Method for producing hydrogenated polymer

By pre-reduction of the catalyst, the hydrogenation reaction speed of the aromatic vinyl compound-based polymer is improved, and the problem of insufficient heat resistance in the prior art is solved, and efficient and heat resistance hydrogenated polymer production is achieved.

CN118984841AInactive Publication Date: 2024-11-19MITSUBISHI GAS CHEM CO INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380033030.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-11
Filing Date
2023-04-10
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The heat resistance of existing styrene cyclic hydrides and copolymers such as styrene/isoprene is insufficient, and the aromatic ring hydrogenation reaction of aromatic vinyl compound-based polymers takes a long time to achieve high cyclic hydrogenation rate. .

Method used

By pre-reduction of the catalyst, the hydrogenation reaction speed is increased, and the aromatic vinyl compound-based polymer, solvent and reduction-treated hydrogenation catalyst are used to perform hydrogenation reaction, thereby shortening the reaction time.

Benefits of technology

The efficient production of hydrogenated polymers with sufficient heat resistance is achieved, and damage to the polymer is reduced by reducing molecular weight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005074591030000241
    Figure BDA0005074591030000241
  • Figure BDA0005074591030000242
    Figure BDA0005074591030000242
  • Figure HDA0005074591040000011
    Figure HDA0005074591040000011
Patent Text Reader

Abstract

Provided is a method for hydrogenation (ring hydrogenation) of an aromatic ring of an aromatic vinyl compound-based polymer for obtaining a hydrogenated polymer having sufficient heat resistance at a high ring hydrogenation rate. More specifically, the present invention provides a method for producing a hydrogenated polymer by hydrogenation (ring hydrogenation) of an aromatic ring of an aromatic vinyl compound-based polymer, characterized in that a hydrogenation catalyst is reduced before use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a hydrogenated polymer. More specifically, the present invention relates to a method for producing a hydrogenated polymer by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation). Background Art

[0002] In recent years, polymers represented by acrylic resins, methacrylic resins, styrene resins, polycarbonate resins, and cyclic polyolefin resins have been used for various purposes, particularly due to their optical properties, as a lot of demands for optical materials such as optical lenses and optical disc substrates. Such optical materials not only require high transparency, but also require high heat resistance, low water absorption, high performance with excellent balance of mechanical properties, etc. In order to cope with such demand, various improvements of polymers have been carried out, and as an example of such improvement, hydrogenation (ring hydrogenation) of aromatic polymers can be cited.

[0003] For example, Japanese Patent No. 5540703 (Patent Document 1) relates to the hydrogenation of aromatic vinyl compounds / (meth)acrylate copolymers, and Japanese Patent Publication No. 2014-77044 (Patent Document 2) relates to a method for producing a ring-hydrogenated polymer using a sulfur-free raw material. In addition, Japanese Patent No. 2890748 (Patent Document 3) relates to a method for producing a hydrogenated styrene resin, and Japanese Patent Publication No. 2001-527095 (Patent Document 4), Japanese Patent Publication No. 2002-511501 (Patent Document 5), and Japanese Patent Publication No. 2002-511508 (Patent Document 6) relate to methods for hydrogenating aromatic polymers. Japanese Patent No. 4224655 (Patent Document 7) and Japanese Patent No. 5007688 (Patent Document 8) relate to alicyclic hydrocarbon copolymers or polymers containing an alicyclic structure, and describe that these polymers can be obtained by hydrogenating aromatic polymers.

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 5540703

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-77044

[0008] Patent Document 3: Japanese Patent No. 2890748

[0009] Patent Document 4: Japanese Patent Application No. 2001-527095

[0010] Patent Document 5: Japanese Patent Publication No. 2002-511501

[0011] Patent Document 6: Japanese Patent Application No. 2002-511508

[0012] Patent Document 7: Japanese Patent No. 4224655

[0013] Patent Document 8: Japanese Patent No. 5007688 Summary of the invention

[0014] Technical problem to be solved by the invention

[0015] However, the heat resistance of the ring hydrogenated products of styrene and the ring hydrogenated products of copolymers such as styrene / isoprene that have been used so far is not satisfactory. In addition, in the method of hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation), a long reaction time is required to achieve a high ring hydrogenation rate.

[0016] Technical means for solving technical problems

[0017] The inventors of the present invention have conducted intensive studies and have found that in a method for producing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation), the reaction rate is increased by pre-reducing the catalyst used in the reaction, thereby completing the present invention.

[0018] That is, the present invention includes the following aspects.

[0019] <1> A method for producing a hydrogenated polymer, comprising hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer to produce a hydrogenated polymer, wherein:

[0020] The aromatic vinyl compound-based polymer comprises a first monomer unit and a second monomer unit.

[0021] The above methods include:

[0022] A step of reducing the hydrogenation catalyst before use; and

[0023] A step of obtaining a hydrogenated polymer by conducting a hydrogenation reaction using the aromatic vinyl compound-based polymer, a solvent and a reduction-treated hydrogenation catalyst,

[0024] The solvent is a mixed solvent comprising at least one first solvent and at least one second solvent,

[0025] The first solvent is a solvent that dissolves the aromatic vinyl compound polymer before hydrogenation.

[0026] The second solvent is a solvent that dissolves the hydrogenated polymer.

[0027] <2> according to <1> In the method for producing a hydrogenated polymer, the at least one first solvent comprises one or more selected from methyl acetate, ethyl acetate, butyl acetate and methyl isobutyrate.

[0028] <3> according to <1> or <2> The method for producing a hydrogenated polymer, wherein the at least one second solvent comprises one or more selected from cyclohexane, C9-C10 alkylcyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane.

[0029] <4> according to <1> ~ <3> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein the first solvent has a boiling point of 50° C. or higher and a flash point of 400° C. or higher.

[0030] <5> according to <1> ~ <4> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein the second solvent has a boiling point of 80° C. or higher and a flash point of 230° C. or higher.

[0031] <6> according to <1> ~ <5> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein the first monomer is selected from the group consisting of styrene, α-methylstyrene, chlorostyrene, 4-methylstyrene, 4-tert-butylstyrene and 4-methoxystyrene.

[0032] <7> according to <1> ~ <6> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein the second monomer is selected from the group consisting of maleic anhydride, butadiene, cyclopentadiene and isoprene.

[0033] <8> according to <1> ~ <7> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein the aromatic vinyl compound-based polymer is selected from the group consisting of a copolymer of styrene and maleic anhydride, a copolymer of styrene and butadiene, and a copolymer of styrene and isoprene.

[0034] <9> according to <8> In the method for producing a hydrogenated polymer, the aromatic vinyl compound-based polymer is a copolymer of styrene and maleic anhydride.

[0035] <10> according to <1> ~ <9> The method for producing a hydrogenated polymer as described in any one of the above, wherein in the aromatic vinyl compound-based polymer, a polymerization ratio (mol %) of the first monomer unit to the second monomer unit is 70:30 or more and less than 100:0.

[0036] <11> according to <1> ~ <10> The method for producing a hydrogenated polymer according to any one of the preceding claims, further comprising the step of forming a polymer resin by devolatilization extrusion after the hydrogenation reaction.

[0037] <12> according to <1> ~ <11> The method for producing a hydrogenated polymer according to any one of the preceding claims, further comprising a concentration step between the hydrogenation reaction and the devolatilization extrusion.

[0038] <13> according to <1> ~ <12> The method for producing a hydrogenated polymer according to any one of the preceding claims, wherein a mass ratio of the at least one first solvent to the at least one second solvent (first solvent:second solvent) is 1:9 to 9:1.

[0039] <14> according to <1> ~ <13> The method for producing a hydrogenated polymer according to any one of the above, wherein the hydrogenation catalyst is a solid catalyst carrying palladium, platinum, ruthenium, rhodium or nickel.

[0040] <15> A method for manufacturing an optical material, comprising: <1> ~ <14> The method for producing a hydrogenated polymer according to any one of the above.

[0041] <16> according to <15> The method for manufacturing an optical material, wherein the optical material is an optical lens.

[0042] Effects of the Invention

[0043] According to the method of the present invention, a method for producing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation) is provided, and the speed of the hydrogenation reaction is increased, so that the hydrogenated polymer can be produced efficiently. Moreover, by shortening the reaction time, damage to the polymer such as molecular weight reduction can be reduced. By the method of the present invention, a hydrogenated polymer with sufficient heat resistance can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The relationship between the hydrogenation reaction time of resin 1 and the hydrogenation rate on the ring is shown. DETAILED DESCRIPTION

[0045] The present invention will be described in detail below. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various ways without departing from the gist of the present invention.

[0046] <Method for producing hydrogenated polymer>

[0047] In an embodiment of the present invention, there is provided a method for producing a hydrogenated polymer by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation).

[0048] In one embodiment of the present invention, there is provided a method for producing a hydrogenated polymer, wherein the hydrogenated polymer is produced by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer, wherein:

[0049] The aromatic vinyl compound-based polymer comprises a first monomer unit and a second monomer unit.

[0050] The above methods include:

[0051] A step of reducing the hydrogenation catalyst before use; and

[0052] A step of obtaining a hydrogenated polymer by conducting a hydrogenation reaction using the aromatic vinyl compound-based polymer, a solvent, and a reduction-treated hydrogenation catalyst.

[0053] <Aromatic vinyl compound polymer>

[0054] The manufacturing method of certain embodiments of the present invention relates to a method for manufacturing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer. In this specification, "aromatic vinyl compound-based polymer" refers to a polymer containing units derived from aromatic vinyl compounds as structural units. Therefore, the aromatic vinyl compound-based polymer can be a polymer (homopolymer) formed by units derived from one aromatic vinyl compound, or a copolymer containing units derived from two or more aromatic vinyl compounds as structural units, or containing units derived from one or more aromatic vinyl compounds and units derived from one or more compounds other than aromatic vinyl compounds as structural units. The unit derived from an aromatic vinyl compound refers to a unit having a structure in which the C=C double bond of the vinyl group in the aromatic vinyl compound is disconnected due to polymerization.

[0055] In one embodiment of the present invention, the aromatic vinyl compound-based polymer includes a first monomer unit and a second monomer unit.

[0056] (monomer)

[0057] The aromatic vinyl compound polymer used in the manufacturing method of certain embodiments of the present invention is not particularly limited, and the following compounds can be cited as the aromatic vinyl compound monomer: styrene; alkyl styrenes such as α-methylstyrene, α-ethylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 1,3-dimethylstyrene, and p-tert-butylstyrene (the number of carbon atoms in the alkyl part is preferably 1 to 5); p-hydroxystyrene; alkoxystyrenes such as p-methoxystyrene, m-butoxystyrene, and p-butoxystyrene (the number of carbon atoms in the alkoxy part is preferably 1 to 5); halogenated styrenes such as o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4-dichlorostyrene, and 2,6-dichlorostyrene; vinylnaphthalene and vinylanthracene, but are not limited to these. These monomers can be used alone or in combination. In a preferred embodiment of the present invention, styrene is used as the aromatic vinyl compound monomer.

[0058] In one embodiment of the present invention, the first monomer is a monomer derived from an aromatic vinyl compound. In one embodiment of the present invention, the first monomer is selected from styrene, α-methylstyrene, chlorostyrene, 4-methylstyrene, 4-tert-butylstyrene and 4-methoxystyrene. In a preferred embodiment of the present invention, the first monomer is styrene.

[0059] The aromatic vinyl compound polymer used in the manufacturing method of some embodiments of the present invention is a polymer using monomers of compounds other than aromatic vinyl compounds in addition to aromatic vinyl compound monomers. As monomers of compounds other than aromatic vinyl compounds, (meth)acrylates, dienes, and acid anhydrides can be cited, but are not limited to these. As (meth)acrylates, for example:

[0060] Alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, dodecyl (meth)acrylate, and octadecyl (meth)acrylate (the number of carbon atoms in the alkyl portion is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5);

[0061] Cycloalkyl (meth)acrylates or cyclic saturated hydrocarbon esters such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate (the number of ring carbon atoms in both esters is preferably 5 to 20, more preferably 5 to 10);

[0062] Hydroxyalkyl (meth)acrylates such as (2-hydroxyethyl) (meth)acrylate, (2-hydroxypropyl) (meth)acrylate, and (2-hydroxy-2-methylpropyl) (meth)acrylate (the number of carbon atoms in the alkyl portion is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5);

[0063] Alkoxyalkyl (meth)acrylates such as (2-methoxyethyl) (meth)acrylate and (2-ethoxyethyl) (meth)acrylate (the number of carbon atoms in the alkyl portion is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5, and the number of carbon atoms in the alkoxy portion is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 or 2);

[0064] Phenyl (meth)acrylate and other phenyl (meth)acrylates;

[0065] Arylalkyl (meth)acrylates such as benzyl (meth)acrylate (the number of carbon atoms in the aryl portion is preferably 6 to 10, and the number of carbon atoms in the alkyl portion is preferably 1 to 5);

[0066] (Meth)acrylates having a phospholipid structure such as 2-(meth)acryloyloxyethyl phosphorylcholine, etc., but not limited to these. The (meth)acrylates may be used alone or in combination of two or more. As the (meth)acrylate, methyl (meth)acrylate is preferred.

[0067] Examples of dienes include, but are not limited to, 1,2-butadiene, 1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,2-hexadiene, 1,3-hexadiene, 1,4-hexadiene, 1,5-hexadiene, 1,3-heptadiene, 1,3-octadiene, 1,3-nonadiene, 1,3-decadiene, isoprene, cyclopentadiene, 1,3-cyclohexadiene, and 1,4-cyclohexadiene. One type of diene may be used alone, or two or more types may be used in combination. As diene, conjugated dienes such as 1,3-butadiene or isoprene are preferred.

[0068] Examples of the acid anhydride include, but are not limited to, anhydrides of maleic acid, itaconic acid, citraconic acid, and aconitic acid. Among them, maleic anhydride is preferred.

[0069] In one embodiment of the present invention, the second monomer is a monomer derived from a conjugated diene compound. In one embodiment of the present invention, the second monomer is selected from maleic anhydride, butadiene, cyclopentadiene and isoprene. In a preferred embodiment of the present invention, the second monomer is maleic anhydride.

[0070] The aromatic vinyl compound polymer used in the production method of certain embodiments of the present invention may contain monomers other than the first monomer and the second monomer as constituent components, as long as the effects of the present invention are not impaired. In the aromatic vinyl compound polymer, for example, the monomer components other than the first monomer and the second monomer may be contained in an amount of 0 to 10% or 0 to 5% by molar ratio relative to all monomer components.

[0071] In a preferred embodiment of the present invention, the aromatic vinyl compound-based polymer includes one or more selected from the copolymers of styrene and butadiene (1,2-butadiene, 1,3-butadiene or a combination thereof), copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene. In another preferred embodiment of the present invention, the aromatic vinyl compound-based polymer is a polymer selected from the copolymers of styrene and butadiene (1,2-butadiene, 1,3-butadiene or a combination thereof), copolymers of styrene and isoprene, copolymers of styrene and methyl methacrylate, copolymers of styrene and maleic anhydride, copolymers of styrene and vinyl acetate, and polystyrene. These polymers can be polymerized from each monomer as described later, or commercial products can be used. For example, as polystyrene, "GPPS HF77" produced by PS Japan can be used.

[0072] In one embodiment of the present invention, the aromatic vinyl compound polymer is selected from copolymers of styrene and maleic anhydride, copolymers of styrene and butadiene, and copolymers of styrene and isoprene. In a preferred embodiment of the present invention, the aromatic vinyl compound polymer is a copolymer of styrene and maleic anhydride.

[0073] (Method for producing aromatic vinyl compound-based polymer)

[0074] Aromatic vinyl compound-based polymers can be produced by polymerizing various monomers. There are no particular limitations on the method of polymerizing one or more aromatic vinyl compounds or the method of copolymerizing an aromatic vinyl compound with a monomer other than an aromatic vinyl compound monomer, and known methods such as free radical polymerization, ionic polymerization, and coordination polymerization can be used. In industry, free radical polymerization is preferred due to its simplicity. As a free radical polymerization method, known methods such as bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization can be appropriately selected. For example, as an example of bulk polymerization or solution polymerization, there is a continuous polymerization method, in which a monomer composition mixed with monomer components, a chain transfer agent, and a polymerization initiator (and a solvent further added during solution polymerization) is continuously supplied to a complete mixing tank, and polymerization is carried out at 100 to 180°C. As the solvent used in the solution polymerization method, for example:

[0075] Hydrocarbon solvents such as toluene, xylene, cyclohexane, methylcyclohexane, etc.

[0076] Ester solvents such as ethyl acetate;

[0077] Ketone solvents such as acetone and butanone;

[0078] Ether solvents such as tetrahydrofuran and 1,4-dioxane;

[0079] The reaction mixture after polymerization is taken out from the complete mixing tank, and then introduced into a devolatilization extruder or a reduced pressure devolatilization tank to distill off volatile components (monomer components and solvent, etc.), thereby obtaining a polymer of an aromatic vinyl compound or a copolymer of an aromatic vinyl compound and a monomer other than the aromatic vinyl compound monomer (also collectively referred to as "aromatic vinyl compound-based polymer").

[0080] In one embodiment of the present invention, the polymerization ratio (mol %) of the first monomer unit to the second monomer unit constituting the aromatic vinyl compound-based polymer may be 70:30 or more and less than 100:0.

[0081] In an embodiment of the present invention, the polymerization ratio (mol %) of the first monomer unit and the second monomer unit constituting the aromatic vinyl compound-based polymer can be, for example, 70:30 or more, 75:25 or more, 80:20 or more, 85:15 or more, 86:14 or more, 87:13 or more, 88:12 or more, 89:11 or more, 90:10 or more, 91:9 or more, 92:8 or more, 93:7 or more, 94:6 or more, 95:5 or more, 96:4 or more, 97:3 or more, 98:2 or more, or 99:1 or more.

[0082] In an embodiment of the present invention, the polymerization ratio (mol %) of the first monomer unit and the second monomer unit constituting the aromatic vinyl compound-based polymer can be, for example, less than 100:0, less than 99:1, less than 98:2, less than 97:3, less than 96:4, less than 95:5, less than 94:6, less than 93:7, less than 92:8, less than 91:9, less than 90:10, less than 89:11, less than 88:12, less than 87:13, less than 86:14, less than 85:15, less than 80:20, or less than 75:25.

[0083] In one embodiment of the present invention, the polymerization ratio (mol%) of the first monomer unit and the second monomer unit constituting the aromatic vinyl compound-based polymer is 70:30 or more and less than 100:0. In an embodiment of the present invention, the polymerization ratio (mol%) of the first monomer unit and the second monomer unit constituting the aromatic vinyl compound-based polymer may be, for example, 70:30 or more and less than 100:0, 75:25 or more and less than 100:0, 80:20 or more and less than 100:0, 85:15 or more and less than 100:0, 86:14 or more and less than 100:0, 87:13 or more and less than 100:0, 88:12 or more and less than 100:0. ∶0, 89:11 or more and less than 100:0, 90:10 or more and less than 100:0, 91:9 or more and less than 100:0, 92:8 or more and less than 100:0, 93:7 or more and less than 100:0, 94:6 or more and less than 100:0, 95:5 or more and less than 100:0, 96:4 or more and less than 100:0, 97:3 or more and less than 100:0, 98:2 or more and less than 100:0, 99:1 or more and less than 100:0;

[0084] 70:30 or more and less than 99:1, 75:25 or more and less than 99:1, 80:20 or more and less than 99:1, 85:15 or more and less than 99:1, 86:14 or more and less than 99:1, 87:13 or more and less than 99:1, 88:12 or more and less than 99:1, 89:11 or more and less than 99:1, 90:10 or more and less than 99:1, 91:9 or more and less than 99:1, 92:8 or more and less than 99:1, 93:7 or more and less than 99:1, 94:6 or more and less than 99:1, 95:5 or more and less than 99:1, 96:4 or more and less than 99:1, 97:3 or more and less than 99:1, 98:2 or more and less than 99:1;

[0085] 70:30 or more and less than 98:2, 75:25 or more and less than 98:2, 80:20 or more and less than 98:2, 85:15 or more and less than 98:2, 86:14 or more and less than 98:2, 87:13 or more and less than 98:2, 88:12 or more and less than 98:2, 89:11 or more and less than 98:2, 90:10 or more and less than 98:2, 91:9 or more and less than 98:2, 92:8 or more and less than 98:2, 93:7 or more and less than 98:2, 94:6 or more and less than 98:2, 95:5 or more and less than 98:2, 96:4 or more and less than 98:2, 97:3 or more and less than 98:2;

[0086] 70:30 or more and less than 97:3, 75:25 or more and less than 97:3, 80:20 or more and less than 97:3, 85:15 or more and less than 97:3, 86:14 or more and less than 97:3, 87:13 or more and less than 97:3, 88:12 or more and less than 97:3, 89:11 or more and less than 97:3, 90:10 or more and less than 97:3, 91:9 or more and less than 97:3, 92:8 or more and less than 97:3, 93:7 or more and less than 97:3, 94:6 or more and less than 97:3, 95:5 or more and less than 97:3, 96:4 or more and less than 97:3;

[0087] 70:30 or more and less than 96:4, 75:25 or more and less than 96:4, 80:20 or more and less than 96:4, 85:15 or more and less than 96:4, 86:14 or more and less than 96:4, 87:13 or more and less than 96:4, 88:12 or more and less than 96:4, 89:11 or more and less than 96:4, 90:10 or more and less than 96:4, 91:9 or more and less than 96:4, 92:8 or more and less than 96:4, 93:7 or more and less than 96:4, 94:6 or more and less than 96:4, 95:5 or more and less than 96:4;

[0088] 70:30 or more and less than 95:5, 75:25 or more and less than 95:5, 80:20 or more and less than 95:5, 85:15 or more and less than 95:5, 86:14 or more and less than 95:5, 87:13 or more and less than 95:5, 88:12 or more and less than 95:5, 89:11 or more and less than 95:5, 90:10 or more and less than 95:5, 91:9 or more and less than 95:5, 92:8 or more and less than 95:5, 93:7 or more and less than 95:5, 94:6 or more and less than 95:5;

[0089] 70:30 or more and less than 94:6, 75:25 or more and less than 94:6, 80:20 or more and less than 94:6, 85:15 or more and less than 94:6, 86:14 or more and less than 94:6, 87:13 or more and less than 94:6, 88:12 or more and less than 94:6, 89:11 or more and less than 94:6, 90:10 or more and less than 94:6, 91:9 or more and less than 94:6, 92:8 or more and less than 94:6, 93:7 or more and less than 94:6;

[0090] 70:30 or more but less than 93:7, 75:25 or more but less than 93:7, 80:20 or more but less than 93:7, 85:15 or more but less than 93:7, 86:14 or more but less than 93:7, 87:13 or more but less than 93:7, 88:12 or more but less than 93:7, 89:11 or more but less than 93:7, 90:10 or more but less than 93:7, 91:9 or more but less than 93:7, 92:8 or more but less than 93:7;

[0091] 70:30 or more but less than 92:8, 75:25 or more but less than 92:8, 80:20 or more but less than 92:8, 85:15 or more but less than 92:8, 86:14 or more but less than 92:8, 87:13 or more but less than 92:8, 88:12 or more but less than 92:8, 89:11 or more but less than 92:8, 90:10 or more but less than 92:8, 91:9 or more but less than 92:8;

[0092] 70:30 or more but less than 91:9, 75:25 or more but less than 91:9, 80:20 or more but less than 91:9, 85:15 or more but less than 91:9, 86:14 or more but less than 91:9, 87:13 or more but less than 91:9, 88:12 or more but less than 91:9, 89:11 or more but less than 91:9, 90:10 or more but less than 91:9;

[0093] 70:30 to 90:10, 75:25 to 90:10, 80:20 to 90:10, 85:15 to 90:10, 86:14 to 90:10, 87:13 to 90:10, 88:12 to 90:10, 89:11 to 90:10;

[0094] 70:30 to 89:11, 75:25 to 89:11, 80:20 to 89:11, 85:15 to 89:11, 86:14 to 89:11, 87:13 to 89:11, 88:12 to 89:11;

[0095] 70:30 to 88:12, 75:25 to 88:12, 80:20 to 88:12, 85:15 to 88:12, 86:14 to 88:12, 87:13 to 88:12;

[0096] 70:30 to 87:13, 75:25 to 87:13, 80:20 to 87:13, 85:15 to 87:13, 86:14 to 87:13;

[0097] 70:30 to 86:14, 75:25 to 86:14, 80:20 to 86:14, 85:15 to 86:14;

[0098] 70:30 or more but less than 85:15, 75:25 or more but less than 85:15, 80:20 or more but less than 85:15;

[0099] 70:30 or more but less than 80:20, 75:25 or more but less than 80:20;

[0100] Any one of 70:30 or more and 75:25 or less.

[0101] The weight average molecular weight of the aromatic vinyl compound-based polymer used in certain embodiments of the present invention is preferably 10,000 to 1,000,000, more preferably 50,000 to 700,000, further preferably 100,000 to 500,000, and particularly preferably 130,000 to 250,000. Although polymers less than 10,000 or more than 1,000,000 can also be hydrogenated on the ring by the method of certain embodiments of the present invention, the mechanical strength of the copolymer with a weight average molecular weight within the above range is sufficient to withstand actual use, and the viscosity is moderate and easy to operate, so it is more preferred. Among them, in this specification, the weight average molecular weight is a value obtained by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent and converted to polystyrene.

[0102] <Hydrogenation>

[0103] In this specification, "hydrogenation of an aromatic vinyl compound polymer" refers to a reaction in which hydrogen is added to the aromatic ring of an aromatic vinyl compound polymer, for example, reduction of a benzene ring to cyclohexane. Such hydrogenation is also referred to as ring hydrogenation or ring hydrogenation.

[0104] (Solvent)

[0105] The aromatic vinyl compound polymer used in some embodiments of the present invention is dissolved in an appropriate solvent for hydrogenation. As a factor to be considered when selecting a solvent, it is preferred that the polymer (i.e., both the aromatic polymer and the hydrogenated polymer) before and after hydrogenation has good solubility and does not have a hydrogenated site. Moreover, a solvent that reacts quickly is more preferred. This is because the hydrogenation rate is increased, the reaction time is shortened, and damage to the polymer such as molecular weight reduction can be reduced. In addition, in the case of devolatilization of the solvent component after assuming hydrogenation, it is preferred that the ignition point of the solvent is high. As long as the devolatilization extrusion process can be performed, the hydrogenated polymer can be efficiently manufactured, so it is preferred.

[0106] The solvent used in the manufacturing method of certain embodiments of the present invention is a mixed solvent comprising at least one first solvent and at least one second solvent. Among them, the first solvent is preferably a solvent with high solubility of the polymer before hydrogenation, and the second solvent is preferably a solvent with high solubility of the polymer after hydrogenation. However, the solubility of the polymer in the solvent is not easy to predict, and mixing these two solvents does not necessarily obtain a solvent that can well dissolve both polymers before and after the hydrogenation reaction.

[0107] In one embodiment of the present invention, the solvent is a mixed solvent comprising at least one first solvent and at least one second solvent, wherein the first solvent is a solvent that dissolves the aromatic vinyl compound-based polymer before hydrogenation, and the second solvent is a solvent that dissolves the hydrogenated polymer.

[0108] In one embodiment of the present invention, the at least one first solvent may be an ester solvent. In one embodiment of the present invention, the at least one first solvent contains one or more selected from methyl acetate, ethyl acetate, butyl acetate and methyl isobutyrate. In one embodiment of the present invention, the first solvent is methyl acetate. In another embodiment of the present invention, the first solvent is ethyl acetate. In another embodiment of the present invention, the first solvent is butyl acetate. In yet another embodiment of the present invention, the first solvent is methyl isobutyrate. In a preferred embodiment of the present invention, the first solvent is methyl isobutyrate.

[0109] In one embodiment of the present invention, the boiling point of the first solvent is above 50° C. and the flash point is above 400° C. By using a solvent having a high boiling point and a flash point, the devolatilization extrusion process can be performed efficiently. Examples of such solvents include methyl isobutyrate, ethyl acetate, and butyl acetate, but are not limited thereto.

[0110] In one embodiment of the present invention, the at least one second solvent may be a hydrocarbon solvent. In one embodiment of the present invention, the at least one second solvent comprises one or more selected from cyclohexane, C9-C10 alkylcyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane.

[0111] In one embodiment of the present invention, the second solvent has a boiling point of 80°C or more and a flash point of 230°C or more. By using a solvent having a high boiling point and a flash point, the devolatilization extrusion process can be performed with high efficiency. Examples of such solvents include cyclohexane, cyclopentane, methylcyclohexane, n-heptane, 2,2,4-trimethylpentane, cyclooctane, 1,3-dimethylcyclohexane, ethylcyclohexane, 1,2,4-trimethylcyclohexane, decalin (cis, trans-decalin) and SWACLEAN150.

[0112] In one embodiment of the present invention, the mass ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) is 1:9 to 9:1. In certain embodiments of the present invention, the mass ratio of the at least one first solvent to the at least one second solvent (first solvent: second solvent) can be, for example:

[0113] 1:9-9:1, 1:9-8:2, 1:9-7:3, 1:9-6:4, 1:9-5:5, 1:9-4:6, 1:9-3:7, 1:9-2:8;

[0114] 2:8-9:1, 2:8-8:2, 2:8-7:3, 2:8-6:4, 2:8-5:5, 2:8-4:6, 2:8-3:7;

[0115] 3:7-9:1, 3:7-8:2, 3:7-7:3, 3:7-6:4, 3:7-5:5, 3:7-4:6;

[0116] 4:6-9:1, 4:6-8:2, 4:6-7:3, 4:6-6:4, 4:6-5:5;

[0117] 5:5-9:1, 5:5-8:2, 5:5-7:3, 5:5-6:4;

[0118] 6:4-9:1, 6:4-8:2, 6:4-7:3;

[0119] 7:3-9:1, 7:3-8:2;

[0120] 8:2 to 9:1. When the aromatic vinyl compound polymer is polystyrene, the first solvent: second solvent is preferably 1:9 to 5:5. When the aromatic vinyl compound polymer is a copolymer of styrene and methyl methacrylate, the first solvent: second solvent is preferably 3:7 to 7:3. When the aromatic vinyl compound polymer is a copolymer of styrene and maleic anhydride, the first solvent: second solvent is preferably 3:7 to 9:1. When the aromatic vinyl compound polymer is a copolymer of styrene and butadiene or isoprene, the first solvent: second solvent is preferably 1:9 to 7:3.

[0121] (Hydrogenation Catalyst)

[0122] As the active ingredient of the hydrogenation catalyst used in some embodiments of the present invention, metal elements with contact hydrogenation performance (hereinafter referred to as "specific metal components") can be cited. As specific metal components, for example, nickel, cobalt, iron, ruthenium, rhodium, palladium, platinum, iridium, copper, silver, molybdenum, tungsten, chromium and rhenium can be cited, but are not limited to these. As long as the specific metal component exhibits hydrogenation performance, it can be either a metallic state or a cationic state. Among these, the hydrogenation performance of the metallic state is usually strong and stable under a reducing environment, so the metallic state is preferred. The specific metal component can be used in a state in which a single one or a combination of two or more is contained in a solid catalyst. In the case of using two or more specific metal components, their combination, mixing ratio and form are not particularly limited, and can be used in the form of a mixture of each metal, or an alloy or an intermetallic compound. In certain embodiments of the present invention, the hydrogenation catalyst is preferably a solid catalyst supported by one or more selected from palladium, platinum, ruthenium, rhodium and nickel, and is particularly preferably a solid catalyst supported by palladium.

[0123] The raw materials of these specific metal components are not particularly limited, and materials used as raw materials when preparing catalysts according to methods known in the prior art can be used. Examples of such raw materials include hydroxides, oxides, fluorides, chlorides, bromides, iodides, sulfates, nitrates, acetates, ammine compounds and carbonyl complexes of various metal elements. These can be used alone or in combination of two or more.

[0124] The hydrogenation catalyst used in certain embodiments of the present invention may also use a specific metal component alone or in combination with a metal that does not have contact hydrogenation performance as a metal component. Examples thereof include: catalysts such as palladium black and platinum black composed of fine metal powders of the specific metal component; and sponge catalysts made by forming an alloy with the specific metal component, aluminum and a small amount of additives, and then leaching all or part of the aluminum.

[0125] In addition, in order to further improve the activity, selectivity and physical properties of the catalyst, compounds of one or more elements selected from lithium, sodium, potassium, rubidium and cesium as alkali metal elements, magnesium, calcium, strontium and barium as alkaline earth metal elements, fluorine, chlorine, bromine and iodine as halogen elements, and mercury, lead, bismuth, tin, tellurium and antimony as auxiliary additive elements (hereinafter referred to as specific additive components) may be added to the catalyst together with the above-mentioned specific metal components.

[0126] The raw materials of these specific additives are not particularly limited, and materials used as raw materials when preparing catalysts by existing known methods can be used. As such raw materials, for example, hydroxides, oxides, fluorides, chlorides, bromides, iodides, sulfates, nitrates, acetates and ammonia compounds of various metal elements can be cited. They can be used alone or in combination of two or more. In addition, there are no particular restrictions on the method of adding the specific additives and the ratio of the specific additives to the specific metal components.

[0127] In the hydrogenation catalyst used in some embodiments of the present invention, non-metallic substances can also be used in combination with specific metal components. As non-metallic substances, mainly include elemental simple substance, carbide, nitride, oxide, hydroxide, sulfate, carbonate and phosphate (hereinafter referred to as "specific non-metallic components"). As its specific example, for example, graphite, diamond, activated carbon, silicon carbide, silicon nitride, aluminum nitride, boron nitride, boron oxide, aluminum oxide (alumina), silicon dioxide (silica), titanium oxide, zirconium oxide, hafnium oxide, lanthanum oxide, cerium oxide, yttrium oxide, niobium oxide, magnesium silicate, calcium silicate, magnesium aluminate, calcium aluminate, zinc oxide, chromium oxide, aluminum silicate, aluminum silicophosphate, aluminum phosphate, boron phosphate, magnesium phosphate, calcium phosphate, strontium phosphate, hydroxyapatite (hydroxy calcium phosphate), apatite chloride, apatite fluoride, calcium sulfate, barium sulfate and barium carbonate can be mentioned. Specific non-metallic components can be used alone or in combination of two or more. When two or more compounds are used in combination, there are no particular restrictions on the combination, mixing ratio, or form, and the compounds may be used in the form of a mixture, a complex, or a complex salt.

[0128] From the perspective of industrial use, it is preferred that the specific non-metallic component can be obtained simply and cheaply. As such a specific non-metallic component, preferably a zirconium compound, an aluminum compound and an apatite compound, more preferably a zirconium compound and an apatite compound. Among them, zirconium oxide and hydroxyapatite (calcium hydroxyphosphate) are particularly preferred. In addition, the above-mentioned specific additives can also be used to modify or ion-exchange some or all of these specific non-metallic components.

[0129] In addition, as the specific non-metallic component, carbides, nitrides, oxides, etc. of specific metal components can also be used. However, once these compounds are exposed to a hydrogen reduction environment, they are partially reduced to metals. Therefore, in this case, part of them is used as the specific metal component and the rest is used as the non-metallic component. As such examples, oxides such as nickel oxide, iron oxide, cobalt oxide, molybdenum oxide, tungsten oxide, and chromium oxide can be cited.

[0130] As the hydrogenation catalyst used in certain embodiments of the present invention, a specific metal component can be used alone, or a specific metal component can be used in combination with a specific non-metal component. Depending on the circumstances, a specific additional component other than this may also be included. The method for manufacturing the hydrogenation catalyst used in certain embodiments of the present invention is not particularly limited, and existing known methods can be used. As examples thereof, there can be cited: a method in which a raw material compound of a specific metal component is impregnated on a specific non-metal component (supporting method); a method in which a raw material compound of a specific metal component and a raw material compound of a specific non-metal component are dissolved together in an appropriate solvent and then precipitated simultaneously using an alkaline compound or the like (coprecipitation method); a method in which a raw material compound of a specific metal component and a specific non-metal component are uniformly mixed in an appropriate proportion (mixing method), etc.

[0131] According to the composition of the hydrogenation catalyst or the conditions of the catalyst preparation method, it is also possible to perform a reduction treatment after preparing a specific metal component in a cationic state to form a metallic state. As the reduction method and reducing agent used for this purpose, existing known methods and substances can be used without special limitation. As reducing agents, for example, reducing inorganic gases such as hydrogen, carbon monoxide gas, ammonia, hydrazine, phosphine and silane, low-level oxygen-containing compounds such as methanol, formaldehyde and formic acid, hydrides such as sodium borohydride and lithium aluminum hydride can be cited. By performing a reduction treatment on a specific metal component in a cationic state in the gas phase or liquid phase in the presence of these reducing agents, the specific metal component is converted into a metallic state. The reduction treatment conditions at this time can be set to appropriate conditions according to the type and amount of the specific metal component and the reducing agent. The reduction treatment operation can be performed by using a catalytic reduction device separately before the hydrogenation reduction in the manufacturing method of certain embodiments of the present invention, or it can be performed in the reactor used in the manufacturing method of certain embodiments of the present invention before the start of the reaction or simultaneously with the reaction operation.

[0132] In addition, the metal content and shape of the hydrogenation catalyst used in certain embodiments of the present invention are not particularly limited. The shape can be powdery or a molded product, and the shape and molding method during molding are not particularly limited. For example, spherical products, tablet molded products, and extruded molded products can be appropriately selected and used, and they can be crushed into shapes of appropriate sizes.

[0133] A particularly preferred specific metal component is palladium, and a catalyst using the specific metal component is described in detail below. When the specific metal component is palladium, considering that palladium is a precious metal, from the perspective of economic efficiency, it is preferred that the amount used is small and the palladium can be effectively utilized. Therefore, it is preferred that the palladium is dispersed and supported on a catalyst carrier for use.

[0134] The palladium compound as a raw material of palladium is preferably a palladium compound that can be dissolved in water or an organic solvent. As such a palladium compound, for example, palladium chloride, tetrachloropalladium salt, tetraammine palladium salt, palladium nitrate and palladium acetate can be cited. Among them, palladium chloride is preferred because of its high solubility in water or an organic solvent and its ease of use for industrial purposes. Palladium chloride can be dissolved in a sodium chloride aqueous solution, dilute hydrochloric acid, ammonia water, etc. for use.

[0135] By adding a solution of a palladium compound to a catalyst support or impregnating the catalyst support into a solution of a palladium compound, palladium or a palladium compound is fixed on the catalyst support. The fixing method generally includes adsorption on the support, crystallization by distillation to remove the solvent, precipitation and deposition of reducing substances and / or alkaline substances acting on the palladium compound, and a suitable method can be used as appropriate. The palladium content in the hydrogenation catalyst obtained by this type of method is preferably 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, and further preferably 0.5 to 5% by mass relative to the total amount of the hydrogenation catalyst in terms of metal palladium conversion. Due to the palladium content of more than 0.01% by mass, a more sufficient hydrogenation rate can be obtained, and the conversion rate of the aromatic vinyl compound-based polymer is further improved. On the other hand, when the palladium content is less than 20% by mass, the dispersion efficiency of palladium in the hydrogenation catalyst becomes higher, so palladium can be used more effectively.

[0136] Depending on the conditions of the palladium compound and the catalyst preparation method, palladium is sometimes supported on the carrier in a cationic state rather than in a metallic state. In this case, the supported cationic palladium (for example, in the state of a palladium compound) can also be reduced to metallic palladium for use. The reduction method and reducing agent used for this purpose can use existing known methods and substances without special restrictions. As a reducing agent, for example: reducing inorganic gases such as hydrogen, carbon monoxide gas, ammonia and hydrazine, low-level oxygen-containing compounds such as methanol, formaldehyde and formic acid, hydrocarbon compounds such as ethylene, propylene, benzene and toluene, hydrides such as sodium borohydride and lithium aluminum hydride. By contacting the cationic palladium with the reducing agent in the gas phase or in the liquid phase, it can be easily reduced to metallic palladium. The reduction treatment conditions at this time can be set to appropriate conditions according to the type and amount of the reducing agent. The reduction treatment operation can be performed using a catalytic reduction device separately before the hydrogenation reduction in the manufacturing method of this embodiment, or it can be performed in the reactor used in the manufacturing method of this embodiment before the start of the reaction or simultaneously with the reaction operation.

[0137] As a specific non-metal component used together with a specific metal component, a zirconium compound is one of the preferred components, and a hydrogenation catalyst containing the compound is described in detail below. The zirconium compound used in certain embodiments of the present invention is preferably selected from zirconium oxide, zirconium hydroxide, zirconium carbonate, alkaline earth zirconate, rare earth zirconate and zircon, either alone or in combination of two or more thereof.

[0138] A particularly preferred zirconium compound is zirconium oxide, and its preparation method is not particularly limited. For example, a method in which an aqueous solution of a soluble zirconium salt is decomposed with an alkaline substance to form zirconium hydroxide or zirconium carbonate, and then prepared by thermal decomposition, etc., is a generally known method. The raw material of the zirconium compound at this time is not limited, and examples thereof include zirconium oxychloride, zirconium oxynitrate, zirconium chloride, zirconium sulfate, tetraalkoxy zirconium, zirconium acetate, and zirconium acetylacetonate. They can be used alone or in combination of two or more. In addition, as alkaline substances for decomposition, examples thereof include ammonia, alkylamines, ammonium carbonate, ammonium bicarbonate, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, potassium carbonate, potassium bicarbonate, magnesium hydroxide, calcium hydroxide, lanthanum hydroxide, yttrium hydroxide, and cerium hydroxide, and they can be used alone or in combination of two or more.

[0139] When zirconium oxide is used as the specific non-metal component, there are no particular restrictions on its physical properties, shape, etc. In addition, there are no particular restrictions on the purity of zirconium oxide, and zirconium oxide of purity grades ranging from commercially available general-purpose products to high-purity products can be appropriately used.

[0140] When a specific non-metal component represented by a zirconium compound is used as a catalyst carrier, there are no particular restrictions on the shape, particle size, porosity and other physical properties of these carriers, as well as the method of supporting the metal component. The shape, carrier physical properties, supporting method, etc. corresponding to the reaction mode and conditions can be appropriately selected and used.

[0141] The hydrogenation catalyst is preferably a hydrogenation catalyst that has been subjected to a reduction treatment before being used in the hydrogenation reaction. By performing a reduction treatment before being used in the hydrogenation reaction, the efficiency of the hydrogenation reaction can be improved. In one embodiment of the present invention, the hydrogenation catalyst is a hydrogenation catalyst that has been subjected to a reduction treatment.

[0142] (Other reaction conditions)

[0143] The concentration of the copolymer (aromatic polymer + hydrogenated polymer on the ring) in the solution during the ring hydrogenation reaction is usually 1 to 50% by weight, preferably 3 to 30% by weight, and more preferably 5 to 25% by weight. By setting the upper limit of the concentration of the copolymer to a value below the specified value, it is possible to avoid handling inconveniences caused by a decrease in reaction rate or an increase in solution viscosity. In addition, from the perspective of productivity and / or economic benefits, it is preferred that the lower limit of the concentration be set to a value above the specified value.

[0144] The hydrogenation (hydrogenation) reaction in the manufacturing method of certain embodiments of the present invention is carried out using a raw material liquid in which an aromatic vinyl compound polymer is dissolved in a solvent, but any one of a suspended bed or a fixed bed can be used for reaction, and known methods such as intermittent reaction or continuous flow reaction can also be used. In the case of using a suspended bed for reaction, the carrier particle size is usually in the range of 0.1 to 1000 μm, preferably 1 to 500 μm, more preferably 5 to 200 μm. By setting the particle size to a specified size or more, the catalyst separation after the hydrogenation reaction is easily achieved, and by setting the upper limit of the particle size to below the specified value, the reaction rate can be prevented from decreasing.

[0145] Preferred reaction conditions are a temperature of 60 to 250°C, a hydrogen pressure of 3 to 30 MPa, and a reaction time of 3 to 30 hours. By setting the reaction temperature to a predetermined temperature or higher, the reaction rate is accelerated; by setting the upper limit of the reaction temperature to a predetermined temperature or lower, side reactions such as polymer decomposition and solvent hydrogenation cracking can be suppressed. In addition, although the reaction rate can be accelerated by setting the hydrogen pressure to a predetermined value or higher, from the perspective of economic benefits, the upper limit is preferably about 30 MPa.

[0146] By separating the hydrogenation catalyst and volatile components (solvent, etc.) from the polymer solution after the hydrogenation reaction, a ring-hydrogenated polymer can be obtained. The catalyst can be separated by known techniques such as filtration or centrifugal separation. Considering coloration, the effect on mechanical properties, etc., the residual catalyst metal concentration in the polymer is preferably as small as possible, preferably 10 ppm or less, more preferably 1 ppm or less.

[0147] As a method for separating volatile components such as solvent from the obtained ring hydrogenated polymer solution after catalyst separation to purify the polymer, the following methods can be used: 1) a method of continuously removing the solvent from the polymer solution to form a concentrated solution, and extruding it in a molten state while heating to granulate it (also called devolatilization extrusion method); 2) a method of evaporating the solvent from the polymer solution to obtain a block, and then granulating it; 3) a method of adding a polymer solution to a poor solvent or adding a poor solvent to the polymer solution to precipitate it, and then granulating it; 4) a method of contacting with hot water to obtain a block, and then granulating it, etc. The manufacturing method of a preferred embodiment of the present invention includes a step of forming a polymer resin by devolatilization extrusion after the hydrogenation reaction. Devolatilization extrusion can be carried out, for example, by maintaining or heating the polymerization solution obtained in the polymerization tank to 120°C to 180°C, and introducing it into a devolatilization extruder equipped with a vent in this state to remove volatile components. The manufacturing method of another preferred embodiment of the present invention also includes a concentration step between the hydrogenation reaction and the devolatilization extrusion.

[0148] When performing catalyst separation and volatile component separation, it is preferred to operate under an inert gas or non-oxidizing gas environment. As the inert gas and non-oxidizing gas, hydrogen or nitrogen, helium, argon can be used, and it is preferred to operate under an environment of industrially cheap nitrogen or hydrogen as a reaction gas.

[0149] The final hydrogenation rate (referring to "final ring hydrogenation rate", "final ring hydrogenation rate") of the hydrogenated polymer obtained by the method of certain embodiments of the present invention is not particularly limited, and is preferably 90% or more, 91% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, 99% or more, or 99.9% or more. In a preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 93% or more. In a more preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 95% or more. In a further preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 96% or more. In a further preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 97% or more. In a further preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 98% or more. In a further preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 99% or more. In the most preferred embodiment, the final hydrogenation rate of the hydrogenated polymer is 99.9% or more. As described in the examples, the hydrogenation rate can be obtained by UV spectrometry before and after the hydrogenation reaction.

[0150] As described above, in a preferred embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer (referring to "initial ring hydrogenation rate" or "initial ring hydrogenation rate") is not particularly limited, and may be 50% or more, 55% or more, 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, 85% or more, 90% or more, 92% or more, 93% or more, 94% or more, 95% or more, 96% or more, 97% or more, 98% or more, 99% or more, or 99.9% or more. In an embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer refers to, for example, the hydrogenation rate at 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 15 hours, and 20 hours after the start of the hydrogenation reaction, but is not limited thereto. In one embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer is the hydrogenation rate at a time point of 3 hours after the start of the hydrogenation reaction. In one embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer is the hydrogenation rate at a time point of 5 hours after the start of the hydrogenation reaction. In one embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer is the hydrogenation rate at a time point of 20 hours after the start of the hydrogenation reaction. By pre-reducing the hydrogenation catalyst to form a reduced hydrogenated catalyst, the reaction rate of the hydrogenation reaction can be increased.

[0151] In a preferred embodiment of the present invention, the initial hydrogenation rate of the hydrogenated polymer is 50% or more. In a more preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 55% or more. In a further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 60% or more. In a further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 65% or more. In a further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 70% or more. In a further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 75% or more. In a further further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 80% or more. In a further further preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 85% or more. In the most preferred embodiment, the initial hydrogenation rate of the hydrogenated polymer is 90% or more. As described in the examples, the hydrogenation rate can be obtained by UV spectroscopy before and after the hydrogenation reaction.

[0152] <Optical material and method for producing the same>

[0153] In one embodiment of the present invention, a method for producing an optical material comprising the above-mentioned method for producing a hydrogenated polymer is provided. In one embodiment of the present invention, the method for producing an optical material comprises a method for producing a hydrogenated polymer by hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer, wherein:

[0154] The aromatic vinyl compound-based polymer comprises a first monomer unit and a second monomer unit.

[0155] The above methods include:

[0156] A step of reducing the hydrogenation catalyst before use; and

[0157] A step of obtaining a hydrogenated polymer by hydrogenating the aromatic vinyl compound-based polymer, a solvent, and a reduction-treated hydrogenation catalyst. The details of the method for producing the hydrogenated polymer are as described above.

[0158] The hydrogenated polymer obtained by the method of certain embodiments of the present invention can be appropriately mixed with additives such as antioxidants, colorants, release agents, surfactants, antibacterial agents, etc. to form an optical material composition. Since the obtained optical material composition has thermoplasticity, it can be used to manufacture precise and cost-effective optical products through various thermal forming processes such as extrusion molding or injection molding, secondary processing molding of sheet molded bodies, etc. As specific uses of optical products, various light guide plates or light guides, display front panels, plastic lens substrates, filters, optical films, lighting covers, lighting signs, etc. can be cited, but are not limited to these. In one embodiment of the present invention, the above-mentioned optical material is an optical lens.

[0159] Example

[0160] The present invention will be described in more detail below by way of examples, but the present invention is not particularly limited by the following examples. The evaluation method of the resin is as follows.

[0161] (1) The ring hydrogenation rate is obtained by UV spectrum measurement before and after the hydrogenation reaction. That is, the resin is dissolved in tetrahydrofuran (THF) as a solvent, and the absorption spectrum at 260 nm is measured using a quartz cuvette. The copolymer resin before the ring hydrogenation reaction is used for calibration to calculate the ratio of unhydrogenated aromatic rings. The instrument used for the measurement is a UV-visible spectrophotometer "GENESYS10S" manufactured by Thermo, but it is not particularly limited to this, as long as it is an equivalent device.

[0162] (2) The weight average molecular weight (Mw) was determined by gel permeation chromatography (GPC). A differential refractive index (RI) detector was used as the detector, THF was used as the solvent, and calibration was performed using standard polystyrene. The instrument used for the measurement was a high-speed liquid chromatography system "Elite LaChrom" manufactured by Shimadzu Scientific Co., Ltd., but it is not particularly limited thereto, and any equivalent equipment may be used.

[0163] (3) The glass transition temperature (Tgm) of the resin was determined by differential scanning calorimetry (DSC). The instrument used for the measurement was DSC7020 manufactured by SII (currently Hitachi High-Technologies Corporation), but the instrument is not particularly limited thereto and any equivalent equipment may be used.

[0164] <Aromatic vinyl compound polymer>

[0165] (Resin 1): A copolymer composed of styrene and maleic anhydride (XIBOND 120 manufactured by POLYSCOPE POLYMERS BV, styrene / maleic anhydride molar ratio = 93 / 7, weight average molecular weight 163,000)

[0166] (Resin 2): A copolymer composed of styrene and maleic anhydride (XIBOND 140 manufactured by POLYSCOPE POLYMERS BV, styrene / maleic anhydride molar ratio = 85 / 15, weight average molecular weight 140,000)

[0167] (Resin 3): Block copolymer composed of styrene and butadiene (Clearen 530L manufactured by Denka Co., Ltd., styrene / butadiene molar ratio = 72.7 / 27.3, weight average molecular weight 133,000)

[0168] (Resin 4): Copolymer composed of styrene and methyl methacrylate (MS200 manufactured by Toyo Styrene Co., Ltd., styrene / methyl methacrylate molar ratio = 8 / 2, weight average molecular weight 258,000)

[0169] <Preparation Example 1 Preparation of Hydrogenation Reaction Raw Material Polymer>

[0170] 0.5 parts by mass of resin 1 having a weight average molecular weight of 163,000 was dissolved in 2.75 parts by mass of methyl isobutyrate (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter referred to as "IBM"), and then the water content was reduced from the polymer solution by distillation operation (0.5 parts by mass was removed by azeotropic distillation). 2.25 parts by mass of cyclohexane (manufactured by Tokyo Chemical Industry Co., Ltd., hereinafter referred to as "CH") was added to the polymer solution after distillation and dehydration to prepare a hydrogenation reaction raw material polymer solution corresponding to 10% by mass.

[0171] <Example 1>

[0172] 0.1 parts by mass of 2.0% Pd / ZrO2 and 1.35 parts by mass of SWACLEAN 150 (manufactured by Maruzen Petrochemical Co., Ltd., a mixture of C9C10 alkylcyclohexanes, hereinafter referred to as "SWC") were added to the reaction vessel. After replacing the reaction vessel with a mixed gas of hydrogen / nitrogen = 5 / 95 (V / V) at room temperature, the catalyst was pre-reduced by stirring at 180°C for one hour. After the pre-reduced reaction vessel was cooled to room temperature, an IBM solution of resin 1 that had been azeotropically dehydrated in the same manner as in Preparation Example 1 was added to prepare a 10% by mass hydrogenation reaction raw material polymer solution (IBM / SWC ratio = 7 / 3). Then, a hydrogenation reaction was carried out for 44 hours under the conditions of a hydrogen pressure of 9.1 MPa and a temperature of 180°C. After the hydrogenation reaction, the catalyst was removed from the polymer solution by filtration, and then the reaction solution was added dropwise to an excess of methanol to precipitate the resin. The obtained resin powder was dried under reduced pressure to obtain a dry resin powder. The obtained hydrogenated resin had a ring hydrogenation rate of 84.4% at 3 hours, 92.3% at 5 hours, 96.9% at 20 hours, and a final ring hydrogenation rate of 98.7% at 44 hours. The weight average molecular weight was 122,000 and Tg was 145°C.

[0173] <Examples 2 to 7>

[0174] The same operation as in Example 1 was carried out except that the conditions were changed to those described in Table 1, and the catalyst was pre-reduced and then hydrogenated to obtain a hydrogenated polymer.

[0175] <Comparative Example 1>

[0176] 5.0 parts by mass of the raw polymer solution and 0.1 parts by mass of 2.0% Pd / ZrO2 were added to a reaction vessel with a stirring device, and a hydrogenation reaction was carried out for 44 hours under the conditions of a hydrogen pressure of 9.1 MPa and a temperature of 200°C. After the hydrogenation reaction, the catalyst was removed from the polymer solution by filtration, and then the reaction solution was dropped into an excess of isopropanol to precipitate the resin. The obtained resin powder was dried under reduced pressure to obtain a dry resin powder. The obtained resin had a ring hydrogenation rate of 79.1% at 3 hours, a ring hydrogenation rate of 85.0% at 5 hours, a ring hydrogenation rate of 97.9% at 20 hours, and a final ring hydrogenation rate of 98.3% at 44 hours. The weight average molecular weight was 116,000 and the Tg was 146°C.

[0177] <Comparative Examples 2 to 7>

[0178] The same procedure as in Comparative Example 1 was carried out except that the conditions were changed to those shown in Table 2, and the hydrogenation reaction was carried out without pre-reduction of the catalyst to obtain a hydrogenated polymer.

[0179] The results obtained in Examples 1 to 7 and Comparative Examples 1 to 7 are shown in Tables 1 and 2, respectively.

[0180] [Table 1]

[0181]

[0182] [Table 2]

[0183]

[0184] Figure 1 The relationship between the hydrogenation reaction time and the ring hydrogenation rate of Resin 1 is shown. It is known that the reaction rate of the hydrogenation reaction can be increased by pre-reducing the hydrogenation catalyst to form a reduced hydrogenation catalyst.

[0185] According to the present invention, it is found that in a method for producing a hydrogenated polymer by hydrogenating the aromatic ring of an aromatic vinyl compound-based polymer (ring hydrogenation), the hydrogenation reaction rate is increased, and the hydrogenated polymer can be produced efficiently. In addition, by shortening the reaction time, it is also possible to obtain an effect that the damage to the polymer such as molecular weight reduction can be reduced. In addition, the hydrogenated polymer obtained by the method of the present invention has sufficient heat resistance and is suitable for optical materials.

Claims

1. A method for producing a hydrogenated polymer, wherein the method comprises hydrogenating an aromatic ring of an aromatic vinyl compound-based polymer to produce a hydrogenated polymer, wherein: The aromatic vinyl compound-based polymer comprises a first monomer unit and a second monomer unit, The method include: A step of reducing the hydrogenation catalyst before use; and a step of obtaining a hydrogenated polymer by conducting a hydrogenation reaction using the aromatic vinyl compound-based polymer, a solvent, and a reduction-treated hydrogenation catalyst, The solvent is a mixed solvent comprising at least one first solvent and at least one second solvent, The first solvent is a solvent that dissolves the aromatic vinyl compound polymer before hydrogenation. The second solvent is a solvent that dissolves the hydrogenated polymer.

2. The method for producing a hydrogenated polymer according to claim 1, It is characterized in that The at least one first solvent comprises one or more selected from methyl acetate, ethyl acetate, butyl acetate and methyl isobutyrate.

3. The method for producing a hydrogenated polymer according to claim 1 or 2, It is characterized in that The at least one second solvent comprises one or more selected from cyclohexane, C9-C10 alkylcyclohexane, C7-C15 monoalkylcyclohexane, C8-C15 dialkylcyclohexane, C9-C15 trialkylcyclohexane, C10-C15 tetraalkylcyclohexane, cyclooctane, C9-C15 monoalkylcyclooctane, C10-C15 dialkylcyclooctane, C11-C15 trialkylcyclooctane, C12-C15 tetraalkylcyclooctane, n-octane and n-decane.

4. The method for producing a hydrogenated polymer according to any one of claims 1 to 3, It is characterized in that The first solvent has a boiling point of 50° C. or higher and a flash point of 400° C. or higher.

5. The method for producing a hydrogenated polymer according to any one of claims 1 to 4, It is characterized in that The second solvent has a boiling point of 80° C. or higher and a flash point of 230° C. or higher.

6. The method for producing a hydrogenated polymer according to any one of claims 1 to 5, It is characterized in that The first monomer is selected from styrene, α-methylstyrene, chlorostyrene, 4-methylstyrene, 4-tert-butylstyrene and 4-methoxystyrene.

7. The method for producing a hydrogenated polymer according to any one of claims 1 to 6, It is characterized in that The second monomer is selected from the group consisting of maleic anhydride, butadiene, cyclopentadiene and isoprene.

8. The method for producing a hydrogenated polymer according to any one of claims 1 to 7, It is characterized in that The aromatic vinyl compound-based polymer is selected from the group consisting of a copolymer of styrene and maleic anhydride, a copolymer of styrene and butadiene, and a copolymer of styrene and isoprene.

9. The method for producing a hydrogenated polymer according to claim 8, It is characterized in that The aromatic vinyl compound-based polymer is a copolymer of styrene and maleic anhydride.

10. The method for producing a hydrogenated polymer according to any one of claims 1 to 9, It is characterized in that In the aromatic vinyl compound-based polymer, a polymerization ratio (mol %) of the first monomer unit to the second monomer unit is 70:30 or more and less than 100:

0.

11. The method for producing a hydrogenated polymer according to any one of claims 1 to 10, It is characterized in that The process comprises the steps of forming a polymer resin by devolatilization extrusion after hydrogenation.

12. The method for producing a hydrogenated polymer according to any one of claims 1 to 11, It is characterized in that A concentration step is also included between the hydrogenation reaction and the devolatilization extrusion.

13. The method for producing a hydrogenated polymer according to any one of claims 1 to 12, It is characterized in that The mass ratio of the at least one first solvent to the at least one second solvent (first solvent:second solvent) is 1:9 to 9:

1.

14. The method for producing a hydrogenated polymer according to any one of claims 1 to 13, It is characterized in that The hydrogenation catalyst is a solid catalyst carrying palladium, platinum, ruthenium, rhodium or nickel.

15. A method for manufacturing an optical material, It is characterized in that A method for producing a hydrogenated polymer according to any one of claims 1 to 14.

16. The method for producing an optical material according to claim 15, It is characterized in that The optical material is an optical lens.

Citation Information

Patent Citations

  • Hydrogenation method for aromatic polymers

    JP2001527095A

  • Hydrogenation method of aromatic polymers in the presence of branched hydrocarbons

    JP2002511501A