Conductive paste, solar cell, and method for manufacturing solar cell

By adjusting the glass frit composition in the conductive paste and using a laser treatment process, the problem of excessive burn-through of the conductive paste on the anti-reflective film is solved, and the light incident surface electrode with low contact resistance and high conversion efficiency is achieved , improves the performance of crystalline silicon solar cells.

CN118985049APending Publication Date: 2024-11-19NAMICS CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202380029259.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-07
Filing Date
2023-03-27
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When the existing crystalline silicon solar cells form the surface electrode on the light incident side, the conductive paste has too strong burn-through properties on the anti-reflection film, resulting in damage to the impurity diffusion layer and reduced performance of the solar cell, and low contact is required in the laser treatment process. It is difficult to realize the conductive paste of resistance.

Method used

Using conductive paste containing silver particles, ethyl cellulose, rosin esters, acrylic resins and organic solvents, the reactivity of the glass frit is controlled by adjusting the alkalinity and content of the glass frit, and combining with the laser treatment process to form low contact. The surface electrode of the resistor light incident side avoids damage to the anti-reflection film.

Benefits of technology

It is achieved to increase the filling factor without reducing the open circuit voltage, suppress damage to the impurity diffusion layer, and improve the conversion efficiency and performance of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052834580000391
    Figure BDA0005052834580000391
  • Figure BDA0005052834580000392
    Figure BDA0005052834580000392
  • Figure BDA0005052834580000401
    Figure BDA0005052834580000401
Patent Text Reader

Abstract

To produce a crystalline silicon solar cell, a conductive paste suitable for forming an electrode by a laser treatment process is provided. A conductive paste for forming an electrode of a solar cell, the conductive paste containing (A) conductive particles, (B) an organic vehicle, and (C) a glass frit, the product BGF * G of the alkalinity BGF of the (C) glass frit and the content G of the (C) glass frit being in the range of 0.25-1.45, the content G of the (C) glass frit is the content of the (C) glass frit in parts by weight in the conductive paste when the content of the (A) conductive particles in the conductive paste is taken as 100 parts by weight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive paste for forming an electrode of a semiconductor device or the like. In particular, the present invention relates to a conductive paste for forming an electrode of a solar cell. In addition, the present invention relates to a solar cell manufactured using the conductive paste for forming an electrode, and a method for manufacturing a solar cell. Background Art

[0002] In the case of semiconductor devices such as crystalline silicon solar cells in which crystalline silicon obtained by processing single crystal silicon or polycrystalline silicon into a flat plate is used as a substrate, in order to make electrical contact with the outside of the device, an electrode is usually formed on the surface of the silicon substrate using a conductive paste for electrode formation. In semiconductor devices in which electrodes are formed in this way, the production of crystalline silicon solar cells has increased significantly in recent years. These solar cells have an impurity diffusion layer, an anti-reflection film, and a light incident side surface electrode on one surface of the crystalline silicon substrate, and a back electrode on the other surface. The light incident side surface electrode and the back electrode enable the power generated by the crystalline silicon solar cell to be taken out to the outside.

[0003] In the conventional formation of electrodes for crystalline silicon solar cells, a conductive paste containing conductive powder, glass frit, organic binder, solvent, and other additives is used. As the conductive powder, silver particles (silver powder) are mainly used.

[0004] Patent document 1 describes a method for improving the ohmic contact behavior between the contact grid (Japanese: コンタクトグリッド) and the emitter layer of a silicon solar cell. Specifically, the method described in patent document 1 describes the following. That is, first, the emitter layer, the contact grid (5) and the back contact (3) are set on the silicon solar cell (1). The contact grid (5) is electrically connected to one electrode of a voltage source. A contact device electrically connected to the other electrode of the voltage source is connected to the back contact (3). A voltage in the opposite direction to the forward direction of the silicon solar cell (1) is applied by the voltage source, and the voltage is lower than the breakdown voltage. During the application of the voltage, a point light source (13) is guided to the side of the silicon solar cell (1) facing the sun. A small segment on the side facing the sun is spot-irradiated, inducing a current flowing in a partial area. The current acts on the small segment during a period of 1 msec to 100 msec. The current is equivalent to 10 to 30 times the short-circuit current of the silicon solar cell (1) measured under standard test conditions, reduced by the ratio of the area of ​​the small segment to the area of ​​the silicon solar cell (1).

[0005] A process for improving the ohmic contact behavior between the contact grid line and the emitter layer in a silicon solar cell unit is described in Patent Document 2. Specifically, as a process in Patent Document 2, it is described that: a prescribed voltage is applied in a direction opposite to the forward direction of the silicon solar cell unit, a point light source is guided to the solar surface side of the silicon solar cell unit, and a cross section of a sub-segment on the solar surface side is irradiated.

[0006] Patent Document 3 describes a method for manufacturing a crystalline silicon solar cell using a conductive paste for forming an electrode of a crystalline silicon solar cell containing an inorganic material. Patent Document 3 describes a conductive paste containing conductive particles and glass frit as an inorganic material. It is described that the glass frit contained in the conductive paste of Patent Document 3 contains 70 to 90% by weight of PbO in 100% by weight of the glass frit and does not contain Al2O3.

[0007] Patent Document 4 describes a conductive composition comprising silver powder, glass powder containing PbO, and a carrier containing an organic substance. Patent Document 4 describes that the conductive composition is a conductive composition for forming an electrode that penetrates a silicon nitride layer and is in electrical communication with an n-type semiconductor layer formed below the silicon nitride layer. In addition, Patent Document 4 describes that the basicity of the glass powder contained in the conductive composition is greater than or equal to 0.6 and less than or equal to 0.8, and that the glass transition temperature is 300°C to 450°C.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent Application No. 2019-525471

[0011] Patent Document 2: Japanese Patent Application No. 2021-513218

[0012] Patent Document 3: Japanese Patent Application Publication No. 2011-86754

[0013] Patent Document 4: Japanese Patent Application Publication No. 2009-231826 Summary of the invention

[0014] exist Figure 5 An example of a cross-sectional schematic diagram of a conventional crystalline silicon solar cell is shown in FIG. Figure 5As shown, in a crystalline silicon solar cell, an impurity diffusion layer 4 (for example, a p-type impurity diffusion layer in which p-type impurities are diffused) is usually formed on the surface (light incident side surface) of a crystalline silicon substrate 1 (for example, an n-type crystalline silicon substrate 1) as the light incident side. An anti-reflection film 2 is formed on the impurity diffusion layer 4. The anti-reflection film 2 also has a function as a passivation film, so the anti-reflection film 2 is sometimes referred to as a passivation film 2. In addition, an electrode pattern of a light incident side surface electrode 20 (surface electrode) is printed on the anti-reflection film 2 using a conductive paste by screen printing or the like, the conductive paste is dried, and fired at a predetermined temperature, thereby forming the light incident side surface electrode 20. In a conventional crystalline silicon solar cell, when fired at the predetermined temperature, the conductive paste burns through the anti-reflection film 2. By this burning through, the light incident side surface electrode 20 can be formed in a manner that contacts the impurity diffusion layer 4. It should be noted that the burn-through means that the anti-reflection film 2 as an insulating film is etched with the glass frit or the like contained in the conductive paste to make the light incident side surface electrode 20 and the impurity diffusion layer 4 conductive. Figure 5 In the example shown, when the electrode pattern is fired, the electrode pattern burns through the anti-reflection film 2, whereby the anti-reflection film 2 disappears, and the surface electrode 20 on the light incident side contacts the impurity diffusion layer 4. A pn ​​junction is formed at the interface between the n-type crystalline silicon substrate 1 and the impurity diffusion layer 4. Most of the incident light incident on the crystalline silicon solar cell passes through the anti-reflection film 2 and the impurity diffusion layer 4 and is incident on the n-type crystalline silicon substrate 1. In this process, light is absorbed in the n-type crystalline silicon substrate 1, generating electron-hole pairs. These electron-hole pairs are separated from the n-type crystalline silicon substrate 1 to the back electrode 15 and the holes are separated from the p-type impurity diffusion layer 4 to the surface electrode 20 on the light incident side due to the electric field generated by the pn junction. Electrons and holes (carriers) are taken out to the outside in the form of electric current via these electrodes.

[0015] exist Figure 2 An example of a schematic diagram of the light incident side surface of a crystalline silicon solar cell is shown in FIG. Figure 2 As shown, on the light incident side surface of the crystalline silicon solar cell, a bus electrode (light incident side bus electrode 20a) and a light incident side finger electrode 20b (sometimes simply referred to as "finger electrode 20b") are arranged as the light incident side surface electrode 20. Figure 5 and Figure 2 In the example shown, among the electron-hole pairs generated by incident light entering the crystalline silicon solar cell, the electrons are collected at the finger electrode 20b and further collected at the light incident side bus electrode 20a. A metal ribbon for interconnection with the periphery covered by solder is welded to the light incident side bus electrode 20a, and current is taken out to the outside through the metal ribbon.

[0016] In order to obtain a crystalline solar cell with high conversion efficiency, it is required that the contact resistance between the light incident side surface electrode 20 and the impurity diffusion layer 4 be low.

[0017] In order to obtain low contact resistance between the light incident side surface electrode 20 and the impurity diffusion layer 4, a method for manufacturing a solar cell using a laser processing process has been proposed. Specific examples of the laser processing process are described in Patent Documents 1 and 2. In this specification, the laser processing process refers to the following technology: after forming the light incident side surface electrode 20, a prescribed voltage is applied in a manner that causes a current to flow in a direction opposite to the forward direction of the crystalline silicon solar cell, and the light incident side surface of the solar cell is irradiated with light from a point light source, thereby obtaining a low contact resistance. Generally, by performing a laser processing process, it is possible to increase the fill factor (Fill Factor: FF) without reducing the open circuit voltage (Open Circuit Voltage: Voc) which is a characteristic of the solar cell. It should be noted that in the laser processing process, when the electrode pattern of the conductive paste is fired at a prescribed temperature, it is preferred that the conductive paste does not burn through the anti-reflection film 2 in most of the anti-reflection film 2 that contacts the electrode pattern. Figure 1 FIG. 1 shows an example of a cross-sectional schematic diagram showing a structure in which a light incident side surface electrode 20 is formed on the light incident side surface of a crystalline silicon solar cell using a laser processing process. Figure 1 As shown, when a laser treatment process is used, an anti-reflection film 2 exists in most of the space between the light incident side surface electrode 20 and the impurity diffusion layer 4. In the laser treatment process, the voltage specified above is applied in such a way that a current flows in the direction opposite to the forward direction in the pn junction, and light from a point light source is irradiated to generate carriers (electrons and holes), thereby causing a current to flow in a tiny area between the light incident side surface electrode 20 and the impurity diffusion layer 4, which is locally heated. By local heating, a tiny portion where the impurity diffusion layer 4 is locally absent is formed between the light incident side surface electrode 20 and the impurity diffusion layer 4. As a result, as shown in FIG. Fig.13 As shown in FIG. 1 , it is considered that the AgSi alloy 30 (alloy of silver and silicon) is locally formed as a tiny electrical conduction portion (local conduction portion) in the impurity diffusion layer 4 in contact with the light incident side surface electrode 20. It should be noted that the AgSi alloy 30 is locally formed in a limited portion, so Figure 1Illustration omitted. It is believed that good electrical conduction between the light incident side surface electrode 20 and the impurity diffusion layer 4 can be achieved through the tiny electrically conductive portion formed locally. In addition, an anti-reflection film 2 (passivation film) exists in most of the space between the light incident side surface electrode 20 and the impurity diffusion layer 4 other than the portion where the local conductive portion is formed. As a result, as a performance of the solar cell, the fill factor (FF) can be improved without reducing the open circuit voltage (Voc). Therefore, the conductive paste used to form the light incident side surface electrode 20 using a laser processing process needs to have properties different from those of the conventional conductive paste (conductive paste that can burn through the anti-reflection film 2).

[0018] In addition, in the case of a conventional crystalline silicon solar cell, when forming the light incident side surface electrode 20, the electrode pattern of the conductive paste is fired, thereby burning through the anti-reflection film 2 and contacting the impurity diffusion layer 4. During this burning, the impurity diffusion layer 4 is damaged, and there is a problem of reduced performance of the crystalline silicon solar cell. In contrast, in the laser processing process, when forming the light incident side surface electrode 20, the anti-reflection film 2 is basically not burned through. Therefore, by using the laser processing process, it is possible to suppress the impurity diffusion layer 4 from being damaged.

[0019] Therefore, an object of the present invention is to provide a conductive paste suitable for forming electrodes by a laser processing process in order to manufacture a crystalline silicon solar cell.

[0020] In addition, the present invention aims to provide a method for manufacturing a high-performance crystalline silicon solar cell, which uses a conductive paste suitable for forming electrodes by a laser processing process. In addition, the present invention aims to provide a high-performance crystalline silicon solar cell, which is manufactured by a manufacturing method including electrode formation based on a laser processing process.

[0021] In order to solve the above-mentioned problems, the present invention has the following configurations.

[0022] (Composition 1)

[0023] Configuration 1 relates to a conductive paste for forming an electrode of a solar cell, the conductive paste comprising:

[0024] (A) conductive particles,

[0025] (B) an organic carrier, and

[0026] (C) glass frit,

[0027] The basicity B of the glass frit (C) GF The product B of the content G of the glass frit (C) GFG is in the range of 0.25 to 1.45, and the content G of the (C) glass frit is the content of the (C) glass frit in the conductive paste in parts by weight when the content of the (A) conductive particles in the conductive paste is 100 parts by weight.

[0028] (Composition 2)

[0029] Configuration 2 is the conductive paste of Configuration 1, wherein the (A) conductive particles include silver particles.

[0030] (Composition 3)

[0031] Configuration 3 is the conductive paste of configuration 1 or 2, wherein the (B) organic vehicle contains at least one selected from the group consisting of ethyl cellulose, rosin ester, acrylic resin, and an organic solvent.

[0032] (Composition 4)

[0033] Configuration 4 is the conductive paste according to any one of Configurations 1 to 3, wherein the content of PbO in the glass frit (C) in mol% is C PbO The product C of the above content G of the above (C) glass frit PbO ·G is in the range of 20 to 139.

[0034] (Composition 5)

[0035] Configuration 5 is the conductive paste according to any one of Configurations 1 to 4, wherein the content G of the (C) glass frit is 0.3 to 4.0 parts by weight.

[0036] (Composition 6)

[0037] Configuration 6 is the conductive paste according to any one of Configurations 1 to 4, wherein the content G of the glass frit (C) is 0.5 to 1.5 parts by weight.

[0038] (Composition 7)

[0039] Configuration 7 is the conductive paste according to any one of Configurations 1 to 6, wherein the glass frit (C) has a glass transition temperature of 300 to 600°C.

[0040] (Composition 8)

[0041] Configuration 8 is the conductive paste according to any one of Configurations 1 to 7, wherein the glass frit (C) contains at least one selected from the group consisting of ZnO, V 2 O 5 , WO 3 , and Nb 2 O 3 .

[0042] (Composition 9)

[0043] Configuration 9 is the conductive paste according to any one of Configurations 1 to 8, wherein the conductive paste further includes (D) aluminum particles.

[0044] (Composition 10)

[0045] Configuration 10 is the conductive paste of configuration 9, wherein the content of the (D) aluminum particles in the conductive paste is 0.1 to 2.0 parts by weight, based on 100 parts by weight of the (A) conductive particles in the conductive paste.

[0046] (Composition 11)

[0047] Configuration 11 relates to the conductive paste according to any one of Configurations 1 to 10, which is a conductive paste for forming an electrode of a solar cell.

[0048] Solar cells contain:

[0049] a semiconductor substrate of a first conductivity type;

[0050] a second conductivity type semiconductor layer disposed on one surface of the first conductivity type semiconductor substrate;

[0051] a back electrode arranged to be electrically connected to the other surface of the semiconductor substrate of the first conductivity type;

[0052] a passivation film arranged to be in contact with a surface of the second conductivity type semiconductor layer; and

[0053] a light incident side surface electrode disposed on at least a portion of the surface of the passivation film,

[0054] The light incident side surface electrode is the light incident side surface electrode processed as follows: while applying a voltage between the back electrode and the light incident side surface electrode, light from a point light source is irradiated onto the light incident side surface of the solar cell so that a current in a direction opposite to the forward direction flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate,

[0055] The conductive paste is a conductive paste for forming the light incident side surface electrode.

[0056] (Composition 12)

[0057] Configuration 12 relates to a solar cell, comprising:

[0058] a semiconductor substrate of a first conductivity type;

[0059] a second conductivity type semiconductor layer disposed on one surface of the first conductivity type semiconductor substrate;

[0060] a back electrode arranged to be electrically connected to the other surface of the semiconductor substrate of the first conductivity type;

[0061] a passivation film arranged to be in contact with a surface of the second conductivity type semiconductor layer; and

[0062] a light incident side surface electrode disposed on at least a portion of the surface of the passivation film,

[0063] The light incident side surface electrode is the light incident side surface electrode processed as follows: while applying a voltage between the back electrode and the light incident side surface electrode, light from a point light source is irradiated onto the light incident side surface of the solar cell so that a current in a direction opposite to the forward direction flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate,

[0064] The light incident side surface electrode is a fired body of the conductive paste according to any one of Items 1 to 10.

[0065] (Composition 13)

[0066] Configuration 13 relates to a solar cell, comprising:

[0067] a crystalline silicon substrate of a first conductivity type;

[0068] a second conductivity type silicon emitter layer disposed on one surface of the first conductivity type crystalline silicon substrate;

[0069] a back electrode arranged to be electrically connected to the other surface of the first conductivity type crystalline silicon substrate;

[0070] a passivation film arranged to be in contact with a surface of the second conductivity type silicon emitter layer; and

[0071] a light incident side surface electrode comprising silver, which is disposed on at least a portion of the surface of the passivation film,

[0072] The second conductivity type silicon emitter layer has a local conductive portion that is in direct contact with the light incident side surface electrode without a passivation film therebetween.

[0073] The local conductive portion includes an alloy of silver and silicon.

[0074] The light incident side surface electrode is a fired body of the conductive paste according to any one of configurations 1 to 10.

[0075] (Composition 14)

[0076] Configuration 14 relates to a method for manufacturing a solar cell, comprising:

[0077] A step of preparing a semiconductor substrate of a first conductivity type;

[0078] forming a second conductivity type semiconductor layer on one surface of the first conductivity type semiconductor substrate;

[0079] forming a back electrode in electrical connection with the other surface of the semiconductor substrate of the first conductivity type;

[0080] forming a passivation film in contact with the surface of the second conductivity type semiconductor layer;

[0081] a step of forming a light incident side surface electrode on at least a portion of the surface of the passivation film, and

[0082] The step of applying a voltage between the back electrode and the light incident side surface electrode and irradiating the light incident side surface of the solar cell with light from a point light source so that a current in a direction opposite to the forward direction flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate,

[0083] The light incident side surface electrode is a fired body of the conductive paste according to any one of Items 1 to 10.

[0084] (Composition 15)

[0085] Configuration 14 relates to use of the conductive paste according to any one of Configurations 1 to 11 for forming an electrode of a solar cell.

[0086] According to the present invention, it is possible to provide a conductive paste suitable for forming electrodes by a laser processing process in order to manufacture a crystalline silicon solar cell.

[0087] In addition, according to the present invention, a method for manufacturing a high-performance crystalline silicon solar cell can be provided, which uses a conductive paste suitable for forming electrodes using a laser processing process. In addition, according to the present invention, a high-performance crystalline silicon solar cell can be provided, which is manufactured by a manufacturing method including electrode formation based on a laser processing process. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] Figure 1 This is an example of a schematic cross-sectional view showing a structure in which a light-incident-side surface electrode is formed on the light-incident-side surface of a crystalline silicon solar cell by a laser processing process using the conductive paste of the present embodiment.

[0089] Figure 2 This is an example of a schematic diagram of the light incident side surface of a crystalline silicon solar cell.

[0090] Figure 3This is an example of a schematic diagram of the back side of a crystalline silicon solar cell.

[0091] Figure 4 This is an example of a schematic cross-sectional view of a double-sided light-receiving crystalline silicon solar cell using the conductive paste of the present embodiment.

[0092] Figure 5 This is an example of a cross-sectional schematic diagram of a conventional crystalline silicon solar cell, in which a surface electrode (finger electrode) on the light incident side exists, and is a cross-sectional schematic diagram showing a state in which the anti-reflection film (passivation film) between the electrode and the impurity diffusion layer disappears due to burn-through.

[0093] Figure 6 This is a schematic plan view showing a resistivity measurement pattern for an electrode formed using a conductive paste.

[0094] Figure 7 This is a schematic plan view showing a pattern for measuring contact resistance of an electrode formed using a conductive paste.

[0095] Figure 8 It is a schematic plan view showing a pattern for measurement by photoluminescence imaging (PL method) of an electrode formed using a conductive paste.

[0096] Fig. 9 This is an image of the photoluminescence intensity of the sample of Example 4 measured by the photoluminescence imaging method (PL method).

[0097] Fig.10 This is an image of the photoluminescence intensity of Comparative Example 1 measured by the photoluminescence imaging method (PL method).

[0098] Fig.11 Is used with Fig. 9 This is a cross-sectional SEM photograph (magnification: 20,000 times) of the sample in which the light-incident-side surface electrode 20 is formed with the same conductive paste as the sample shown, showing the vicinity of the passivation film on the light-incident-side surface.

[0099] Fig.12 Is used with Fig.10 This is a cross-sectional SEM photograph (magnification: 20,000 times) of the sample in which the light-incident-side surface electrode 20 is formed with the same conductive paste as the sample shown, showing the vicinity of the passivation film on the light-incident-side surface.

[0100] Fig.13 It is a cross-sectional SEM photograph (magnification 20,000 times) of an AgSi alloy in which an impurity diffusion layer in contact with the surface electrode on the light incident side of a sample produced under the same conditions as in Example 5 locally forms a tiny electrically conductive portion (local conductive portion). DETAILED DESCRIPTION

[0101] Hereinafter, embodiments of the present invention will be described in detail. It should be noted that the following embodiments are only modes for embodying the present invention, and are not intended to limit the scope of the present invention.

[0102] In this specification, "crystalline silicon" includes single crystal and polycrystalline silicon. In addition, "crystalline silicon substrate" refers to a material in which crystalline silicon is formed into a flat plate or other shape suitable for forming a component in order to form a semiconductor device such as an electrical component or an electronic component. Any method can be used to manufacture crystalline silicon. For example, in the case of single crystal silicon, the Czochralski method can be used, and in the case of polycrystalline silicon, the casting method can be used. In addition, polycrystalline silicon ribbons produced by other manufacturing methods, such as the ribbon pulling method, and polycrystalline silicon formed on heterogeneous substrates such as glass can also be used as crystalline silicon substrates. In addition, a "crystalline silicon solar cell" refers to a solar cell made using a crystalline silicon substrate.

[0103] In this specification, glass frit is mainly composed of various oxides, for example, metal oxides, and is usually used in the form of glassy particles.

[0104] The present embodiment is a conductive paste for forming an electrode of a solar cell. The conductive paste of the present embodiment comprises (A) conductive particles, (B) an organic vehicle, and (C) glass frit. The conductive paste of the present embodiment is characterized in that the alkalinity of the (C) glass frit and the content of the (C) glass frit in the conductive paste are appropriately controlled.

[0105] The light-to-electricity conversion efficiency of a solar cell (sometimes referred to as "conversion efficiency") is represented by the product of the fill factor (FF), the open circuit voltage (Voc), and the short circuit current (Jsc). Basically, FF and Voc are in a trade-off relationship, and it is difficult to improve both FF and Voc at the same time. For example, it is described in Patent Documents 1 and 2 that by using a laser processing process when manufacturing crystalline silicon solar cells, the ohmic contact behavior between the electrode in the shape of a grid line as the surface electrode on the light incident side and the impurity diffusion layer (emitter layer) can be improved, and the contact resistance between the surface electrode on the light incident side and the impurity diffusion layer can be greatly reduced. Therefore, by performing a laser processing process, FF can be improved without reducing Voc.

[0106] The present inventors have found that when a laser treatment process is applied to a solar cell having a surface electrode on the light incident side formed using a conventional conductive paste (e.g., the conductive paste described in Patent Document 3), an adverse effect is caused on the anti-reflection film (passivation film) and the impurity diffusion layer (and substrate), and the conversion efficiency of the solar cell is reduced. In addition, the present inventors have found that the reason is that the existing conductive paste has too strong burn-through (reactivity) to the anti-reflection film (passivation film). In addition, the present inventors have found that by setting the alkalinity and content of the glass frit to an appropriate range, the reactivity of the glass frit to the anti-reflection film (passivation film) can be made appropriate. The present inventors who have obtained the above insights have found a conductive paste that can be preferably used when manufacturing crystalline silicon using a laser treatment process, thereby completing the present invention.

[0107] By using the conductive paste of this embodiment to form the electrode of the crystalline silicon solar cell and performing a laser treatment process, a low contact resistance can be obtained between the electrode and the impurity diffusion layer of the solar cell without damaging the function of the passivation film of the anti-reflection film. Therefore, by using the conductive paste of this embodiment to perform a laser treatment process, a crystalline silicon solar cell with high conversion efficiency can be obtained. The conductive paste of this embodiment forms a light incident side surface electrode by a laser treatment process when manufacturing a crystalline silicon solar cell, so it can be preferably used.

[0108] In the laser processing process using the conductive paste of the present embodiment, when forming the light incident side surface electrode 20, the anti-reflection film 2 (passivation film) is basically not burned through. In addition, even if the light incident side surface electrode 20 is subjected to the laser processing process, most of the anti-reflection film 2 (passivation film) in contact with the light incident side surface electrode 20 will not disappear. That is, the anti-reflection film 2 (passivation film) exists in most of the area between the light incident side surface electrode 20 and the impurity diffusion layer 4 (for example, more than 90% of the area of ​​the interface, preferably more than 95% of the area, and more preferably more than 99% of the area). Therefore, by using the laser processing process when forming the light incident side surface electrode 20, it is possible to suppress the occurrence of damage to the impurity diffusion layer 4.

[0109] like Figure 1 As shown in FIG. 1 , a finger electrode 20b is arranged as a light incident side surface electrode 20 on the light incident side surface of the crystalline silicon solar cell. Figure 1 In the example shown, among the electron-hole pairs generated by incident light entering the crystalline silicon solar cell, the holes are collected at the finger electrodes 20b through the impurity diffusion layer 4 (for example, the p-type impurity diffusion layer 4). Therefore, it is required that the contact resistance between the finger electrodes 20b and the impurity diffusion layer 4 is low. The conductive paste of this embodiment can be preferably used for forming the finger electrodes 20b.

[0110] In addition, in this specification, the light incident side surface electrode 20 and the back surface electrode 15 which are electrodes for extracting electric current from the crystalline silicon solar cell to the outside are sometimes simply referred to as "electrodes" in combination.

[0111] One type of crystalline silicon solar cell is a double-sided power generation type crystalline silicon solar cell that generates electricity by incident light from two surfaces (the first and second light incident side surfaces). In this case, the conductive paste of this embodiment can be used, and preferably electrodes formed on the first and second light incident side surfaces are used.

[0112] The conductive paste of the present embodiment can be preferably used to form a light incident side surface electrode 20, which is formed on the surface (light incident side surface) of the anti-reflection film 2 (passivation film) formed on the impurity diffusion layer, but is not limited to this. For example, the conductive paste of the present embodiment can also be used to form a back electrode 15 on the surface (back side) opposite to the light incident side surface. Sometimes a passivation film is formed on the back side of a crystalline silicon solar cell, and a back electrode 15 is formed on the passivation film. In the case of a solar cell of this structure, as described above, the conductive paste of the present embodiment can be used to form an electrical contact between the back electrode 15 and the crystalline silicon substrate 1 of the solar cell through the passivation film on the back side.

[0113] The conductive paste of the present invention is described below by taking the case of forming a light incident side electrode 20 (surface electrode) of a crystalline silicon solar cell using an n-type crystalline silicon substrate 1 as an example. In the case of this crystalline silicon solar cell, the impurity diffusion layer 4 formed on the light incident side surface is a p-type impurity diffusion layer 4. It should be noted that in this specification, the impurity diffusion layer 4 in the case of a solar cell using a crystalline silicon substrate 1 is sometimes referred to as a "silicon emitter layer". In addition, an anti-reflection film 2 is formed on the surface of the p-type impurity diffusion layer 4.

[0114] The passivation film (anti-reflection film 2) may be a film formed of a single layer or multiple layers. In the case where the passivation film is a single layer, a thin film (SiN film) made of silicon nitride (SiN) is preferred from the perspective of being able to effectively passivate the surface of the silicon substrate. In addition, in the case where the passivation film is a multilayer film, it may be a laminated film (SiN / SiO2) of a thin film made of silicon nitride and a thin film made of silicon oxide. x It should be noted that in SiN / SiO x When the film is a passivation film, SiO is preferably used because the surface of the silicon substrate can be passivated more effectively. x The SiN / SiO film is formed in a way that it contacts the silicon substrate 1 x Film. SiOx The film may be a natural oxide film of a silicon substrate.

[0115] The crystalline silicon solar cell may have a light incident side bus electrode 20a and / or a back TAB electrode 15a. The light incident side bus electrode 20a has the function of electrically connecting the finger electrode 20b for collecting the current generated by the solar cell to the metal strip for interconnection. Similarly, the back TAB electrode 15a has the function of electrically connecting the back full-surface electrode 15b for collecting the current generated by the solar cell to the metal strip for interconnection. If the finger electrode 20b is in contact with the crystalline silicon substrate 1, the surface defect density of the surface (interface) of the crystalline silicon substrate 1 in the portion where the finger electrode 20b is in contact increases, and the performance of the solar cell decreases. The conductive paste of the present invention, especially as a conductive paste facing the finger electrode 20b, has low burn-through (reactivity) to the anti-reflection film 2, so the anti-reflection film 2 will not be completely burned through. Therefore, when the finger electrode 20b is formed using the conductive paste of the present invention, the passivation film in the portion in contact with the crystalline silicon substrate 1 can be kept in the same state, and the increase in the surface defect density that causes the recombination of carriers can be prevented. Therefore, the conductive paste of the present embodiment described above can be suitably used as a conductive paste for forming the finger electrodes 20b of a crystalline silicon solar cell. Figure 4 As shown, the conductive paste of this embodiment can also be suitably used as the back electrode 15 (back finger electrodes 15c) of a double-sided light-receiving crystalline silicon solar cell. In addition, the entire electrode 20 can be formed using the conductive paste of this embodiment.

[0116] Regarding the conductive paste of this embodiment, by applying the above-mentioned predetermined voltage in the laser processing process and irradiating light from a point light source, a current flows in a tiny area between the light incident side surface electrode 20 and the impurity diffusion layer 4 (silicon emitter layer), and the area is locally heated. As a result, Fig.13 As shown, an AgSi alloy 30 is formed as a local electrical conduction portion (local conduction portion) in the impurity diffusion layer 4 (silicon emitter layer) in contact with the light incident side surface electrode 20. It is considered that good electrical conduction between the light incident side surface electrode 20 and the impurity diffusion layer 4 (silicon emitter layer) can be achieved through this locally formed electrical conduction portion. Therefore, the conductive paste used to form the light incident side surface electrode by the laser processing process needs to have properties different from the conventional conductive paste (conductive paste that can burn through the anti-reflection film 2).

[0117] The conductive paste according to this embodiment will be described in detail.

[0118] <(A) Conductive particles>

[0119] The conductive paste of this embodiment contains (A) conductive particles.

[0120] In the conductive paste of the present embodiment, metal particles or alloy particles can be used as conductive particles. As metals contained in metal particles or alloy particles, silver, gold, copper, nickel, zinc and tin can be cited. As metal particles, silver particles (Ag particles) can be used. It should be noted that the conductive paste of the present embodiment may contain other metals other than silver, such as gold, copper, nickel, zinc and tin. From the perspective of obtaining low resistance and high reliability, the conductive particles are preferably silver particles formed of silver. It should be noted that other metal elements inevitably contained as impurities may be contained in the silver particles formed of silver. In addition, a plurality of silver particles (Ag particles) are sometimes referred to as silver powder (Ag powder). The same is true for other particles.

[0121] The particle shape and particle size (also referred to as particle diameter or particle diameter) of the conductive particles are not particularly limited. As particle shapes, for example, spherical and flaky shapes can be used. The particle size of the conductive particles can be specified by the particle size (D50) of 50% of the cumulative value of all particles. In this specification, D50 is also referred to as the average particle diameter. It should be noted that the average particle diameter (D50) can be obtained by measuring the particle size distribution using the Microtrac method (laser diffraction scattering method) based on the results of the particle size distribution measurement.

[0122] The average particle diameter (D50) of the conductive particles is preferably 0.5 to 2.5 μm, more preferably 0.8 to 2.2 μm. By making the average particle diameter (D50) of the conductive particles within a specified range, the reactivity of the conductive paste to the passivation film can be suppressed during the firing of the conductive paste. It should be noted that when the average particle diameter (D50) is greater than the above range, problems such as clogging may occur during screen printing.

[0123] The size of the silver particles can be expressed as the BET specific surface area (also simply referred to as "specific surface area"). The BET specific surface area of ​​the silver particles is preferably 0.1 to 1.5 m 2 / g, more preferably 0.2 to 1.2 m 2 The BET specific surface area can be measured using, for example, a fully automatic specific surface area measuring device, Macsoeb (manufactured by MOUNTEC).

[0124] <(B) Organic carrier>

[0125] The conductive paste of this embodiment contains (B) an organic vehicle.

[0126] The organic vehicle may include an organic binder and a solvent. The organic binder and the solvent play roles such as adjusting the viscosity of the conductive paste, and are not particularly limited. The organic binder may be dissolved in a solvent and used.

[0127] The conductive paste of this embodiment preferably has (B) an organic vehicle containing at least one selected from ethyl cellulose, rosin ester, acrylic resin and an organic solvent. By making (B) an organic vehicle containing at least one selected from ethyl cellulose, rosin ester, acrylic resin and an organic solvent, the conductive paste can be screen-printed appropriately, and the shape of the printed pattern can be made into an appropriate shape.

[0128] As an organic binder, it can be selected from cellulose resins (such as ethyl cellulose, nitrocellulose, etc.) and (meth) acrylic resins (such as polymethacrylate, polymethyl methacrylate, etc.). The organic carrier contained in the conductive paste of this embodiment preferably includes at least one selected from ethyl cellulose, rosin ester, butyral, acrylic resin and organic solvent. The amount of the organic binder added is usually 0.1 to 30 parts by weight, preferably 0.2 to 5 parts by weight, relative to 100 parts by weight of silver particles.

[0129] As the organic solvent, one or more kinds can be selected from alcohols (such as terpineol, α-terpineol, β-terpineol, etc.), esters (such as hydroxyl-containing esters, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, diethylene glycol monobutyl ether acetate (butyl carbitol acetate), etc.). The amount of the solvent added is usually 0.5 to 30 parts by weight, preferably 2 to 25 parts by weight, relative to 100 parts by weight of the silver particles. As a specific example of the organic solvent, diethylene glycol monobutyl ether acetate (butyl carbitol acetate) can be cited.

[0130] <(C) Glass frit>

[0131] The conductive paste of this embodiment contains (C) glass frit.

[0132] Regarding the conductive paste of this embodiment, (C) the basicity B of the glass frit GF The product of (C) the content of glass frit G GF G is in the range of 0.25 to 1.45, preferably in the range of 0.3 to 1.4, and more preferably in the range of 0.4 to 1.2, wherein the content G of the glass frit (C) is the content of the glass frit (C) in the conductive paste in parts by weight when the content of the conductive particles (A) in the conductive paste is 100 parts by weight. GF The product of B and content G GFWhen G is within an appropriate range, the reactivity of the glass frit to the antireflection film 2 (passivation film) can be made appropriate. Therefore, when crystalline silicon is produced using a laser processing process, the conductive paste of the embodiment can be preferably used.

[0133] The basicity of the glass frit can be calculated by the method described in Patent Document 4 (Japanese Patent Application Laid-Open No. 2009-231826). That is, the basicity of the glass powder can be defined by the formula shown in "K. Morinaga, H. Yoshida and H. Takebe: J. Am Cerm. Soc., 77, 3113 (1994)". Specifically, it is as follows.

[0134] Oxide M i O'M i The bonding force between -O is given by the following formula as the attraction force Ai between cation and oxygen ion.

[0135] A i =Z i ·Z 02- / (r i +r 02- ) 2 =Zi·2 / (r i +1.40) 2

[0136] Z i : The valence of the cation, oxygen ion is 2

[0137] r i : Ionic radius of the cation

[0138] The ionic radius of oxygen ions is r i is 1.40 nm. i The reciprocal of B i (=1 / A i ) as a single component oxide M i Oxygen supply capacity.

[0139] B i ≡1 / A i

[0140] If the B i Standardized to BCaO = 1, BSiO2 = 0, the B of each single component oxide is given i -Indicator. The B of each component is measured by the cation fraction. i - When the index is extended to a multi-component system, the basicity (=B GF ).

[0141] BGF =Σn i ·B i

[0142] n i : Cation fraction

[0143] The alkalinity (B GF ) indicates the oxygen supply capacity as described above. The larger the value, the easier it is to supply oxygen, and the easier it is to transfer oxygen with other metal oxides. That is, "basicity" can indicate the degree of dissolution into the glass melt.

[0144] The content G of the glass frit (C) is a ratio relative to the content of the conductive particles (A), and is therefore a dimensionless number. i It is a value normalized to BCaO=1 and BSiO2=0, so (C) the basicity B of the glass frit is GF (=Σn i ·B i ) is a dimensionless number. Therefore, (C) the basicity B of the glass frit GF The product of B and content G GF G is also a dimensionless number.

[0145] The basicity (B GF ) is preferably 0.30 to less than 0.80, more preferably 0.35 to 0.75, and further preferably 0.40 to 0.70. GF ) is within such a range, by adjusting the amount of glass frit added to the conductive paste, the reactivity of the glass frit to the passivation film can be made appropriate.

[0146] The content G of the glass frit in the conductive paste of the present embodiment is preferably 0.3 to 4.0 parts by weight, more preferably 0.4 to 3.0 parts by weight, further preferably 0.5 to 2.0 parts by weight, and particularly preferably 0.5 to 1.5 parts by weight, relative to 100 parts by weight of the conductive particles. GF ) together, the reactivity of the glass frit to the passivation film can be made appropriate.

[0147] The glass frit contained in the conductive paste of the present embodiment preferably contains one or more selected from PbO, SiO2, Al2O3, B2O3, ZnO, V2O5, WO3, and Nb2O3. The glass frit contained in the conductive paste of the present embodiment more preferably contains PbO, SiO2, Al2O3, B2O3, and ZnO.

[0148] In the conductive paste of the present embodiment, it is preferred that the glass frit (C) contains at least one selected from ZnO, V2O5, WO3, and Nb2O3. By making the glass frit contain at least one of these oxides, the basicity of the glass frit can be adjusted to a suitable range.

[0149] The glass frit preferably contains PbO. The content of PbO in the glass frit (100 mol%) is preferably 25 to 60 mol%, more preferably 30 to 55 mol%, and further preferably 40 to 55 mol%. When the glass frit contains PbO, the reactivity to the passivation film can be suppressed and the contact resistance can be reduced.

[0150] The glass frit preferably contains SiO 2. The content of SiO 2 in the glass frit (100 mol%) is preferably 20 to 65 mol%, more preferably 25 to 60 mol%. When the glass frit contains SiO 2, the reactivity with the passivation film can be suppressed.

[0151] The glass frit preferably contains Al 2 O 3. The content of Al 2 O 3 in the glass frit (100 mol %) is preferably 3.0 to 6.8 mol %, more preferably 3.5 to 6 mol %. When the glass frit contains Al 2 O 3, the reactivity with the passivation film can be suppressed.

[0152] The glass frit preferably contains B 2 O 3. The content of B 2 O 3 in the glass frit (100 mol %) is preferably 3.0 to 15 mol %, more preferably 3.5 to 12 mol %.

[0153] The glass frit preferably contains ZnO. The content of ZnO in the glass frit (100 mol%) is preferably 5 to 20 mol%, more preferably 8 to 15 mol%. When the glass frit contains ZnO, the basicity of the glass frit can be adjusted to a suitable range.

[0154] Regarding the conductive paste of the present embodiment, (C) the content of PbO in the glass frit in mol% is C PbO The product of (C) the content G of the glass frit PbO G is preferably in the range of 20 to 139, more preferably in the range of 22 to 130, and still more preferably in the range of 26 to 105. PbO When G exceeds 139, the reactivity between the glass frit and the passivation film becomes too high. PbO When G is less than 20, the contact resistance between the obtained electrode and the impurity diffusion layer becomes too high.

[0155] In the conductive paste of the present embodiment, the glass transition temperature (Tg) of the glass frit (C) is preferably 300 to 600° C., more preferably 320 to 500° C., and even more preferably 350 to 450° C. By setting the glass transition temperature (Tg) of the glass frit (C) to 300° C. or higher, the reactivity to the passivation film can be suppressed. In addition, by setting the glass transition temperature (Tg) to 600° C. or lower, the contact resistance between the obtained electrode and the impurity diffusion layer can be reduced.

[0156] The glass transition temperature (Tg) can be measured as follows. That is, a differential thermobalance (TG-DTA2000S manufactured by MAC Science Co., Ltd.) is used, a glass powder as a sample and a reference substance are set in the differential thermobalance, and as a measurement condition, the temperature is raised from room temperature to 900°C at a heating rate of 10°C / min, and a curve (DTA curve) is obtained by plotting the temperature difference between the glass powder as a sample and the reference substance relative to the temperature. For the DTA curve thus obtained, the first inflection point can be used as the glass transition temperature Tg.

[0157] The shape of the glass frit particles is not particularly limited, and for example, spherical or amorphous shapes can be used. In addition, the particle size is not particularly limited. From the perspective of workability, the average particle diameter (D50) of the particles is preferably in the range of 0.1 to 10 μm, and more preferably in the range of 0.5 to 5 μm.

[0158] The particles of the glass frit can use one kind of particles each containing a predetermined amount of a plurality of desired oxides. In addition, particles formed of a single oxide can be used as different particles for each of the plurality of desired oxides. In addition, a plurality of particles having different compositions of the plurality of desired oxides can be used in combination.

[0159] <Aluminum particles>

[0160] The conductive paste of this embodiment may further contain (D) aluminum particles. The (D) aluminum particles may be contained in the form of particles different from the (A) conductive particles.

[0161] In a crystalline silicon substrate, aluminum has the property of being a p-type impurity. When the conductive paste printed on the crystalline silicon is fired, the aluminum in the conductive paste diffuses into the crystalline silicon and becomes a p-type impurity. Therefore, when an electrode is formed on the surface of the p-type impurity diffusion layer of the crystalline silicon substrate, by making the conductive paste contain aluminum particles, a low contact resistance can be obtained between the electrode and the p-type impurity diffusion layer. Therefore, when an electrode is formed on the surface of the p-type impurity diffusion layer of the crystalline silicon substrate, the conductive paste preferably contains aluminum particles.

[0162] When the conductive paste of the present embodiment includes the (D) aluminum particles, the content of the (D) aluminum particles in the conductive paste is preferably 0.1 to 2.0 parts by weight, and more preferably 0.5 to 2.0 parts by weight, based on 100 parts by weight of the (A) conductive particles in the conductive paste. By including a predetermined amount of aluminum particles in the conductive paste, a low contact resistance can be obtained between the electrode and the p-type impurity diffusion layer.

[0163] On the other hand, when an electrode is formed on the n-type impurity diffusion layer of a crystalline silicon substrate or on the surface of an n-type crystalline silicon substrate, the aluminum in the conductive paste diffuses into the n-type impurity diffusion layer, etc., thereby adversely affecting the characteristics of the solar cell. Therefore, when an electrode is formed on the n-type impurity diffusion layer of a crystalline silicon substrate or on the surface of an n-type crystalline silicon substrate, the conductive paste of this embodiment preferably does not contain (D) aluminum particles (the content of (D) aluminum particles is zero).

[0164] The aluminum particles mainly contain aluminum elements. The purity of aluminum in the aluminum particles is preferably 99.7% or more, and more preferably 99.9% or more. The aluminum particles may contain impurities other than aluminum, such as other metal elements that are inevitably contained. In addition, the aluminum particles may contain alloys of aluminum and other metal elements, and aluminum oxides, etc.

[0165] The shape of the aluminum particles may be spherical or ellipsoidal, but is not limited thereto. The shape of the aluminum particles is preferably spherical from the viewpoint of good printability and good reaction with a semiconductor substrate.

[0166] The average particle size (D50) of the aluminum particles is not particularly limited. If the average particle size (D50) of the aluminum particles is 1 μm or more and 20 μm or less, the printability of the paste composition is improved and the reactivity with the semiconductor substrate is also improved, which is preferred. The more preferred average particle size (D50) of the aluminum particles is 2 to 4 μm.

[0167] <Other ingredients>

[0168] The conductive paste of the present embodiment may contain additives and additives other than the above-mentioned substances within a range that does not adversely affect the solar cell characteristics of the obtained solar cell.

[0169] The conductive paste of the present embodiment may further contain additives selected from plasticizers, defoamers, dispersants, leveling agents, stabilizers, adhesion promoters, etc. as additives as needed. Among them, as a plasticizer, at least one selected from phthalates, glycolates, phosphates, sebacates, adipic acid esters, and citrates may be used.

[0170] The conductive paste of the present embodiment may contain additives other than those mentioned above within a range that does not adversely affect the solar cell characteristics of the obtained solar cell. For example, the conductive paste of the present embodiment may further contain at least one additive selected from titanium resinate (Japanese: チタンレジネート), titanium oxide, cobalt oxide, cerium oxide, silicon nitride, copper manganese tin, aluminosilicate and aluminum silicate. By including these additives, the bonding strength of the electrode relative to the passivation film can be improved. These additives can be in the form of particles (additive particles). The amount of additive added relative to 100 parts by weight of silver particles is preferably 0.01 to 5 parts by weight, and more preferably 0.05 to 2 parts by weight. In order to obtain higher bonding strength, the additive is preferably copper manganese tin, aluminosilicate or aluminum silicate. The additive may include both aluminosilicate and aluminum silicate.

[0171] <Method for producing conductive paste>

[0172] Next, a method for producing the conductive paste of the present embodiment will be described. The conductive paste of the present embodiment can be produced by adding silver particles, glass frit, and other additives and / or additives as needed to an organic binder and a solvent, followed by mixing and dispersing.

[0173] Mixing can be performed using a planetary mixer, for example. In addition, dispersion can be performed using a three-roll mill. Mixing and dispersion are not limited to these methods, and various known methods can be used.

[0174] <Solar Cell>

[0175] Next, a solar cell according to this embodiment will be described. This embodiment is a solar cell in which at least a portion of an electrode is formed using the above-mentioned conductive paste. Figure 1 and Figure 4 A schematic cross-sectional view of a crystalline silicon solar cell is shown in FIG.

[0176] In the solar cell of this embodiment, as the material of the semiconductor substrate, crystalline silicon, silicon carbide, germanium, gallium arsenide, etc. can be used. From the perspective of safety and cost as a solar cell, the material of the semiconductor substrate is preferably crystalline silicon (single crystal silicon and polycrystalline silicon, etc.).

[0177] The solar cell of the present embodiment includes: a semiconductor substrate of the first conductivity type; a semiconductor layer of the second conductivity type, which is arranged on one surface of the semiconductor substrate of the first conductivity type; a passivation film (anti-reflection film 2), which is arranged in contact with the surface of the semiconductor layer of the second conductivity type; and a light incident side surface electrode 20, which is arranged on at least a portion of the surface of the passivation film. In addition, the solar cell of the present embodiment may include a back electrode 15 arranged in electrical connection with the other surface of the semiconductor substrate of the first conductivity type. Figure 1 In the example, the first conductivity type semiconductor substrate is a crystalline silicon substrate 1 , the second conductivity type semiconductor layer is an impurity diffusion layer 4 , and the passivation film is an anti-reflection film 2 .

[0178] The semiconductor substrate of the first conductivity type is an n-type semiconductor substrate or a p-type semiconductor substrate. The semiconductor layer of the second conductivity type refers to a p-type semiconductor layer or an n-type semiconductor layer. When the semiconductor substrate is an n-type semiconductor substrate, a p-type semiconductor layer (p-type impurity diffusion layer 4) is arranged on one surface of the semiconductor substrate. When the semiconductor substrate is a p-type semiconductor substrate, an n-type semiconductor layer (n-type impurity diffusion layer 4) is arranged on one surface of the semiconductor substrate. The material of the semiconductor substrate is preferably silicon. Therefore, the semiconductor substrate is preferably a crystalline silicon substrate.

[0179] The passivation film may be the anti-reflection film 2. The passivation film is preferably a thin film made of silicon nitride.

[0180] The light incident side surface electrode 20 of the solar cell of the present embodiment may be a fired product of the conductive paste of the present embodiment. The conductive paste of the present embodiment can be used to manufacture a solar cell of this structure.

[0181] In order to form the light incident side surface electrode 20 of the crystalline silicon solar cell using a laser processing process, the conductive paste of the present embodiment can be preferably used. The laser processing process refers to the following processing: while applying a voltage to the back electrode 15 and the light incident side surface electrode 20, the light incident side surface of the solar cell is irradiated with light from a point light source, so that between the above-mentioned second conductive type semiconductor layer and the above-mentioned first conductive type semiconductor substrate, a current in the opposite direction to the forward direction flows in the pn junction. The light from the point light source generates carriers (electron-hole pairs) inside the semiconductor substrate, and the application of voltage enables the movement of carriers, that is, the flow of current. The voltage is applied in such a way that the flow direction of the current in the pn junction becomes the opposite direction to the forward direction. Therefore, when the semiconductor substrate is an n-type semiconductor substrate and the semiconductor layer is a p-type semiconductor layer, a voltage is applied to the back electrode 15 and the light incident side surface electrode 20 in such a way that the current flows from the n-type semiconductor substrate to the p-type semiconductor layer. When the semiconductor substrate is a p-type semiconductor substrate and the semiconductor layer is an n-type semiconductor layer, voltage is applied to the back electrode 15 and the light incident side surface electrode 20 so that current flows from the n-type semiconductor layer to the p-type semiconductor substrate.

[0182] The first conductive type semiconductor substrate of the solar cell of the present embodiment is preferably an n-type semiconductor substrate, and more preferably an n-type crystalline silicon substrate. In addition, the second conductive type semiconductor layer of the solar cell of the present embodiment is preferably a p-type semiconductor layer, and more preferably a p-type impurity diffusion layer 4 made of crystalline silicon. Generally, the mobility of electrons as carriers in an n-type crystalline silicon substrate is higher than the mobility of holes as carriers in a p-type crystalline silicon substrate. Therefore, in order to obtain a solar cell with high conversion efficiency, it is advantageous to use an n-type crystalline silicon substrate.

[0183] In the following description, a solar cell in which the first conductivity type semiconductor substrate is an n-type crystalline silicon substrate 1 and the second conductivity type semiconductor layer is a p-type impurity diffusion layer 4 (sometimes simply referred to as “impurity diffusion layer 4”) is described as an example.

[0184] like Figure 1 As shown in FIG. 1 , when a laser treatment process is used, an anti-reflection film 2 (passivation film) exists in most of the space between the light incident side surface electrode 20 and the impurity diffusion layer 4. In the laser treatment process, the voltage specified above is applied in such a way that a current flows in the opposite direction to the forward direction in the pn junction, and light (such as laser) from a point light source is irradiated, thereby flowing a current in a tiny area between the light incident side surface electrode 20 and the impurity diffusion layer 4, causing local heating. As a result, as shown in FIG. Fig.13 As shown, an AgSi alloy 30 (alloy of silver and silicon) is locally formed as an electrical conduction portion (local conduction portion) between the light incident side surface electrode 20 and the impurity diffusion layer 4. That is, the local conduction portion contains an alloy of silver and silicon. In addition, in the local conduction portion, the impurity diffusion layer 4 (silicon emitter layer of the second conductivity type) is in direct contact with the above-mentioned light incident side surface electrode without the anti-reflection film 2 (passivation film) in between. Through this locally formed electrical conduction portion (local conduction portion), good electrical conduction between the light incident side surface electrode 20 and the impurity diffusion layer 4 can be achieved. Compared with conventional conductive pastes, the conductive paste of this embodiment has a lower reactivity to the anti-reflection film 2 and has a reactivity with the anti-reflection film 2 (passivation film) suitable for laser processing. Therefore, the conductive paste of this embodiment can be preferably used to form the light incident side surface electrode 20 of a crystalline silicon solar cell using a laser processing process.

[0185] Figure 1 The crystalline silicon solar cell shown may have Figure 3 The back electrode 15 is configured to be electrically connected to the other surface of the semiconductor substrate of the first conductivity type. Figure 3 As shown, the back electrode 15 may generally include a back entire surface electrode 15 b and a back TAB electrode 15 a electrically connected to the back entire surface electrode 15 b .

[0186] exist Figure 4 An example of a schematic cross-sectional view of a double-sided light-receiving crystalline silicon solar cell is shown in FIG. Figure 4 The double-sided light-receiving type crystalline silicon solar cell shown has an impurity diffusion layer 4, an anti-reflection film 2, and a back passivation film 14. In the double-sided light-receiving type crystalline silicon solar cell, in order to form the light-incident side surface electrode 20 (especially the finger electrode 20b) and the back electrode 15 (back finger electrode 15c) on the light-incident side surface, by using the conductive paste of this embodiment, a portion (local conductive portion) electrically connected to the passivation film (anti-reflection film 2) on the light-incident side surface and the back passivation film 14 can be formed using a laser processing process.

[0187] Therefore, the conductive paste of the present embodiment can be suitably used as a conductive paste for forming the finger electrodes 20b of a crystalline silicon solar cell. In addition, the conductive paste of the present embodiment can also be used as a conductive paste for forming the back electrode 15 of a double-sided light-receiving crystalline solar cell.

[0188] Figure 1 The busbar electrode of the crystalline silicon solar cell shown includes Figure 2 The light incident side busbar electrode 20a shown in FIG. Figure 3 The back TAB electrode 15a is shown. A metal ribbon for interconnection with the surroundings covered with solder is welded to the light incident side bus electrode 20a and the back TAB electrode 15a. Through this metal ribbon, the current generated by the solar cell is taken out to the outside of the crystalline silicon solar cell unit. Figure 4 The double-sided light-receiving crystalline solar cell shown may include a light-incident-side bus bar electrode 20 a and a back-side TAB electrode having the same shape as that of the light-incident-side bus bar electrode 20 a .

[0189] The width of the bus electrode (the bus electrode 20a on the light incident side and the back TAB electrode 15a) can be the same width as the metal strip used for interconnection. In order to make the bus electrode low resistance, the width is preferably wide. On the other hand, in order to increase the incident area of ​​light on the light incident side surface, the width of the bus electrode 20a on the light incident side is preferably narrower. Therefore, the bus electrode width can be 0.05 to 5 mm, preferably 0.08 to 3 mm, more preferably 0.1 to 2 mm, and further preferably 0.15 to 1 mm. In addition, the number of bus electrodes can be determined according to the size of the crystalline silicon solar cell. The number of bus electrodes is arbitrary. Specifically, the number of bus electrodes can be set to 3 or 4, or more than that. The optimal number of bus electrodes can be determined by simulating the operation of the solar cell in a manner that maximizes the conversion efficiency of the crystalline silicon solar cell. It should be noted that, since the crystalline silicon solar cells are connected in series by the metal ribbon for interconnection, it is preferred that the number of the light incident side busbar electrode 20a and the back TAB electrode 15a are the same. For the same reason, the width of the light incident side busbar electrode 20a and the back TAB electrode 15a is preferably the same.

[0190] In order to increase the incident area of ​​light on the crystalline silicon solar cell, it is preferred that the area occupied by the light incident side surface electrode 20 in the light incident side surface is as small as possible. Therefore, it is preferred that the finger electrodes 20b on the light incident side surface have as thin a width as possible and have a smaller number. On the other hand, from the viewpoint of reducing electrical loss (ohmic loss), it is preferred that the finger electrodes 20b have a wide width and a large number. In addition, from the viewpoint of reducing the contact resistance between the finger electrodes 20b and the crystalline silicon substrate 1 (impurity diffusion layer 4), it is also preferred that the finger electrodes 20b have a wide width. Based on the above, in addition, the number of bus electrodes can be determined according to the size of the crystalline silicon solar cell and the width of the bus electrode. The optimal width and number of the finger electrodes 20b (the spacing between the finger electrodes 20b) can be determined by simulating the operation of the solar cell so as to maximize the conversion efficiency of the crystalline silicon solar cell. It should be noted that with regard to Figure 4 The width and number of the back finger electrodes 15 c of the back electrode 15 of the double-sided light-receiving crystalline silicon solar cell shown are determined in the same manner.

[0191] <Method for manufacturing solar cell>

[0192] Next, a method for manufacturing a solar cell according to the present embodiment will be described. The solar cell may be a crystalline silicon solar cell. In the following description, an example in which the solar cell is a crystalline silicon solar cell will be described.

[0193] The manufacturing method of the solar cell of the present embodiment includes the following steps: printing the above-mentioned conductive paste on the surface of the anti-reflection film 2 on the second conductive type semiconductor layer (impurity diffusion layer 4), drying and firing, thereby forming an electrode (light incident side surface electrode). The manufacturing method of the solar cell of the present embodiment is described in more detail below.

[0194] The method for manufacturing a solar cell of the present embodiment includes a step of preparing a semiconductor substrate of a first conductivity type (p-type or n-type) (e.g., a crystalline silicon substrate 1). As the semiconductor substrate of the first conductivity type, an n-type crystalline silicon substrate 1 is preferably used. Hereinafter, the case of manufacturing a crystalline silicon solar cell using an n-type crystalline silicon substrate 1 is described as an example.

[0195] It should be noted that, from the viewpoint of obtaining high conversion efficiency, the surface of the light incident side of the crystalline silicon substrate 1 preferably has a pyramid-shaped texture structure.

[0196] Next, the method for manufacturing a solar cell according to the present embodiment includes the step of forming a second conductivity type semiconductor layer on one surface of the first conductivity type semiconductor substrate.

[0197] The method for manufacturing a crystalline silicon solar cell of the present embodiment includes: a step of forming a semiconductor layer (impurity diffusion layer 4) of a second conductive type on one surface of the crystalline silicon substrate 1 prepared in the above step. When an n-type crystalline silicon substrate 1 is used as the crystalline silicon substrate 1, as the impurity diffusion layer 4, for example, a p-type impurity diffusion layer 4 obtained by diffusing B (boron) or the like as a p-type impurity can be formed. It should be noted that a crystalline silicon solar cell can also be manufactured using a p-type crystalline silicon substrate. In this case, as the impurity diffusion layer, an n-type impurity diffusion layer 4 obtained by diffusing P (phosphorus) or the like as an n-type impurity is formed.

[0198] When the impurity diffusion layer 4 is formed, the impurity diffusion layer 4 may be formed so that the sheet resistance thereof becomes 40 to 150 Ω / □ (square), preferably 45 to 120 Ω / □.

[0199] In addition, in the method for manufacturing a crystalline silicon solar cell of the present embodiment, the depth of the impurity diffusion layer 4 can be set to 0.3 μm to 1.0 μm. It should be noted that the depth of the impurity diffusion layer 4 refers to the depth from the surface of the impurity diffusion layer 4 to the pn junction. The depth of the pn junction can be set to the depth from the surface of the impurity diffusion layer 4 to the impurity concentration in the impurity diffusion layer 4 to the impurity concentration of the substrate.

[0200] The method for manufacturing a solar cell of the present embodiment includes a step of forming a back electrode 15 in a manner electrically connected to the other surface of a semiconductor substrate of the first conductivity type (n-type crystalline silicon substrate). It should be noted that the back electrode 15 may be formed before or after the light incident side surface electrode 20 is formed. In addition, the firing for forming the back electrode 15 may be performed simultaneously with the firing for forming the light incident side surface electrode 20 or may be performed separately.

[0201] Specifically, in the method for manufacturing a crystalline silicon solar cell according to the present embodiment, a conductive paste is printed on the other surface (back surface) of the crystalline silicon substrate 1 and fired to form the back surface electrode 15 .

[0202] It should be noted that in manufacturing Figure 4 In the case of a double-sided light-receiving crystalline solar cell as shown, a second impurity diffusion layer 16 can be formed. On the other hand, by forming the back electrode 15 using the conductive paste (conductive composition) of this embodiment and performing a laser treatment process, a low-resistance conductive portion can be formed between the back electrode 15 and the crystalline silicon substrate 1. Therefore, in the case of a double-sided light-receiving crystalline solar cell, it is preferable to form the back electrode 15 using the conductive paste of this embodiment. In this case, the back electrode 15 is a sintered body of the conductive paste of this embodiment.

[0203] Next, the method for manufacturing a solar cell of the present embodiment includes the step of forming a passivation film in contact with the surface of the second conductivity type semiconductor layer (impurity diffusion layer 4 ). The passivation film may be the antireflection film 2 .

[0204] Specifically, regarding the manufacturing method of the crystalline silicon solar cell of the present embodiment, an anti-reflection film 2 having the function of a passivation film is formed on the surface of the impurity diffusion layer 4 formed by the above-mentioned process. As the anti-reflection film 2, a silicon nitride film (SiN film) can be formed. In the case of using a silicon nitride film as the anti-reflection film 2, the layer of the silicon nitride film also has the function of a passivation film on the surface of the light incident side. Therefore, in the case of using a silicon nitride film as the anti-reflection film 2, a high-performance crystalline silicon solar cell can be obtained. In addition, by making the anti-reflection film 2 a silicon nitride film, it is possible to exert an anti-reflection function on the incident light. The silicon nitride film can be formed by a PECVD (Plasma Enhanced Chemical Vapor Deposition) method or the like.

[0205] The manufacturing method of the solar cell of the present embodiment includes a step of forming a light incident side surface electrode 20 on at least a portion of the surface of the passivation film (anti-reflection film 2). In the manufacturing method of the present embodiment, the above-mentioned conductive paste is used to form the light incident side surface electrode 20. Therefore, the light incident side surface electrode 20 is a sintered body of the above-mentioned conductive paste.

[0206] In the manufacturing method of the crystalline silicon solar cell of this embodiment, the light incident side surface electrode 20 is formed by printing the conductive paste on the surface of the anti-reflection film 2 and firing. It should be noted that when firing to form the light incident side surface electrode 20, firing to form the back electrode 15 can be performed simultaneously.

[0207] Specifically, first, the pattern of the light incident side surface electrode 20 printed using the conductive paste of the present embodiment is dried at a temperature of about 100 to 150° C. for several minutes (e.g., 0.5 to 5 minutes). It should be noted that at this time, the light incident side bus electrode 20a and the light incident side finger electrode 20b of the light incident side surface electrode 20 can be formed using the conductive paste of the present embodiment.

[0208] After the pattern of the light incident side surface electrode 20 is printed and dried, the conductive paste for forming the back electrode 15 is printed and dried. The conductive paste of this embodiment can be preferably used to form the electrodes (the light incident side surface electrode 20 and the back electrode 15 according to the situation) of solar cells such as crystalline silicon solar cells.

[0209] Then, a sintering furnace such as a tubular furnace is used to sinter the material obtained by drying the printed conductive paste in the atmosphere under prescribed sintering conditions. As sintering conditions, the sintering atmosphere is in the atmosphere, and the sintering temperature is 500 to 1000°C, more preferably 600 to 1000°C, further preferably 500 to 900°C, and particularly preferably 700 to 900°C. Firing is preferably carried out in a short time, and the temperature distribution (temperature-time curve) during sintering is preferably peak-shaped. For example, taking the above-mentioned temperature as the peak temperature, the time of entering and exiting the sintering furnace is preferably 10 to 100 seconds, more preferably 20 to 80 seconds for sintering, and further preferably 40 to 60 seconds for sintering.

[0210] During firing, it is preferred to simultaneously fire the conductive pastes for forming the light incident side surface electrode 20 and the back electrode 15, and simultaneously form both electrodes. In this way, by printing a predetermined conductive paste on the light incident side surface and the back surface, and firing them simultaneously, firing for forming electrodes can be performed only once. Therefore, a crystalline silicon solar cell can be manufactured at a lower cost.

[0211] The manufacturing method of the solar cell of the present embodiment includes the step of performing the above-mentioned laser treatment process. That is, the manufacturing method of the solar cell of the present embodiment includes: applying a voltage between the back electrode 15 and the light incident side surface electrode 20, while irradiating the light incident side surface of the solar cell with light from a point light source (for example, laser), so that a current in a direction opposite to the forward direction flows between the second conductive type semiconductor layer (p-type impurity diffusion layer 4) and the first conductive type semiconductor substrate (n-type crystalline silicon substrate 1). Through the laser treatment process, good electrical conduction between the light incident side surface electrode 20 and the impurity diffusion layer 4 can be achieved.

[0212] As described above, the crystalline silicon solar cell of this embodiment can be manufactured.

[0213] The crystalline silicon solar cell of the present embodiment obtained as described above is electrically connected using a metal ribbon for interconnection, and is laminated using a glass plate, a sealing material, a protective sheet, etc., thereby obtaining a solar cell module. As the metal ribbon for interconnection, a metal ribbon (e.g., a ribbon made of copper) covered around with solder can be used. As the solder, a solder with tin as the main component can be used, specifically, a leaded solder containing lead and a lead-free solder that can be obtained on the market can be used.

[0214] In the crystalline silicon solar cell of the present embodiment, a high-performance crystalline silicon solar cell can be obtained by forming a predetermined electrode of the solar cell using the conductive paste of the present embodiment and performing a laser processing process.

[0215] [Example]

[0216] Hereinafter, the present embodiment will be specifically described with reference to Examples, but the present invention is not limited to these Examples.

[0217] In the examples and comparative examples, a measurement substrate simulating a single crystal silicon solar cell is used to evaluate the degree of degradation of the passivation film based on the photoluminescence imaging method (PL method), as well as the contact resistance and resistivity of the formed electrode, thereby evaluating the performance of the conductive paste of the examples and comparative examples of the present embodiment.

[0218] <Materials and preparation ratios of conductive paste>

[0219] The compositions of the conductive pastes of Examples 1 to 14 and Comparative Examples 1 to 4 are shown in Tables 1 to 3. The compositions shown in Tables 1 to 3 and the compositions of the following components are expressed as parts by weight of each component based on 100 parts by weight of the (A) silver particles. The components contained in the conductive paste are as follows.

[0220] (A) Silver particles

[0221] Table 4 shows the product number, manufacturing company, shape, average particle size (D50), TAP density and BET specific surface area of ​​the silver particles A1 and A2 used in the conductive paste of the embodiment and the comparative example. Tables 1 to 3 show the compounding amounts of the silver particles A1 and A2 in the conductive paste of the embodiment and the comparative example. It should be noted that the average particle size (D50) is obtained by measuring the particle size distribution using the Microtrac method (laser diffraction scattering method) and obtaining the value of the median particle size (D50) based on the results of the particle size distribution measurement. The same is true for the average particle size (D50) of other components. In addition, the BET specific surface area is measured using a fully automatic specific surface area measuring device Macsoeb (manufactured by MOUNTEC). The BET specific surface area is measured as follows: pre-dry at 100°C, pass nitrogen for 10 minutes, and then measure by the BET single point method using nitrogen adsorption.

[0222] (B) Organic carrier

[0223] As the organic vehicle, an organic binder and a solvent were used. As the organic binder, ethyl cellulose (0.4 parts by weight) having an ethoxy content of 48 to 49.5% by weight was used. As the solvent, diethylene glycol monobutyl ether acetate (butyl carbitol acetate) (3 parts by weight) was used.

[0224] (C) Glass Frit

[0225] The composition, basicity, and glass transition temperature of glass frits A to G used in the conductive pastes of Examples and Comparative Examples are shown in Table 5. The average particle size (D50) of glass frits A to G is 2 μm. Tables 1 to 3 show the type (any one of A to G) and content G (parts by weight) of the (C) glass frits of the conductive pastes of Examples and Comparative Examples.

[0226] The glass transition temperatures of glass frits A to G were measured. The measured values ​​of the glass transition temperatures of glass frits A to G are shown in Table 5. The glass transition temperature of the glass frit was measured as follows. That is, about 50 mg of glass frits A to G were placed in a platinum pool as a sample, and alumina powder was used as a standard sample. In an air atmosphere, a differential thermal analyzer (TG-8120 manufactured by Rigaku Co., Ltd.) was used to increase the temperature from room temperature to 800°C at a heating rate of 20°C / min to obtain a DTA curve. The starting point (extrapolated point) of the first endothermic of the DTA curve was taken as the glass transition temperature.

[0227] Glass frits A to G are manufactured as follows. That is, first, the powders of the oxides that become the raw materials are measured, mixed, and put into a crucible. The crucible is placed in a heated oven, and the contents of the crucible are heated to the melting temperature (Melttemperature), and the raw materials are maintained at the melting temperature until they are fully melted. Next, the crucible is taken out of the oven and the molten contents are uniformly stirred. Next, the contents of the crucible are quenched at room temperature using a stainless steel double roller to obtain a plate-shaped glass. Finally, the plate-shaped glass is evenly dispersed while being crushed in a mortar, and sieved with a mesh sieve, thereby obtaining a glass frit with the desired particle size. The material that passes through a 100-mesh sieve and remains on a 200-mesh sieve is sieved out, thereby obtaining a glass frit with an average particle size (D50) of 149 μm. By further crushing the glass frit, a glass frit with an average particle size (D50) of 2 μm can be obtained.

[0228] (D) Aluminum particles

[0229] The product number, manufacturer, shape and average particle diameter (D50) of aluminum particles D1 and D2 used in the conductive pastes of Examples and Comparative Examples are shown in Table 6. The blending amounts (parts by weight) of aluminum particles D1 and D2 in the conductive pastes of Examples and Comparative Examples are shown in Tables 1 to 3.

[0230] Next, the materials having the weight ratios shown in Tables 1 to 3 were mixed with a planetary mixer, and further dispersed with a three-roll mill to form a paste, thereby preparing conductive pastes of Examples and Comparative Examples.

[0231] <Evaluation of the reactivity of conductive paste to passivation film by PL method>

[0232] The reactivity of the conductive paste to the passivation film is evaluated by the photoluminescence imaging method (referred to as the "PL method"). The PL method can evaluate the reactivity of the conductive paste to the passivation film in a non-destructive and non-contact manner in a short time. Specifically, the PL method is a method of irradiating a sample with light having an energy greater than the bandgap width to make it emit light, and evaluating the state of defects in the crystal and surface / interface defects based on the state of its light emission. In the case where the sample has defects in the single crystal silicon substrate and surface / interface defects, the defects act as recombination centers for electron-hole pairs generated by the irradiation of light, and the band edge emission intensity based on photoluminescence decreases accordingly. That is, when the passivation film is eroded by the printed / fired electrode and a surface defect is formed at the interface between the passivation film and the single crystal silicon substrate (i.e., the surface of the single crystal silicon substrate), the photoluminescence intensity of the portion where the surface defect is formed (i.e., the portion formed on the electrode of the sample) decreases. The reactivity of the prototype conductive paste with the passivation film can be evaluated based on the intensity of the photoluminescence.

[0233] The method for prototyping a substrate for evaluation by the PL method is as follows.

[0234] An n-type single crystal silicon substrate (substrate thickness: 200 μm) was used as the substrate.

[0235] First, a silicon oxide layer of about 20 μm was formed on the substrate by dry oxidation, and then etching was performed with a solution containing hydrogen fluoride, pure water and ammonium fluoride to remove damage on the substrate surface. In addition, heavy metal cleaning was performed with an aqueous solution containing hydrochloric acid and hydrogen peroxide.

[0236] Next, a texture structure (convex and concave shape) is formed on both sides of the substrate by wet etching. Specifically, a pyramid-shaped texture structure is formed on both sides (the light incident side surface and the back side) by wet etching (sodium hydroxide aqueous solution). Then, it is cleaned with an aqueous solution containing hydrochloric acid and hydrogen peroxide. Next, boron is injected into one surface of the above-mentioned substrate having a texture structure (the light incident side surface) to form a p-type diffusion layer at a depth of about 0.5μm. The sheet resistance of the p-type diffusion layer is 60Ω / □. In addition, phosphorus is injected into the other surface of the above-mentioned substrate having a texture structure (the back side) to form an n-type diffusion layer at a depth of about 0.5μm. The sheet resistance of the n-type diffusion layer is 20Ω / □. The injection of boron and phosphorus is carried out simultaneously by thermal diffusion.

[0237] Next, after forming a thin oxide film layer of 1 to 2 nm on the surface of the substrate on which the p-type diffusion layer is formed (the surface on the light incident side) and the surface of the substrate on which the n-type diffusion layer is formed (the back side), a silicon nitride film is formed to a thickness of about 60 nm using silane gas and ammonia gas by plasma CVD. Specifically, a silicon nitride film (anti-reflection film 2) having a film thickness of about 70 nm is formed by glow discharge decomposition of a mixed gas of 1 Torr (133 Pa) of NH3 / SiH4=0.5 using plasma CVD.

[0238] The substrate obtained in this way was cut into a square of 25 mm×25 mm to prepare a substrate 1 .

[0239] Next, if Figure 8 As shown, a square electrode pattern 22 of 13 mm×13 mm is printed on the surface of the substrate 1 using a conductive paste for forming an electrode, and then dried.

[0240] The substrate 1 having the electrode pattern 22 printed on the surface with the conductive paste as described above was fired using a belt furnace (firing furnace) CDF7210 manufactured by Despatch Industries, Inc. at a peak temperature of 720° C. and a firing furnace entry and exit time of 50 seconds.

[0241] As described above, a substrate (sample) for PL measurement is prepared.

[0242] The measurement by the PL method was performed using a Photoluminescence Imaging System (Model LIS-R2) manufactured by BT Imaging Co., Ltd. Light from an excitation light source (wavelength 650 nm, output power 3 mW) was irradiated onto the back side of the substrate (the surface on the side where the electrode pattern of the light incident side surface electrode 20 was not formed), and an image of the light emission intensity of photoluminescence was obtained.

[0243] exist Fig. 9 and Fig.10 An image of the photoluminescence intensity measured by the PL method is shown in FIG.

[0244] exist Fig. 9 FIG. 2 shows an image of the photoluminescence intensity of a sample in which an electrode pattern 22 is formed using the conductive paste of Example 4, measured by the PL method. Fig. 9 It can be seen that the image of the portion where the electrode pattern 22 is formed is different from the image of the portion where the electrode pattern 22 is formed. Fig.10 This means that the decrease in the photoluminescence intensity of the portion where the electrode pattern of the light incident side surface electrode 20 is formed is suppressed. Fig. 9 In the case of the sample shown, it can be said that the passivation function of the passivation film is maintained by forming the electrode pattern of the light incident side surface electrode 20. Fig. 9 In the case of the sample using the conductive paste of Example 4 shown, it can be said that the surface defect density of the surface of the single crystal silicon substrate 1 did not increase.

[0245] On the other hand, Fig.10 In the preparation of the samples shown, the conductive paste of Comparative Example 1 was used to form the light incident side surface electrode 20. Fig.10 It can be seen that Fig. 9 Compared with the sample shown in FIG. 1 , the image of the portion where the electrode pattern of the light incident side surface electrode 20 is formed becomes darker. This means that the photoluminescence intensity of the portion where the electrode pattern of the light incident side surface electrode 20 is formed is reduced. Fig.10 In the case of the sample using the conductive paste of Comparative Example 1, it can be said that the passivation function of the passivation film is impaired by forming the electrode pattern of the light incident side surface electrode 20, and the surface defect density of the surface of the single crystal silicon substrate 1 increases.

[0246] Tables 1 to 3 show the measured values ​​(PL values) of the photoluminescence intensity of the embodiments and comparative examples. The PL value is the average value of the photoluminescence intensity near the electrode. It should be noted that the PL value is a numerical value that varies depending on the spectrum and intensity of the irradiated light from the light source for excitation, the optical system used for measurement, etc., and is a value of an arbitrary unit. When the conditions for measuring the PL value, such as the spectrum and intensity of the irradiated light, and the optical system used for measurement, are set to be the same, by comparing the PL values ​​of each sample, it can be said that the degree of recombination of carriers in each sample (the degree of degradation of the passivation function) can be evaluated. It can be said that the higher the PL value, the better the passivation function brought by the passivation film.

[0247] It should be noted that, for confirmation, the Fig. 9 and Fig.10 The cross section of the specimen is shown. Fig.11 The use of Fig. 9 A cross-sectional SEM photograph (magnification: 20,000 times) of a sample (corresponding to Example 4) in which the light incident side surface electrode 20 is formed under the same conditions using the same conductive paste as the sample shown. Fig.12 The use of Fig.10 A cross-sectional SEM photograph (magnification: 20,000 times) of a sample (corresponding to Comparative Example 1) in which the light incident side surface electrode 20 was formed under the same conditions using the same conductive paste as the sample shown. Fig.11 It can be seen that in the case of the sample with a high PL value, even after the light incident side surface electrode 20 is formed, the anti-reflection film 2 (passivation film) maintains a substantially original shape, and the anti-reflection film 2 (passivation film) is not corroded by the glass frit. Fig.12 It can be seen that in the case of the sample with a low PL value, the anti-reflection film 2 (passivation film) is corroded by the glass frit, and the anti-reflection film 2 (passivation film) is almost completely disappeared. That is, the conductive paste of Comparative Example 1 can be said to be a conductive paste that can burn through the passivation film. Fig.12 The portion described as "glass" in is a glass component derived from the glass frit contained in the conductive paste. As described above, the reactivity of the conductive paste with respect to the antireflection film 2 (passivation film) can be evaluated by measuring the PL value by the above-mentioned PL method.

[0248] According to Tables 1 to 3, the PL value of the sample obtained using the conductive paste (conductive composition) of Examples 1 to 14 of the present embodiment is 5522 (Example 2) or more. In contrast, the PL value of Comparative Example 1 is 4900, and the PL value of Comparative Example 2 is 4800, which is a low value. Therefore, in Comparative Examples 1 and 2, the passivation function brought by the passivation film is low compared to the examples of the present embodiment, so it can be said that the performance of the solar cell is reduced. In addition, this suggests that when the conductive paste of Comparative Examples 1 and 2 is used to form an electrode, the open circuit voltage (Voc) in the solar cell characteristics is reduced.

[0249] It should be noted that the cross section of the sample of Comparative Example 2 having a PL value of 4800 near the interface between the electrode and the silicon substrate was observed by SEM, and the result was the same as that of Comparative Example 1 having a PL value of 4900 (see Fig.12 ), in the sample of Comparative Example 2, it was confirmed that no anti-reflection film 2 (passivation film) remained. On the other hand, the cross section near the interface between the electrode and the silicon substrate of the sample of Example 2 with a PL value of 5522 was observed by SEM, and the result was the same as that of Example 4 (refer to Fig.11 ), it was confirmed that in the sample of Example 2, the anti-reflection film 2 (passivation film) remained between the electrode and the silicon substrate. Therefore, according to the evaluation results of the photoluminescence imaging method (PL method) used in the evaluation of Examples 1 to 14 and Comparative Examples 1 to 4, it is clear that when the PL value is 5000 or more, preferably when the PL value is 5500 or more, the anti-reflection film 2 (passivation film) remains between the electrode and the silicon substrate, and a high-performance (especially high Voc) solar cell can be expected.

[0250] It is noted that the PL value did not change significantly before and after the laser treatment process. This is believed to be because the laser treatment process is a process for locally forming a minute electrical conduction portion and does not affect most of the antireflection film 2 (passivation film).

[0251] <Measurement of contact resistance before laser treatment>

[0252] Similar to the sample used for measurement based on the PL method, a p-type impurity diffusion layer is formed on one surface of an n-type crystalline silicon substrate (substrate thickness: 200 μm), and further, a silicon nitride film (anti-reflection film 2 serving as a passivation film) having a thickness of approximately 60 nm is formed on the p-type impurity diffusion layer, thereby obtaining a substrate for measuring contact resistance.

[0253] The conductive pastes shown in Tables 1 to 3 were used as the conductive pastes for forming electrodes on the surface (light incident side surface) of the substrate on which the p-type diffusion layer was formed in the single crystal silicon solar cells of the examples and comparative examples.

[0254] The conductive paste was printed by screen printing on the antireflection film 2 of the substrate in a pattern including a 1.5 mm wide light incident side bus electrode 20 a and a 60 μm wide light incident side finger electrode 20 b so as to have a film thickness of about 20 μm, and then dried at 150° C. for about 1 minute.

[0255] As the back electrode 15 (the electrode on the surface where the n-type diffusion layer is formed), a commercially available Ag paste was printed by screen printing. It should be noted that the electrode pattern of the back electrode 15 is the same electrode pattern shape as the light incident side electrode 20. Then, it was dried at 150°C for about 60 seconds. The film thickness of the conductive paste for the back electrode 15 after drying was about 20μm. Then, using a belt furnace (firing furnace) CDF7210 manufactured by Despatch Industries, Inc., double-sided simultaneous firing was performed under the conditions of a peak temperature of 720°C and a firing furnace entry and exit time of 50 seconds. As described above, a single crystal silicon solar cell was produced.

[0256] like Figure 7 As shown in FIG. 1 , the solar cell unit thus obtained was cut into 15 mm×15 mm squares to obtain a sample for contact resistance measurement. Figure 7 As shown, on the light incident side surface of the cut solar cell (contact resistance measurement sample), light incident side finger electrodes 20b with a width of 60 μm and a length of 15.0 mm were arranged at intervals of 1.5 mm. The light incident side finger electrodes 20b were used as contact resistance measurement patterns. The contact resistance of the contact resistance measurement patterns of the examples and comparative examples before the laser treatment process was determined by the TLM method (Transfer length method) using GP 4TEST Pro manufactured by GPSolar.

[0257] As samples for contact resistance measurement, three samples were prepared under the same conditions, and the measured value was calculated as the average value of the three values.

[0258] <Measurement of contact resistance after laser treatment>

[0259] A single crystal silicon solar cell is prepared in the same manner as the measurement of contact resistance before the above laser treatment process, and the light incident side surface of the solar cell is subjected to the laser treatment process. That is, a negative voltage is applied to the back electrode 15 and a contact resistance formed on the light incident side surface is applied to the back electrode 15. Figure 2The light incident side electrodes 20 of the pattern shown are respectively applied with a positive voltage, while the light incident side surface of the solar cell is irradiated with laser light so that a current in the direction opposite to the positive direction flows between the p-type impurity diffusion layer 4 of the solar cell unit and the n-type crystalline silicon substrate 1. The applied voltage during the laser treatment process is 20V, and the irradiated laser intensity is 100W / cm 2 , the voltage application and laser irradiation time were set to 2 seconds.

[0260] like Figure 7 As shown, the solar cell obtained in this way was cut into squares of 15 mm×15 mm, and the contact resistance after the laser treatment process was determined by the same method as the contact resistance measurement before the laser treatment process.

[0261] First, the contact resistance before the laser treatment process is 450mΩ·cm 2 In the following cases, the electrode can be used as a solar cell electrode by laser processing. Similarly, when the contact resistance is 300Ω·cm 2 In the following cases, the material can be more preferably used as an electrode of a solar cell by performing a laser processing process.

[0262] Next, the contact resistance after the laser treatment process was set to 20 mΩ·cm 2 The following can be preferably used as the electrode 20 of the solar cell. Similarly, the contact resistance is 9 mΩ·cm 2 The following can be more preferably used as electrodes of solar cells.

[0263] As is clear from Tables 1 to 3, the contact resistance of the samples obtained using the conductive pastes (conductive compositions) of Examples 1 to 14 of the present embodiment before the laser treatment process was 440 mΩ·cm 2 (Example 1) or less. In contrast, the contact resistance of Comparative Example 3 is 640 mΩ·cm 2 The contact resistance of Comparative Example 4 is 804 mΩ·cm 2 In addition, the contact resistance of the samples obtained using the conductive pastes (conductive compositions) of Examples 1 to 14 of the present embodiment after the laser treatment process was 18 mΩ·cm 2 (Example 1) or less. In contrast, the contact resistance of Comparative Example 3 is 21 mΩ·cm 2 The contact resistance of Comparative Example 4 is 32 mΩ·cm 2 Therefore, in Comparative Examples 3 and 4, the contact resistance is high compared to the example of the present embodiment, so it can be said that the performance of the solar cell is reduced. That is, in the case of Comparative Examples 3 and 4, it can be said that it is not preferable to use it as an electrode of a solar cell.

[0264] [Measurement of resistivity]

[0265] The resistivity of the conductive film pattern for resistivity measurement obtained by firing the conductive paste of the example and the comparative example was measured.

[0266] The resistivity of the examples and comparative examples was measured according to the following procedure. That is, a silicon substrate with a width of 15 mm, a length of 15 mm, and a thickness of 180 μm was prepared. On this substrate, a 325-mesh stainless steel screen was used to print the following Figure 6 The pattern formed by the conductive paste is shown.

[0267] Next, the silicon substrate having the patterns of the embodiment and the comparative example printed on the surface thereof applied to the substrate was simultaneously fired on both sides using a belt furnace (firing furnace) CDF7210 manufactured by Despatch Industries, Inc. at a peak temperature of 720° C. and a firing furnace entry and exit time of 50 seconds. As described above, a sample for resistivity measurement was prepared.

[0268] The resistivity of the conductive film pattern of the sample for resistivity measurement obtained by sintering the conductive paste of the embodiment and the comparative example was measured. First, the resistance value was measured by the 4-terminal method using a multimeter 2001 manufactured by TOYO Corporation. The cross-sectional area of ​​the conductive film pattern was measured using a confocal microscope OPTELICS H1200 and a surface roughness shape measuring machine 1500SD2 manufactured by Lasertec. 50 locations within a range of 1.6 mm were measured and the average value was obtained. The resistivity was calculated using the cross-sectional area and the measured resistance value.

[0269] In addition, as a sample for resistivity measurement, four samples were prepared under the same conditions, and the measured value was calculated|required as the average value of four. The measurement results are shown in Tables 1-3.

[0270] As can be seen from Tables 1 to 3, the resistivity of the conductive film obtained using the conductive pastes (conductive compositions) of Examples 1 to 14 and Comparative Examples 1 to 4 of the present embodiment is 8 μΩ·cm (Examples 11 and 18) or less. Generally, if the resistivity is 15 μΩ·cm or less, it can be said that it is suitable for use as an electrode. Therefore, by using the conductive paste of the present embodiment, an electrode with a preferred resistivity can be obtained.

[0271] It should be noted that, as described above, when the conductive pastes of Comparative Examples 1 and 2 were used, there was a problem of low PL value. In addition, when the conductive pastes of Comparative Examples 3 and 4 were used, there was a problem of high contact resistance between the electrode and the impurity diffusion layer. Therefore, when the conductive pastes of Comparative Examples 1 to 4 were used, it was clear that a high-performance solar cell could not be manufactured.

[0272] In contrast, in the case of an electrode formed using the conductive paste of this embodiment, the PL value is sufficiently high, the contact resistance is low, and the resistivity is also low. Therefore, it can be said that a high-performance crystalline silicon solar cell can be obtained by using the conductive paste of this embodiment.

[0273] As described above, in the case of an electrode formed using the conductive paste of the present embodiment, it was confirmed that the contact resistance was reduced by performing a laser treatment process. When the contact resistance is low, the filling factor (FF) increases. In addition, according to the evaluation results based on the above-mentioned PL method, when the conductive paste of the present embodiment is used, the residual rate of the anti-reflection film 2 (passivation film) between the electrode 20 and the impurity diffusion layer 4 is high, so the recombination of carriers is suppressed to a low level. Therefore, when the conductive paste of the present embodiment is used, it can be said that the possibility of a decrease in the open circuit voltage (Voc) is low. Based on the above, it can be said that when an electrode is formed using the conductive paste of the present embodiment, a solar cell having the characteristic of being able to improve the filling factor (FF) without reducing the open circuit voltage (Voc) can be obtained.

[0274] exist Fig.13 , a SEM photograph (magnification: 20,000 times) obtained by observing the cross section of a solar cell after the laser treatment process produced under the same conditions as in Example 5 using a high-magnification scanning electron microscope (SEM). Fig.13 As shown, it can be understood that the impurity diffusion layer 4 (silicon emitter layer) in contact with the light incident side surface electrode of the solar cell manufactured under the same conditions as in Example 5 locally forms the AgSi alloy 30 (local conductive portion) as a tiny electrical conduction portion (local conductive portion). In the solar cell of this embodiment, the conductive paste of this embodiment is used to form the electrode (light incident side surface electrode 20), so it can be said that the local conductive portion can be formed in the impurity diffusion layer 4. Therefore, it can be said that by forming the electrode (light incident side surface electrode 20) using the conductive paste of this embodiment, a low contact resistance can be obtained between the electrode and the impurity diffusion layer 4 of the solar cell.

[0275] [Table 1]

[0276]

[0277] [Table 2]

[0278]

[0279] [Table 3]

[0280]

[0281] [Table 4]

[0282]

[0283] [Table 5]

[0284]

[0285] [Table 6]

[0286]

[0287] Description of Reference Numerals

[0288] 1: Crystalline silicon substrate

[0289] 2: Anti-reflection film (passivation film)

[0290] 4: Impurity diffusion layer

[0291] 14: Back passivation film

[0292] 15: Back electrode

[0293] 15a: Back TAB electrode (back bus electrode) 15b: Back electrode (back full surface electrode)

[0294] 15c: Back finger electrodes

[0295] 16: Second impurity diffusion layer 20: Light incident side surface electrode (surface electrode)

[0296] 20a: Bus electrode on the light incident side

[0297] 20b: Finger electrodes on the light incident side

[0298] 22: Electrode pattern

[0299] 30: AgSi alloy (local conductive part)

Claims

1. A conductive paste for forming an electrode of a solar cell, the conductive paste comprising: (A) conductive particles, (B) an organic carrier, and (C) glass frit, (C) Basicity B of the glass frit GF The product B of the content G of the glass frit (C) GF G is in the range of 0.25 to 1.45, and the content G of the (C) glass frit is the content of the (C) glass frit in the conductive paste in parts by weight when the content of the (A) conductive particles in the conductive paste is 100 parts by weight.

2. The conductive paste according to claim 1, wherein The (A) conductive particles include silver particles.

3. The conductive paste according to claim 1 or 2, wherein (B) The organic vehicle contains at least one selected from the group consisting of ethyl cellulose, rosin ester, acrylic resin, and organic solvent.

4. The conductive paste according to any one of claims 1 to 3, wherein (C) The content of PbO in the glass frit in mol% PbO The product C of the content G of the (C) glass material PbO ·G is in the range of 20 to 139.

5. The conductive paste according to any one of claims 1 to 4, wherein The content G of the (C) glass frit is 0.3 parts by weight to 4.0 parts by weight.

6. The conductive paste according to any one of claims 1 to 4, wherein The content G of the (C) glass frit is 0.5 parts by weight to 1.5 parts by weight.

7. The conductive paste according to any one of claims 1 to 6, wherein The glass transition temperature of the (C) glass frit is 300°C to 600°C.

8. The conductive paste according to any one of claims 1 to 7, wherein The (C) glass frit includes at least one selected from the group consisting of ZnO, V2O5, WO3 and Nb2O3.

9. The conductive paste according to any one of claims 1 to 8, wherein The conductive paste further contains (D) aluminum particles.

10. The conductive paste according to claim 9, wherein When the content of the (A) conductive particles in the conductive paste is 100 parts by weight, the content of the (D) aluminum particles in the conductive paste is 0.1 parts by weight to 2.0 parts by weight.

11. The conductive paste according to any one of claims 1 to 10, which is a conductive paste for forming an electrode of a solar cell. Solar cells contain: a semiconductor substrate of a first conductivity type; a second conductivity type semiconductor layer disposed on one surface of the first conductivity type semiconductor substrate; a back electrode configured to be electrically connected to the other surface of the semiconductor substrate of the first conductivity type; a passivation film arranged to be in contact with a surface of the second conductivity type semiconductor layer; as well as a light incident side surface electrode, which is arranged on at least a portion of the surface of the passivation film, The light incident side surface electrode is the light incident side surface electrode that has been processed as follows: while applying a voltage between the back electrode and the light incident side surface electrode, light from a point light source is irradiated onto the light incident side surface of the solar cell so that current flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate in a direction opposite to the forward direction, The conductive paste is a conductive paste for forming the light incident side surface electrode.

12. A solar cell comprising: a semiconductor substrate of a first conductivity type; a second conductivity type semiconductor layer disposed on one surface of the first conductivity type semiconductor substrate; a back electrode configured to be electrically connected to the other surface of the semiconductor substrate of the first conductivity type; a passivation film arranged to be in contact with a surface of the second conductivity type semiconductor layer; as well as a light incident side surface electrode, which is arranged on at least a portion of the surface of the passivation film, The light incident side surface electrode is the light incident side surface electrode processed as follows: while applying a voltage between the back electrode and the light incident side surface electrode, light from a point light source is irradiated onto the light incident side surface of the solar cell so that a current in a direction opposite to a forward direction flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate, The light incident side surface electrode is a sintered body of the conductive paste according to any one of claims 1 to 10.

13. A solar cell comprising: a crystalline silicon substrate of a first conductivity type; a second conductivity type silicon emitter layer disposed on one surface of the first conductivity type crystalline silicon substrate; a back electrode arranged to be electrically connected to the other surface of the first conductivity type crystalline silicon substrate; a passivation film arranged to be in contact with a surface of the second conductivity type silicon emitter layer; as well as a light incident side surface electrode comprising silver, which is disposed on at least a portion of the surface of the passivation film, The second conductivity type silicon emitter layer has a local conductive portion that is in direct contact with the light incident side surface electrode without a passivation film therebetween. The local conductive portion includes an alloy of silver and silicon. The light incident side surface electrode is a sintered body of the conductive paste according to any one of claims 1 to 10.

14. A method for manufacturing a solar cell, comprising: A step of preparing a semiconductor substrate of a first conductivity type; forming a second conductivity type semiconductor layer on one surface of the first conductivity type semiconductor substrate; forming a back electrode in electrical connection with the other surface of the semiconductor substrate of the first conductivity type; forming a passivation film in contact with the surface of the second conductivity type semiconductor layer; a step of forming a light incident side surface electrode on at least a portion of the surface of the passivation film, and The step of applying a voltage between the back electrode and the light incident side surface electrode and irradiating the light incident side surface of the solar cell with light from a point light source so that a current in a direction opposite to the forward direction flows between the second conductive type semiconductor layer and the first conductive type semiconductor substrate, The light incident side surface electrode is a sintered body of the conductive paste according to any one of claims 1 to 10.

15. Use of the conductive paste according to any one of claims 1 to 11 for forming an electrode of a solar cell.

Citation Information

Patent Citations

  • Conductive composition, solar cell using the same, manufacturing method thereof, and solar cell module formed using the solar cell

    JP2009231826A

  • Method for improving the ohmic contact behavior between contact grid and emitter layer of silicon solar cells

    JP2019525471A

  • Method for improving ohmic contact behavior between contact grid and emitter layer of silicon solar cells

    JP2021513218A