Method for producing liquid crystal polymer film, liquid crystal polymer film, method for producing high-frequency circuit board material, and method for producing high-frequency circuit board

By forming a thermoplastic liquid crystal polymer layer on the surface of the liquid crystal polymer film, the problem of easy cracking of the liquid crystal polymer film is solved, and the manufacturing of liquid crystal polymer film with excellent strength and high frequency circuit board material is realized, thereby improving the dielectric properties of the high frequency circuit board.

CN118984852APending Publication Date: 2024-11-19FUJIMORI KOGYO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380029572.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-09
Filing Date
2023-06-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Liquid crystal polymer films are prone to cracking and are difficult to produce and process. Existing technologies make it difficult to manufacture liquid crystal polymer films with excellent strength and high-frequency circuit substrate materials.

Method used

A thermoplastic liquid crystal polymer layer is formed by using liquid thermoplastic liquid crystal polymer. The thermoplastic liquid crystal polymer layer is formed on the surface of the thermoplastic liquid crystal polymer film by methods such as coating and melt extrusion, thereby optimizing the strength and anisotropy of the film.

Benefits of technology

The strength and dielectric properties of the liquid crystal polymer film are improved, making it suitable for high-frequency circuit board materials and enhancing the performance of high-frequency circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984852A_ABST
    Figure CN118984852A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a liquid crystal polymer film having excellent strength, a liquid crystal polymer film manufactured by the method, a method for manufacturing a high-frequency circuit board material, and a method for manufacturing a high-frequency circuit board. More specifically, the present invention provides a method for producing a liquid crystal polymer film provided with a thermoplastic liquid crystal polymer film and a thermoplastic liquid crystal polymer layer, the method comprising: forming a liquid crystal polymer layer on the surface of the plastic liquid crystal polymer film; a step for forming a thermoplastic liquid crystal polymer layer using a liquid thermoplastic liquid crystal polymer; a liquid crystal polymer film produced by this method; a method for producing a high-frequency circuit board material; and a method for producing a high-frequency circuit board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a liquid crystal polymer film, a liquid crystal polymer film manufactured by the method, a method for manufacturing a high-frequency circuit substrate material, and a method for manufacturing a high-frequency circuit substrate. Background Art

[0002] Patent Document 1 describes that, in the production of a resin multilayer substrate, a liquid crystal polymer coating is applied to a region where the thickness of the liquid crystal polymer resin layer is insufficient.

[0003] Patent Document 2 describes applying a paste containing a thermoplastic resin to a part of a resin sheet containing a liquid crystal polymer as a main component for integrating electronic components.

[0004] Patent Document 3 describes that when a dispersion of a powdered thermoplastic resin material is applied to the surface of a thermoplastic resin layer, the main material of the thermoplastic resin material is a liquid crystal polymer, which is the same as the main material of the thermoplastic resin layer.

[0005] Patent Document 4 describes applying a paste containing a powder of a liquid crystal polymer onto a main surface of a resin layer containing a liquid crystal polymer as a main material and having a conductive pattern arranged thereon.

[0006] Patent Document 1: International Publication No. 2014 / 109139

[0007] Patent Document 2: International Publication No. 2015 / 029783

[0008] Patent Document 3: International Publication No. 2017 / 061423

[0009] Patent Document 4: International Publication No. 2017 / 217126 Summary of the invention

[0010] Since liquid crystal polymer (LCP) has anisotropy, the film is easily cracked and difficult to produce, handle, etc.

[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a liquid crystal polymer film having excellent strength, a liquid crystal polymer film produced by the method, a method for producing a high-frequency circuit board material, and a method for producing a high-frequency circuit board.

[0012] To solve the above problems, the present invention provides a method for manufacturing a liquid crystal polymer film, wherein the liquid crystal polymer film comprises a thermoplastic liquid crystal polymer film and a thermoplastic liquid crystal polymer layer, and the manufacturing method comprises the step of forming the thermoplastic liquid crystal polymer layer on the surface of the thermoplastic liquid crystal polymer film using a liquid thermoplastic liquid crystal polymer.

[0013] The step of forming the thermoplastic liquid crystal polymer layer is preferably a step of applying a thermoplastic liquid crystal polymer solution.

[0014] The step of forming the thermoplastic liquid crystal polymer layer is preferably a step of extruding a molten thermoplastic liquid crystal polymer.

[0015] The thermoplastic liquid crystal polymer solution is preferably applied by a method selected from the group consisting of die coating, gravure coating, screen printing, and ink jetting.

[0016] The thermoplastic liquid crystal polymer film is preferably produced by a method selected from the group consisting of melt extrusion, stretching, inflation and solution casting.

[0017] The thermoplastic liquid crystal polymer film is preferably a film of liquid crystal polyester or liquid crystal polyester amide, and the thermoplastic liquid crystal polymer layer is preferably a layer of liquid crystal polyester or liquid crystal polyester amide.

[0018] Furthermore, the present invention provides a liquid crystal polymer film produced by the above-mentioned method for producing a liquid crystal polymer film.

[0019] The elastic modulus in the TD direction of the liquid crystal polymer film obtained by forming the TLCP layer is preferably greater than the elastic modulus in the TD direction of the TLCP film before forming the TLCP layer.

[0020] The anisotropy of the linear expansion coefficient (CTE) of the liquid crystal polymer film obtained by forming the TLCP layer is preferably smaller than the anisotropy of the linear expansion coefficient (CTE) of the TLCP film before forming the TLCP layer.

[0021] The liquid crystal polymer film is preferably used for the production of high-frequency circuit substrate materials.

[0022] Furthermore, the present invention provides a method for manufacturing a high-frequency circuit substrate material, comprising the steps of manufacturing a liquid crystal polymer film by the above-mentioned method for manufacturing a liquid crystal polymer film; and laminating a copper foil on the surface of the above-mentioned thermoplastic liquid crystal polymer film on the opposite side to the above-mentioned thermoplastic liquid crystal polymer layer.

[0023] In addition, the present invention provides a method for manufacturing a high-frequency circuit substrate, comprising the steps of manufacturing a liquid crystal polymer film by the above-mentioned method for manufacturing a liquid crystal polymer film; a step of laminating a copper foil on the surface of the above-mentioned thermoplastic liquid crystal polymer film on the opposite side to the above-mentioned thermoplastic liquid crystal polymer layer; and a step of forming a circuit by the above-mentioned copper foil.

[0024] According to the present invention, a method for producing a liquid crystal polymer film having excellent strength can be provided. Furthermore, by using the obtained liquid crystal polymer film, a high-frequency circuit board material and a high-frequency circuit board having excellent dielectric properties can be produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a cross-sectional view showing an example of the liquid crystal polymer film of the present invention. DETAILED DESCRIPTION

[0026] Hereinafter, the present invention will be described based on preferred embodiments.

[0027] Figure 1 An example of the liquid crystal polymer film of the present invention is schematically shown.

[0028] The liquid crystal polymer film 10 includes a thermoplastic liquid crystal polymer layer 12 formed on the surface of a thermoplastic liquid crystal polymer film 11 using a liquid thermoplastic liquid crystal polymer.

[0029] The method for producing the liquid crystal polymer film 10 includes a step of forming a thermoplastic liquid crystal polymer layer 12 on the surface of a thermoplastic liquid crystal polymer film 11 using a liquid thermoplastic liquid crystal polymer.

[0030] The thermoplastic liquid crystal polymer film 11 can be produced by a method selected from the group consisting of melt extrusion, stretching, blow molding, and solution casting. The thermoplastic liquid crystal polymer film 11 preferably has a strength that allows it to maintain its shape even in a single layer. If necessary, the thermoplastic liquid crystal polymer film 11 can be processed by coating or the like while being supported.

[0031] The thermoplastic liquid crystal polymer film 11 is not particularly limited as long as it is a film of a thermoplastic resin having liquid crystallinity, but a film of a liquid crystal polyester or a liquid crystal polyester amide is preferred.

[0032] The TLCP layer 12 may be any layer formed using a liquid TLCP, and may be, although not particularly limited, a coating layer obtained by coating a TLCP solution, an extruded layer obtained by extruding a molten TLCP, or the like.

[0033] The coating layer of the thermoplastic liquid crystal polymer is not particularly limited, and may be formed by coating a thermoplastic liquid crystal polymer solution by a method selected from the group consisting of die coating, gravure coating, screen printing, and inkjet.

[0034] The extruded layer of the thermoplastic liquid crystal polymer is not particularly limited, and may be formed using a T-die, etc. The melting of the thermoplastic liquid crystal polymer is not particularly limited, and an extruder equipped with a screw, etc. may be used.

[0035] The thermoplastic liquid crystal polymer layer 12 is not particularly limited as long as it is a thermoplastic resin layer having liquid crystal properties, and is preferably a liquid crystal polyester or liquid crystal polyester amide layer, and may be a coating layer or an extruded layer of liquid crystal polyester or liquid crystal polyester amide.

[0036] The thermoplastic liquid crystal polymer solution used for forming the coating layer of the thermoplastic liquid crystal polymer is not particularly limited as long as it is a solution of a thermoplastic resin having liquid crystallinity, but a solution of a liquid crystal polyester or a liquid crystal polyester amide layer is preferred.

[0037] The thermoplastic liquid crystal polymer film 11 and the thermoplastic liquid crystal polymer layer 12 may use the same thermoplastic liquid crystal polymer or different thermoplastic liquid crystal polymers, and may both be liquid crystal polyester, liquid crystal polyester amide, or a combination of liquid crystal polyester and liquid crystal polyester amide.

[0038] In the case of liquid crystal polyester, the main chain of the liquid crystal polymer may have repeated ester bonds. In the case of liquid crystal polyester amide, the main chain of the liquid crystal polymer may have repeated ester bonds and amide bonds.

[0039] The TLCP layer 12 may be formed on at least one surface of the TLCP film 11. In order to provide the TLCP film 11 on one surface of the TLCP film 10, it is preferred to form the TLCP layer 12 only on one surface of the TLCP film 11. The TLCP layer 12 may also be formed on both surfaces of the TLCP film 10.

[0040] When forming the TLCP layer 12, the TLCP film 11 may be transported by a roll-to-roll method. The TLCP layer 12 may be formed on the entire surface of the TLCP film 11 or may be formed on a portion of the TLCP film 11 except for both ends in the width direction.

[0041] The liquid thermoplastic liquid crystal polymer used for coating, melt extrusion, etc. preferably does not contain particles, and particularly preferably does not contain particles having a particle size larger than the film thickness of the thermoplastic liquid crystal polymer layer 12 .

[0042] The thermoplastic liquid crystal polymer solution used for coating is preferably a solution in which a solvent-soluble thermoplastic liquid crystal polymer is dissolved in a solvent.

[0043] The solvent used in the thermoplastic liquid crystal polymer solution is not particularly limited as long as it is a solvent that can dissolve the thermoplastic liquid crystal polymer. Examples of the solvent include polar solvents such as ether solvents, ketone solvents, ester solvents, carbonate solvents, amide solvents, nitrile solvents, and sulfur-containing compound solvents. It may also be an aprotic polar solvent.

[0044] Examples of the ether solvent include diethyl ether (DEE), tetrahydrofuran (THF), and dioxane.

[0045] Examples of the ketone solvent include acetone and methyl ethyl ketone (MEK).

[0046] Examples of the ester solvent include non-cyclic ester solvents such as ethyl acetate (EA) and cyclic ester solvents (lactone solvents) such as γ-butyrolactone.

[0047] Examples of the carbonate-based solvent include ethyl carbonate (EC) and propylene carbonate (PC).

[0048] Examples of the amide solvent include dimethylformamide (DMF), dimethylacetamide (DMA), and N-methylpyrrolidone (NMP).

[0049] Examples of the nitrile solvent include acetonitrile (AN), propionitrile, and succinonitrile.

[0050] Examples of the sulfur-containing compound-based solvent include dimethyl sulfoxide (DMSO) and sulfolane.

[0051] When the TLCP solution is applied to form the TLCP layer 12, the conditions for drying the applied solvent are not particularly limited as long as the solvent can be sufficiently dried. As for the temperature for drying the solvent, in order to increase the adhesion between the TLCP film 11 and the TLCP layer 12, it is preferred to heat at a temperature at which a polymerization reaction caused by transesterification occurs between the liquid crystal polymer molecules in the TLCP layer 12, and more preferably between the liquid crystal polymer of the TLCP film 11 and the liquid crystal polymer of the TLCP layer 12. For example, this temperature is preferably 180° C. or higher, more preferably 200° C. or higher, and even more preferably 250° C. or higher. Furthermore, from the viewpoint of suppressing oxidative degradation of the liquid crystal polymer, the temperature for drying the solvent is preferably 350° C. or lower, and more preferably 300° C. or lower. Furthermore, as for the time for drying the solvent, it is not particularly limited, but preferably 30 minutes or more, and more preferably 1 hour or more. From the viewpoint of suppressing oxidative degradation of the liquid crystal polymer, the time for drying the solvent is preferably 5 hours or less, and more preferably 3 hours or less.

[0052] The liquid crystal polymer film 10 having the thermoplastic liquid crystal polymer layer 12 formed using a liquid thermoplastic liquid crystal polymer has a higher strength than the thermoplastic liquid crystal polymer film 11 before the thermoplastic liquid crystal polymer layer 12 is formed. For example, the elastic modulus of the liquid crystal polymer film 10 in the TD direction preferably has a larger value than the elastic modulus of the thermoplastic liquid crystal polymer film 11 in the TD direction.

[0053] The liquid crystal polymer film 10 having the thermoplastic liquid crystal polymer layer 12 formed using a liquid thermoplastic liquid crystal polymer preferably has a more moderate anisotropy than the thermoplastic liquid crystal polymer film 11 before forming the thermoplastic liquid crystal polymer layer 12. For example, the anisotropy of the linear expansion coefficient (CTE) of the liquid crystal polymer film 10 preferably has a smaller value than the anisotropy of the linear expansion coefficient (CTE) of the thermoplastic liquid crystal polymer film 11.

[0054] The anisotropy of physical properties such as the coefficient of linear expansion (CTE) can be expressed by the absolute value of the difference between the physical properties in two directions perpendicular to each other on the film surface (for example, the difference between the value in the MD direction and the value in the TD direction). When the values ​​of the physical properties in the two directions are equal to each other, the anisotropy is zero. In the case where the values ​​of the physical properties in the two directions are different, the anisotropy will be positive.

[0055] The TD direction and MD direction of the TLCP film 11 formed by melt extrusion or the like and the TD direction and MD direction of the TLCP layer 12 formed of liquid TLCP may be the same as or different from each other.

[0056] When the TLCP layer 12 is formed by coating, the method for treating the TLCP film 11 is not particularly limited and can be appropriately set. For example, a TLCP solution may be coated on one side of the TLCP film 11 two or more times to laminate two or more TLCP layers 12. Alternatively, the TLCP layer 12 may be formed by coating the TLCP solution on both sides of the TLCP film 11 simultaneously or successively.

[0057] When the thermoplastic liquid crystal polymer layer 12 is formed by melt extrusion, the method for processing the thermoplastic liquid crystal polymer film 11 is not particularly limited and can be appropriately set. For example, a melted thermoplastic liquid crystal polymer may be extruded twice or more on one side of the thermoplastic liquid crystal polymer film 11 to laminate two or more layers of the thermoplastic liquid crystal polymer layer 12. Furthermore, the thermoplastic liquid crystal polymer layer 12 may be formed by extruding melted thermoplastic liquid crystal polymers on both sides of the thermoplastic liquid crystal polymer film 11 simultaneously or successively.

[0058] When the thermoplastic liquid crystal polymer layer 12 is formed on both sides of the thermoplastic liquid crystal polymer film 11, the methods for forming the respective thermoplastic liquid crystal polymer layers 12 may be the same or different. For the same thermoplastic liquid crystal polymer film 11, the thermoplastic liquid crystal polymer layer 12 may be formed on one side by coating, and the thermoplastic liquid crystal polymer layer 12 may be formed on the other side by melt extrusion.

[0059] The use of the liquid crystal polymer film 10 is not particularly limited, and it can be used, for example, as a substrate for a circuit corresponding to a high frequency, an insulating material, etc. The laminated structure of the high frequency circuit substrate material is not particularly limited, and a conductive layer such as copper foil may be provided on at least one side of an insulating material such as a resin film.

[0060] The LCP film 10 may include the TLCP layer 12 on only one side of the TLCP film 11, and a conductor layer such as copper foil 13 may be laminated on the TLCP film 11. In this case, the conductor layer such as copper foil 13 may be used to form a circuit or the like.

[0061] The method of forming a high-frequency circuit by the conductor layer such as the copper foil 13 is not particularly limited, and for example, etching, lithography, etc. can be cited. The circuit pattern of the conductor layer is not particularly limited, and wiring patterns, antenna patterns, etc. can be cited. Holes can be formed in the liquid crystal polymer film 10 by laser or the like, and a conductor portion penetrating the substrate can be formed in the hole using a conductive paste, a plating process, etc.

[0062] The TLCP film 11 preferably has better dielectric properties than the TLCP layer 12, for example, the dielectric constant and dielectric loss tangent are preferably lower than those of the TLCP layer 12. By providing a conductor layer such as the copper foil 13 on the TLCP film 11 side, a circuit with better high-frequency characteristics can be formed. The copper foil 13 can be laminated on the surface of the TLCP film 11 opposite to the surface on which the TLCP layer 12 is formed.

[0063] The film thickness of the TLCP film 11 and the TLCP layer 12 is not particularly limited, and the one having better dielectric properties is preferably thicker. Furthermore, when the TLCP film 11 has better dielectric properties, the film thickness of the TLCP layer 12 is preferably the minimum film thickness that can alleviate the anisotropy of the TLCP film 11.

[0064] Specifically, when the thickness of the thermoplastic liquid crystal polymer film 11 is 10 μm or more and less than 30 μm, the thickness of the thermoplastic liquid crystal polymer layer 12 is preferably 0.5 μm or more and 8 μm or less; when the thickness of the thermoplastic liquid crystal polymer film 11 is 30 μm or more and less than 60 μm, the thickness of the thermoplastic liquid crystal polymer layer 12 is preferably 0.5 μm or more and 20 μm or less, and more preferably 0.5 μm or more and 15 μm or less; When the thickness of the thermoplastic liquid crystal polymer film 11 is greater than 60 μm and less than 90 μm, the thickness of the thermoplastic liquid crystal polymer layer 12 is preferably greater than 0.5 μm and less than 30 μm, and more preferably greater than 0.5 μm and less than 20 μm; when the thickness of the thermoplastic liquid crystal polymer film 11 is greater than 90 μm, the thickness of the thermoplastic liquid crystal polymer layer 12 is preferably greater than 0.5 μm and less than 50 μm, and more preferably greater than 0.5 μm and less than 30 μm.

[0065] The thermoplastic liquid crystal polymer film 11 preferably has dielectric properties that allow it to be used at high frequencies used in current or next-generation high-speed, high-capacity communications. As high-frequency frequencies, frequencies higher than 2 GHz are preferred, and specific examples include 3.7 GHz bands, 4.5 GHz bands, 28 GHz bands, 90-300 GHz bands, or high-frequency bands above them. These frequency bands may have, for example, a width of about ±0.5 GHz or about ±1 GHz.

[0066] As the dielectric property at high frequency of the thermoplastic liquid crystal polymer film 11, for example, it is preferable that the dielectric loss tangent at a measurement frequency of 10 GHz is 0.002 or less. Among resins with excellent dielectric properties, liquid crystal polymer has a lower water absorption rate than polyimide and the like, and has better adhesion to copper foil than fluororesin, and is therefore suitable as a high-frequency circuit substrate material.

[0067] As described above, the LCP film 10 can be a resin film having both dielectric properties and tear resistance by forming the TLCP layer 12 using a liquid TLCP on at least one surface of the TLCP film 11 .

[0068] In the above, the present invention is described based on preferred embodiments, but the present invention is not limited to the above embodiments, and various changes can be made without changing the gist of the present invention. As changes, the addition, replacement, omission, and other changes of the constituent elements in the embodiments can be listed.

[0069] Example

[0070] Hereinafter, the present invention will be specifically described according to examples.

[0071] (Liquid Crystal Polymer Film of Comparative Example)

[0072] The liquid crystal polymer film of the comparative example is a thermoplastic liquid crystal polyester film manufactured by melt extrusion using a T-shaped die. The tear resistance of this thermoplastic liquid crystal polymer film (without forming a thermoplastic liquid crystal polymer layer) is poor, at least to the extent that it can be easily torn by hand in the TD direction. Therefore, the strength of the liquid crystal polymer film of the comparative example is low, at least to the extent that the elastic modulus in the TD direction cannot be measured, and it is insufficient for use as a substrate material.

[0073] (Liquid Crystal Polymer Film of Example 1)

[0074] A solvent-soluble polymer solution of a thermoplastic liquid crystal polyester (solvent: N-methylpyrrolidone) is applied to one side of a thermoplastic liquid crystal polyester film produced by a melt extrusion method, dried at 100°C for 10 minutes, and then baked at 230°C for 60 minutes to prepare a liquid crystal polymer film. The film thickness of the thermoplastic liquid crystal polymer layer formed by coating the above polymer solution is about 10 μm, and the film thickness of the liquid crystal polymer film is 56 to 58 μm. The film of the thermoplastic liquid crystal polyester has such high adhesion to the thermoplastic liquid crystal polymer layer that it cannot be peeled off. It is believed that the reason why such high adhesion can be achieved is that during the baking process, the molecules in the thermoplastic liquid crystal polymer film and the molecules in the thermoplastic liquid crystal polymer layer undergo an ester exchange reaction to form a chemical bond.

[0075] (Determination of linear expansion coefficient)

[0076] A sample with a width of 4 mm and a length of 15 mm was cut out from the obtained liquid crystal polymer film as a measurement sample, and the measurement was performed using a thermomechanical analyzer (manufactured by Hitachi High-Tech Science Co., Ltd., product name "TMA7100"). The tensile load applied to the measurement sample is set according to the film thickness of the sample (the load is set to 100 mN when the film thickness is 40 to 60 μm, and the load is set to 150 mN when the film thickness is 75 to 95 μm). The linear expansion coefficient is measured by the dimensional change corresponding to the temperature change of the measurement sample. The measurement sample is heated from 30°C to 250°C at a heating rate of 15°C / min, and after being maintained at 250°C for 10 minutes, it is cooled to 30°C at a cooling rate of 15°C / min, and maintained at 30°C for 5 minutes, and then heated again to 300°C at a heating rate of 10°C / min.

[0077] The coefficient of linear expansion (CTE) of the liquid crystal polymer film of the comparative example was -14 ppm / K in the MD direction and 101 ppm / K in the TD direction, and the anisotropy of CTE was 115 ppm / K.

[0078] The coefficient of linear expansion (CTE) of the liquid crystal polymer film of Example 1 was -9 ppm / K in the MD direction and 72 ppm / K in the TD direction, and the anisotropy of CTE was 81 ppm / K.

[0079] This shows that the CTE anisotropy value of the liquid crystal polymer film obtained by applying the thermoplastic liquid crystal polymer solution is small, and the anisotropy can be relaxed.

[0080] (Determination of elastic modulus)

[0081] A sample with a width of 4 mm and a length of 20 mm was cut out from the obtained liquid crystal polymer film as a measurement sample, and the measurement was performed using a dynamic viscoelasticity measuring device (manufactured by TA Instruments Japan Co., Ltd., product name "ARES-G2"). The measurement temperature was 10 to 300°C (heating rate 5°C / min), and a strain of 0.3% was applied at a frequency of 1 Hz. The elastic modulus was measured from the waveform of the shear stress as a response and their phase difference.

[0082] The elastic modulus of the liquid crystal polymer film obtained by applying the thermoplastic liquid crystal polymer solution was 17 GPa in the MD direction and 1.8 GPa in the TD direction. It can be confirmed that the liquid crystal polymer film of the example has a larger elastic modulus than the thermoplastic liquid crystal polymer film before applying the thermoplastic liquid crystal polymer solution at least in the TD direction.

[0083] (Liquid Crystal Polymer Film of Example 2)

[0084] A liquid crystal polymer film was prepared in the same manner as in Example 1 except that a solvent-soluble thermoplastic liquid crystal polymer solution was applied, dried at 100°C for 10 minutes, and then the baking conditions were set to 270°C for 150 minutes, which is more conducive to causing an ester exchange reaction between the molecules in the thermoplastic liquid crystal polymer film and the molecules in the thermoplastic liquid crystal polymer layer. The linear expansion coefficient (CTE) of the obtained liquid crystal polymer film was -1 ppm / K in the MD direction and 17 ppm / K in the TD direction, and the anisotropy of CTE was 18 ppm / K. Furthermore, the elastic modulus of the obtained liquid crystal polymer film was 13 GPa in the MD direction and 8.4 GPa in the TD direction.

[0085] (Liquid Crystal Polymer Film of Example 3)

[0086] The liquid crystal polymer film was prepared in the same manner as in Example 2 except that the film thickness of the thermoplastic liquid crystal polymer layer was about 15 μm and the film thickness of the liquid crystal polymer film was 70 to 72 μm. The linear expansion coefficient (CTE) of the obtained liquid crystal polymer film was -6 ppm / K in the MD direction and 17 ppm / K in the TD direction, and the anisotropy of CTE was 23 ppm / K. Furthermore, the elastic modulus of the obtained liquid crystal polymer film was 18 GPa in the MD direction and 11 GPa in the TD direction.

[0087] (Explanation of Reference Numerals)

[0088] 10: Liquid crystal polymer film

[0089] 11: Thermoplastic Liquid Crystal Polymer Film

[0090] 12: Thermoplastic liquid crystal polymer layer

[0091] 13: Copper foil

Claims

1. A method for producing a liquid crystal polymer film, the liquid crystal polymer film comprising a thermoplastic liquid crystal polymer film and a thermoplastic liquid crystal polymer layer, The manufacturing method includes a step of forming a thermoplastic liquid crystal polymer layer on a surface of a thermoplastic liquid crystal polymer film using a liquid thermoplastic liquid crystal polymer.

2. The manufacturing method according to claim 1, wherein: The step of forming the thermoplastic liquid crystal polymer layer is a step of coating a thermoplastic liquid crystal polymer solution.

3. The manufacturing method according to claim 1, wherein: The step of forming the thermoplastic liquid crystal polymer layer is a step of extruding a molten thermoplastic liquid crystal polymer.

4. The manufacturing method according to claim 2, wherein: The TLCP solution is coated by a method selected from the group consisting of die coating, gravure coating, screen printing, and inkjetting.

5. The manufacturing method according to claim 1, wherein: The thermoplastic liquid crystal polymer film is manufactured by a method selected from the group consisting of a melt extrusion method, a stretching method, a blow molding method, and a solution casting method.

6. The manufacturing method according to claim 1, wherein: The thermoplastic liquid crystal polymer film is a film of liquid crystal polyester or liquid crystal polyester amide, and the thermoplastic liquid crystal polymer layer is a layer of liquid crystal polyester or liquid crystal polyester amide. 7 . A liquid crystal polymer film produced by the production method according to claim 1 .

8. The liquid crystal polymer film according to claim 7, wherein The elastic modulus in the TD direction of the liquid crystal polymer film obtained by forming the thermoplastic liquid crystal polymer layer has a larger value than the elastic modulus in the TD direction of the thermoplastic liquid crystal polymer film before forming the thermoplastic liquid crystal polymer layer.

9. The liquid crystal polymer film according to claim 7, wherein The anisotropy of the linear expansion coefficient (CTE) of the liquid crystal polymer film obtained by forming the TLCP layer has a smaller value than the anisotropy of the linear expansion coefficient (CTE) of the TLCP film before forming the TLCP layer.

10. The liquid crystal polymer film according to claim 7, wherein The liquid crystal polymer film is used for manufacturing high-frequency circuit substrate materials.

11. A method for producing a high-frequency circuit substrate material, comprising: a step of producing a liquid crystal polymer film by the production method according to any one of claims 1 to 6; and a step of laminating a copper foil on a surface of the thermoplastic liquid crystal polymer film opposite to the thermoplastic liquid crystal polymer layer.

12. A method for manufacturing a high-frequency circuit substrate, comprising: a step of manufacturing a liquid crystal polymer film by the manufacturing method described in any one of claims 1 to 6; a step of laminating a copper foil on the surface of the thermoplastic liquid crystal polymer film on the opposite side to the thermoplastic liquid crystal polymer layer; and a step of forming a circuit from the copper foil.

Citation Information

Patent Citations

  • Resin multilayer substrate, and manufacturing method therefor

    WO2014109139A1

  • Method for manufacturing component-integrated sheet, method for manufacturing resin multilayer substrate in which electronic component is incorporated, and resin multilayer substrate

    WO2015029783A1

  • Manufacturing method for treated sheet and manufacturing method for multilayered resin substrate

    WO2017061423A1

  • Method for manufacturing resin multilayer substrate

    WO2017217126A1