-point eutectic superoxide, the material forms a spherical mixture of solid and solid solution with a diameter of 0.1 cm to 3 cm due to the addition of cold material;
[0044] (2) Initially heating to 790°C~810°C to convert all the spherical materials mixed with solid and solid solution into a liquid-solid mixture, wherein the liquid is a low-melting-point eutectic superoxide melt and the solid is a ferrochrome powder. Then stopping heating and using the heat released by the strong oxidation reaction of the material to continuously raise the system temperature to 940°C~960°C. After the strong oxidation reaction is basically completed and the temperature in the kettle is gradually reduced to 890°C~910°C, heating again to a temperature of not less than 890°C and keeping the temperature to form a molten material. At this time, the elemental chromium in the ferrochrome powder is oxidized by sodium superoxide to sodium chromate, and the elemental iron reacts with the oxygen in the air to form red iron oxide.
[0045] (3) Forced water dissolution: obtaining a mixed slurry of dissolved sodium chromate and red iron oxide;
[0046] (4) Filtration and separation: obtain sodium chromate solution and red iron oxide.
[0047] Furthermore, S3 includes the following steps:
[0048] The acid solution reacts with the ferrochrome alloy powder and is heated to dissolve. Oxalic acid is added to the obtained mixed solution of ferrous salt and chromium salt, and ammonia water is added dropwise to adjust the pH value to 1-1.96, and the negative electrode solution is filtered to prepare.
[0049] Further, in step S4, the cathode liquid flow pump and the cathode liquid flow pump are started simultaneously.
[0050] Further, in step S5, the cathode liquid and the anode liquid recovered from the battery are mixed and then processed through the following steps:
[0051] S51, adding oxalic acid and dropping ammonia water to precipitate ferrous oxalate crystals and a mixed solution of chromium salt and ammonium salt and filtering;
[0052] S52, adding the bottom liquid into the reactor, and dropping the filtrate obtained in S51 and ammonia water into the reactor, stirring and reacting at the same time, to precipitate chromium hydroxide;
[0053] S53, preparing chromic anhydride comprises: uniformly stirring the obtained chromium hydroxide and a low melting point eutectic oxide, reacting at a high temperature to obtain solid sodium chromate, dissolving the solid sodium chromate with boiling water, adding dilute sulfuric acid or other acidic mother liquor to adjust the pH value, and then evaporating and filtering to obtain a sodium dichromate solution, adding concentrated sulfuric acid to the sodium dichromate solution and heating it to 200-205° C. to obtain a chromic anhydride product.
[0054] The beneficial effects of the present invention are as follows:
[0055] The chromium-iron liquid flow battery manufacturing process proposed in the present invention has the following significant beneficial effects:
[0056] 1. Solve the core problem and improve battery performance
[0057] Effectively inhibit hydrogen evolution reaction: By optimizing reaction conditions and additives, the phenomenon of hydrogen evolution at the negative electrode during charging is significantly reduced, thereby improving the coulombic efficiency and cycle life of the battery.
[0058] Reduce the mixing of positive and negative electrode liquid flows: Carefully designed battery stack structure and flow channels effectively prevent cross-contamination of positive and negative electrode liquid flows, ensuring long-term stable operation of the battery.
[0059] 2. Process optimization and cost reduction
[0060] Efficient production: By optimizing reaction conditions and process flow, production efficiency is improved and production cycle is reduced.
[0061] 3. Environmentally friendly and sustainable development
[0062] The process designs the recycling of electrolyte, reduces the consumption of raw materials and achieves sustainable development.
[0063] 4. Strong adaptability and wide application
[0064] Due to its modular design and scalability, it can adapt to the needs of large-scale energy storage and meet the needs of peak load and valley filling of the power grid.
[0065] 5. High safety and good reliability
[0066] Aqueous electrolyte: Using aqueous electrolyte has mild reaction conditions, high safety, and is not prone to safety accidents such as explosion.
[0067] Stable operation: Through careful process design and control, the long-term stable operation of the battery is guaranteed under the temperature conditions of 70℃~-40℃. DETAILED DESCRIPTION
[0068] 1. Preparation of cathode solution
[0069] Preparation of Red Iron Oxide
[0070] Using ferrochrome as raw material, red iron oxide is prepared by the following steps:
[0071] The ferrochrome alloy powder is added to the pre-prepared low-melting point eutectic super oxide, and the material forms a spherical object with a diameter of 0.1 cm to 3 cm, which is a mixture of solid and solid solution.
[0072] The mixture is heated to 790℃~810℃ to convert the spherical mixture of solid and solid melt into a liquid-solid mixture, and the heating is stopped. The system temperature is continuously raised to 940℃~960℃ by utilizing the heat released by the strong oxidation reaction of the material, and this temperature is maintained. After the reaction is basically completed, the temperature is raised again to not less than 890℃ and kept warm to form a molten material.
[0073] In this process, the elemental iron in the ferrochrome alloy powder is oxidized to generate red iron oxide. For detailed production process, those skilled in the art may refer to the production process disclosed in CN116986633A.
[0074] Preparation of cathode solution
[0075] The prepared red iron oxide is added into hydrochloric acid to react and generate a cathode solution.
[0076] Reactants: ferric iron (Fe³⁺)
[0077] Reaction process: During discharge, trivalent iron ions accept electrons at the positive electrode and are reduced to divalent iron ions.
[0078] Chemical equation:
[0079] Fe 3+ +𝑒 − →Fe 2+
[0080] The reverse reaction during charging: the divalent iron ions lose electrons and are reoxidized to trivalent iron ions.
[0081] Chemical equation:
[0082] Fe 2+ →Fe 3+ +𝑒 −
[0083] 2. Preparation of negative electrode solution
[0084] Acid dissolution of ferrochrome
[0085] Under the protection of inert gas, the ferrochrome alloy powder is added into hydrochloric acid for acid dissolution to generate chromite ion (Cr²⁺) acid solution.
[0086] Oxalic acid treatment
[0087] The acid solution is reacted with oxalic acid, and then ammonia water is added dropwise to adjust the pH value to 1-1.96. The ferrous oxalate precipitate is filtered to obtain the ferrous oxalate precipitate, and the solution containing divalent chromium ions is retained as the negative electrode solution.
[0088] Reactants: Divalent chromium ions (Cr²⁺)
[0089] Reaction process: During discharge, divalent chromium ions lose electrons at the negative electrode and are oxidized to trivalent chromium ions.
[0090] Chemical equation:
[0091] Cr 2+ →Cr 3+ +𝑒 −
[0092] The reverse reaction during charging: trivalent chromium ions accept electrons and are reduced to divalent chromium ions.
[0093] Chemical equation:
[0094] Cr 3+ +𝑒 − →Cr 2+
[0095] 3. Battery Assembly
[0096] Addition of positive and negative electrolytes
[0097] The prepared cathode solution and anode solution are added into the cathode and anode solution storage tanks of the iron-chromium liquid flow battery respectively.
[0098] Starting battery
[0099] The liquid flow pump of the iron-chromium flow battery is started to allow the positive and negative liquids to enter the battery stack respectively for redox reactions. During the discharge process, the external circuit generates current and the battery starts to work.
[0100] Charging process
[0101] When charging, the battery is charged through an external power source, the divalent iron ions in the positive electrode liquid are oxidized to trivalent iron ions, and the trivalent chromium ions in the negative electrode liquid are reduced to divalent chromium ions, and the battery is converted from the primary battery mode to the energy storage battery mode.
[0102] 4. Solution Recovery and Treatment
[0103] After the positive and negative solutions of the iron-chromium flow battery have undergone more than 1,000 charge and discharge cycles, the solutions are recycled to prepare chromic anhydride and ferrous oxalate. The specific steps are as follows:
[0104] Oxalic acid precipitation
[0105] The positive electrode solution recovered after discharge is mixed with the negative electrode solution, oxalic acid is added and ammonia water is added dropwise to precipitate ferrous oxalate crystals.
[0106] Preparation of chromium hydroxide
[0107] Add the base liquid to the mixed solution, and drop ammonia water to adjust the pH value to precipitate chromium hydroxide.
[0108] Preparation of chromic anhydride
[0109] Chromium hydroxide is mixed with a low melting point eutectic oxide and reacted at high temperature to obtain solid sodium chromate. Then, the pH value is adjusted with hydrochloric acid, and a sodium dichromate solution is obtained by evaporation and filtration, and finally a chromic anhydride product is prepared by reaction with concentrated sulfuric acid. Those skilled in the art can refer to the technical solution disclosed in CN112429776A for the detailed operation process.
[0110] In the above embodiment, taking the power demand: 0.5 MW and the energy storage capacity: 1 MWh as an example:
[0111] 1. Volume of positive and negative electrolytes
[0112] The energy storage capacity determines the required electrolyte volume. Assuming the energy density of the electrolyte is about 40 Wh / L (typical value, the specific density depends on the chemical composition and concentration of the electrolyte), you need:
[0113] Total liquid volume = 1000 kWh / 40 Wh / L = 25000 L = 25 m3
[0114] Because the liquid is recycled, this volume needs to be divided between the positive and negative electrolytes, usually a 1:1 split, so each electrolyte requires about 12.5 m³.
[0115] 2. Number of battery stacks
[0116] The number of stacks determines the power output of the battery. Assuming that each stack can provide about 10 kW of power (the power density of a common iron-chromium flow battery stack is about 0.1 W / cm² of electrode area, and each stack has an effective electrode area of 1000 cm²), the number of stacks required is:
[0117] Number of battery stacks = 500 kW / 10 kW / battery stack = 50 stacks
[0118] 3. Electrode area
[0119] The power output of a stack is related to the electrode area. Assuming the electrode area is 1000 cm² (per stack), the total electrode area of 50 stacks is:
[0120] Total electrode area = 50 stacks × 1000 cm2 = 50000 cm2 = 5 m2
[0121] 4. Liquid flow rate
[0122] The liquid flow rate should match the reaction rate and power requirements. Assuming the flow rate requirement for each stack is 10 L / min, the total flow rate requirement is:
[0123] Total flow rate = 50 stacks × 10 L / min = 500 L / min
[0124] This means that the positive and negative solutions each require a flow rate of 500 L / min, and the flow rate can be adjusted by pump control.
[0125] 5. Tank size
[0126] The tanks should be sized to hold the required electrolyte volume with an appropriate margin. Approximately 12.5 m³ of tank is required for each liquid, but some additional capacity is usually added for system safety and buffer. It is recommended that each tank be designed for at least 15 m³.
[0127] 6. Pump selection
[0128] The pump needs to support the required flow rate and pressure. Ensure that the pump can operate continuously and can cope with pressure changes under different load conditions. Redundant pumps are usually required to ensure system reliability.
[0129] 7. Other Components
[0130] Pipes and Valves: Corrosion-resistant materials should be selected, the diameter of the pipes should be large enough to support the flow of liquid, and the valves should facilitate the control and regulation of the flow rate.
[0131] Cooling system: Since the electrochemical reaction generates heat, a cooling system is required to maintain the appropriate operating temperature.
[0132] Control system: used to monitor and regulate the battery's operating parameters such as voltage, current, flow rate and temperature.
[0133] 8. Iron and chromium ion concentrations in the electrolyte
[0134] Assume that the concentrations of iron and chromium ions in the electrolyte are:
[0135] Iron ion (Fe³⁺): 1 mol / L
[0136] Chromium ion (Cr²⁺): 1 mol / L
[0137] 9. Volume of electrolyte
[0138] From previous calculations, we determined that we would need approximately 12.5 m³ (or 12,500 L) of each electrolyte.
[0139] 3. Molar amounts of iron and chromium required
[0140] For the iron:
[0141] For ease of calculation, in this embodiment, it is assumed that the molar concentration of iron ions and the molar concentration of chromium ions are 1 mol / L, and the actual concentrations are lower than 1 mol / L.
[0142] Moles of iron = iron ion concentration × cathode liquid volume = 1 mol / L × 12500 L = 12500 mol
[0143] For Chrome:
[0144] Moles of chromium = chromium ion concentration × cathode liquid volume = 1 mol / L × 12500 L = 12500 mol
[0145] 4. Calculate the amount of reaction materials required
[0146] a. Iron source
[0147] Assuming the iron source is red iron oxide (Fe2O3), its molar mass is 159.69 g / mol:
[0148] Required iron oxide red = number of moles of iron × 159.69 g / mol / 2 = 12500 × 159.69 / 2 = 997937.5 g = 997.94 kg
[0149] b. Chromium source
[0150] Assuming the chromium source is ferrochrome (FeCr) with a chromium content of 54%, its molar mass is assumed to be about 52 g / mol (considering only chromium):
[0151] Required ferrochrome = number of moles of chromium × 52 g / mol / 0.54 = 12500 × 52 / 0.54 = 1203703.7 g = 1203.7 kg
[0152] 5. Acid requirement
[0153] Using hydrochloric acid as the acidifying agent, the amount of acid required can be estimated by balancing the chemical equation. Assuming that 1 mol of Fe2O3 requires 6 mol of hydrochloric acid for the acidification reaction:
[0154] Hydrochloric acid required = number of moles of iron × 6 = 12500 × 6 = 75000 mol
[0155] The molar mass of hydrochloric acid (HCl) is 36.46 g / mol:
[0156] Mass of hydrochloric acid = 75000 × 36.46 g / mol = 2734500 g = 2734.5 kg
[0157] 6. Other raw materials
[0158] Depending on the detailed chemical steps of the process, the amount of other auxiliary reagents such as sodium hydroxide and ammonia may also need to be considered. The specific amount needs to be accurately calculated based on the chemical reaction equation in the process flow and the chemical measurement of each step.
[0159] Summarize
[0160] To achieve the energy storage requirement of 0.5 MW / 1 MWh, the required raw materials are estimated as follows:
[0161] Red iron oxide (Fe2O3): about 997.94 kg
[0162] Ferrochrome (FeCr): about 1,203.7 kg
[0163] Hydrochloric acid (HCl): about 2,734.5 kg.
Claims
1. A method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material, characterized in that: The following steps are included: S1: Produce red iron oxide using ferrochrome as raw material; S2: adding the red iron oxide obtained in S1 to one or more of sulfuric acid, nitric acid or hydrochloric acid to form a cathode solution; S3: dissolving the ferrochrome alloy in an acid solution under the protection of an inert gas and separating the oxalic acid to obtain a cathode solution; S4: adding the positive electrode liquid and the negative electrode liquid produced above into the positive and negative electrode solution storage tanks of the iron-chromium liquid flow battery respectively; starting the liquid flow pump of the iron-chromium liquid flow battery; when the two liquid flows enter the battery stack, a redox reaction occurs and the external circuit generates current discharge, that is, a primary battery is formed; When connected to an external power source, the positive electrode liquid of the discharged primary battery is reduced from trivalent to divalent, and the negative electrode liquid is oxidized from divalent to trivalent by itself, and then transformed into an energy storage battery; S5: When the number of charge and discharge times of the positive and negative electrode solutions of the iron-chromium flow battery reaches more than 1,000 times, the solution is recovered and processed to prepare chromic anhydride and ferrous oxalate.
2. The method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material according to claim 1, characterized in that: S1 includes the following steps: S11. Preparing a low melting point eutectic oxide; S12. Preparation of low melting point eutectic super oxide; S13. Prepare sodium chromate solution and red iron oxide.
3. The method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material according to claim 2, characterized in that: Preparation of low melting point eutectic oxide: Sodium nitrate and sodium chromate are used as raw materials, heated to 630°C~640°C and maintained until all the materials form a molten liquid to obtain a low melting point eutectic oxide; Preparation of low-melting point eutectic superoxide: Stop heating the low-melting point eutectic oxide and cool the material to 590°C~610°C and maintain it, while blowing air in to cause the low-melting point eutectic oxide to enter a super-strong oxidation state. At this time, sodium nitrate decomposes to release nitric oxide to form sodium superoxide, until the molten liquid is completely converted into an aqueous solution and no nitric oxide gas is discharged, thereby forming a low-melting point eutectic superoxide composed of sodium superoxide and sodium chromate.
4. The method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material according to claim 1, characterized in that: S3 includes the following steps: The acid solution reacts with the ferrochrome alloy powder and is heated to dissolve. Oxalic acid is added to the obtained mixed solution of ferrous salt and chromium salt, and ammonia water is added dropwise to adjust the pH value to 1-1.
96. The ferrous oxalate crystals are filtered out to obtain a filtrate as the negative electrode liquid.
5. The method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material according to claim 1, characterized in that: In step S4, the cathode liquid flow pump and the cathode liquid flow pump are started simultaneously.
6. The method for preparing an iron-chromium liquid flow primary battery and an energy storage battery using an iron-chromium alloy as a raw material according to claim 1, characterized in that: In step S5, the positive electrode liquid and the negative electrode liquid recovered from the battery are mixed and then processed through the following steps: S51, adding oxalic acid and dropping ammonia water to precipitate ferrous oxalate crystals and a mixed solution of chromium salt and ammonium salt and filtering; S52, adding the bottom liquid into the reactor, and dropping the filtrate obtained in S51 and ammonia water into the reactor, stirring and reacting at the same time, to precipitate chromium hydroxide; S53, preparing chromic anhydride comprises: uniformly stirring the obtained chromium hydroxide and a low melting point eutectic oxide, reacting at a high temperature to obtain solid sodium chromate, dissolving the solid sodium chromate with boiling water, adding dilute sulfuric acid or other acidic mother liquor to adjust the pH value, and then evaporating and filtering to obtain a sodium dichromate solution, adding concentrated sulfuric acid to the sodium dichromate solution and heating it to 200-205° C. to obtain a chromic anhydride product.