Coating film for tablets and preparation method thereof
The coating film is prepared by combining cellulose acetate and green plasticizers, combined with heat stabilizers or antioxidants, which solves the problems of organic solvent pollution and thermal oxidation of cellulose acetate, and achieves high heat resistance and environmentally friendly production. Coated film.
Patent Information
- Application Number
- CN202411006135.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
AI Technical Summary
The use of organic solvents in the existing coating process leads to environmental pollution, and cellulose acetate is prone to thermal oxidation and degradation during hot melt processing, affecting the stability and aesthetics of the product.
Using a combination of cellulose acetate, green edible plasticizer, pore-generating agent, heat stabilizer or antioxidant, coated films are prepared through drying, granulating and casting processes, avoiding the use of organic solvents, and stabilizing by adding heat Agents or antioxidants improve the heat resistance and stability of the coating film.
It realizes low-temperature processing without modification of cellulose acetate, reduces environmental pollution, improves the thermal decomposition temperature and stability of the coating film, extends the shelf life, reduces yellowing, enhances toughness and aesthetics, and has environmentally friendly and pollution-free process.
Smart Images

Figure CN118986912A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a coating film for tablets and a preparation method thereof, belonging to the technical field of drug packaging. Background Art
[0002] As the third generation of preparations, oral sustained-release preparations have promoted the rapid development of the preparation industry as a whole. They can achieve constant or non-constant release of drugs according to specific requirements, effectively maintain a stable blood drug concentration, avoid the "peak and valley" phenomenon, improve drug safety and increase patient adaptability. Compared with sustained-release preparations, the blood drug concentration of controlled-release preparations is more stable and has less "peak and valley" fluctuations until the drug is completely absorbed.
[0003] Film coating is a pharmaceutical preparation technology, commonly used for coating pharmaceutical tablets or granules. Its main purpose is to protect the drug from the external environment, mask the taste of the drug, improve the stability and solubility of the drug, and delay the release rate of the drug.
[0004] The coating film contains water-soluble components (porogens) Diffusion principle: When the coating film contains water-soluble components, the components will form a concentration gradient inside and outside the film, causing the components to diffuse outward or inward. By regulating the properties and thickness of the coating film, the diffusion rate and degree of the water-soluble components can be controlled to achieve the effect of sustained or controlled release of the drug and achieve zero-order release at different rates.
[0005] Cellulose acetate is a thermoplastic resin obtained by esterifying cellulose with acetic acid or acetic anhydride under the action of a catalyst. It is a material with a wide range of applications among cellulose derivatives. Due to the different degrees of acetylation of the hydroxyl groups in cellulose acetate, the material can be subdivided into cellulose acetate, diacetate and triacetate. Cellulose acetate is white, and its appearance is affected by the production process conditions, and it is a solid in the form of particles, flakes or powder. Its performance is related to the specific structural differences of cellulose acetate, that is, it is related to the degree of acetylation of the hydroxyl groups. Cellulose acetate has the characteristics of good gloss, transparency, good toughness, high mechanical properties, and biodegradability. Cellulose diacetate has better toughness and strength, and its tensile strength is about twice that of cellulose diacetate. Cellulose acetate also has excellent biodegradability. Biodegradability can be controlled by its degree of substitution. Cellulose acetate with a DS of 3 cannot be biodegraded in the environment, while cellulose acetate with a DS of 2.5 degrades relatively slowly. Once the DS is less than 2.2, it can be degraded rapidly in the environment.
[0006] The increase of acetyl groups in cellulose acetate can improve its thermal stability. Due to the decrease of acetyl groups in diacetyl cellulose, its heat resistance is not as good as triacetyl cellulose. The melting temperature and decomposition temperature of diacetyl cellulose are similar. During the melt processing, cellulose acetate is prone to thermal oxidation degradation, resulting in yellowing of the product, poor mechanical properties, and harsh storage conditions.
[0007] At present, the coating process commonly used in industrial production is the spray coating process. Before spraying, the coating liquid must be prepared, and the prepared coating liquid is atomized into small droplets by a spray device, and then sprayed on the surface of the solid preparation. Under hot air or heating conditions, the solvent evaporates, and the polymer is wrapped on the surface of the solid preparation. Repeated spraying and drying complete the coating process. The problem is that the volatilization of organic solvents will cause environmental pollution. Summary of the invention
[0008] The present invention provides a coating film for tablets and a preparation method thereof, aiming to use green edible plasticizers to reduce pollutant emissions in industrial production processes, reduce resource consumption, and improve production efficiency, thereby achieving sustainable development and environmentally friendly production.
[0009] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0010] A coating film for tablets, comprising the following components by weight:
[0011] 80-90 parts of cellulose acetate, 20-30 parts of plasticizer;
[0012] Porogen;
[0013] The porogen accounts for 5-10% of the total weight of the cellulose acetate and the plasticizer;
[0014] Heat stabilizers or antioxidants may also be included.
[0015] Preferably, the coating film further comprises a heat stabilizer or an antioxidant;
[0016] The heat stabilizer or antioxidant accounts for 0.1-2% of the total weight of the cellulose acetate and the plasticizer.
[0017] Preferably, the plasticizer is one or more of citrates, polyvinyl alcohols, glycerol, and propylene glycol.
[0018] Furthermore, the plasticizer is a citrate ester.
[0019] Preferably, the porogen is one or more of mannitol, sucrose, polyethylene glycols, and sodium chloride.
[0020] Furthermore, the porogen is solid polyethylene glycol.
[0021] Preferably, the heat stabilizer is one or more of sucrose acetate isobutyrate, epoxidized soybean oil, and diisononyl cyclohexane-1,2-dicarboxylate.
[0022] Furthermore, the heat stabilizer is epoxidized soybean oil.
[0023] Preferably, the antioxidant is selected from one or more of didodecyl thiodipropionate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and dimethyltin isooctyl dithioacetate.
[0024] Furthermore, the antioxidant is one of didodecyl thiodipropionate and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
[0025] Preferably, the coating film for tablet medicine comprises the following components by weight: 90 parts of cellulose acetate, 30 parts of citrate esters, 12 parts of solid polyethylene glycol, and 1.5 parts of epoxidized soybean oil.
[0026] Preferably, the coating film for tablet medicine comprises the following components by weight: 90 parts of cellulose acetate, 30 parts of citrate, 12 parts of solid polyethylene glycol, and 1.5 parts of didodecyl thiodipropionate or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
[0027] Preferably, the cellulose acetate is cellulose diacetate, with an acetylation degree of 38-42% and an esterification degree of 220-270.
[0028] The method for preparing the above-mentioned tablet coating film comprises the following steps:
[0029] The cellulose acetate is mixed with a plasticizer, a heat stabilizer or an antioxidant in proportion, and the mixture is dried, granulated and cast to obtain the product.
[0030] Preferably, before preparing the coating film, the cellulose acetate needs to be subjected to a primary drying treatment.
[0031] Preferably, the first drying and drying after mixing are both carried out in a vacuum drying oven, wherein the drying power is 800-1000 W, the drying time is 24-48 h, the mixing is carried out in a mixer, and the mixing time is 15-45 min, the speed during mixing is 60-65 r / min, the drying time after mixing is 24-48 h, the granulation adopts a twin-screw particle size process, wherein the granulation temperature is 160-190° C., the particle size is 3-5 mm, the twin-screw speed is 100-300 rpm, and the casting adopts a single-screw casting process, wherein the casting temperature is 190-220° C., and the single-screw speed is 50-100 rpm.
[0032] Furthermore, the drying power is 1000W, the first drying time is 48h, the mixing is carried out in a mixer, and the mixing time is 30min, the rotation speed during mixing is 63r / min, the drying time after mixing is 48h, and the granulation adopts a twin-screw particle size process, wherein the granulation temperature is 180°C, the particle size is 3-5mm, the twin-screw speed is 150rpm, and the casting adopts a single-screw casting process, wherein the casting temperature is 200°C and the single-screw speed is 70rpm.
[0033] The beneficial effects of the present invention are:
[0034] (1) The present invention does not require modification of cellulose acetate. The purpose of adding plasticizer is to reduce the processing temperature of cellulose acetate so that it is easy to process by hot melt casting.
[0035] (2) The present invention does not use modifiers and cross-linking agents, and mainly adds heat stabilizers or antioxidants, the purpose of which is to delay the thermal oxidation or aging of the coating film in the present invention;
[0036] (3) The present invention uses a green and environmentally friendly plasticizer, namely, a citrate ester, which has a lower environmental impact, helps reduce the use of fossil fuels and reduce environmental pollution, and improves the safety and sustainability of the product; the green and environmentally friendly plasticizer can improve the tensile properties and increase the softness of cellulose acetate while reducing the processing temperature of cellulose acetate;
[0037] (4) Cellulose diacetate has good degradability and can be rapidly degraded in the natural environment, reducing environmental pollution and reducing dependence on resources;
[0038] (5) The present invention uses an environmentally friendly heat stabilizer, such as epoxidized soybean oil, to improve the stability of the product, or uses an antioxidant, such as pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and didodecyl thiodipropionate, to reduce the quality change caused by oxidation and high temperature and maintain the stability of the product; extend the shelf life of the product, prevent the product from decomposing or degrading during high-temperature processing or storage, maintain the quality stability of the product, improve the market competitiveness of the product without affecting the drug release, and the drug sustained release time is consistent;
[0039] (6) In the present invention, the addition of a heat stabilizer or an antioxidant can increase the thermal decomposition temperature of the coating film. After adding a heat stabilizer, the thermal decomposition temperature of the coating film is 7.14% higher than that of the coating film without adding a heat stabilizer. After adding an antioxidant, the thermal decomposition temperature of the coating film can reach up to 4.58% higher than that of the coating film without adding an antioxidant. Therefore, it can be shown that the coating film has high heat resistance.
[0040] (7) In the present invention, the addition of a heat stabilizer or an antioxidant can also reduce the yellowness index of the coating film. After adding the heat stabilizer, the yellowness index of the coating film is 60.51% lower than that of the coating film without adding the heat stabilizer; after adding the antioxidant, the yellowness index of the coating film is 26.34% lower than that of the coating film without adding the heat stabilizer. Therefore, it can be explained that the coating film has high heat resistance and high aesthetics; and will not affect the light transmittance of the coating film and the sustained release time of the drug.
[0041] (8) The addition of heat stabilizer in the present invention increases the melt index. Compared with the case where no heat stabilizer is added, the melt index increases by 28.36%, which indicates that the fluidity of the melt is improved after hot melting, making it easier to process into a film, but does not affect the film-forming property.
[0042] (9) The addition of thermal stabilizers and antioxidants can enhance the toughness of the coating film, which is beneficial to the subsequent coating process.
[0043] (10) When the coating film is used to coat tablets, no organic solvents such as acetone are required, and the entire process is green and environmentally friendly, wrinkle-free, and has high coating efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a test diagram of the processability of the coating film prepared in Example 1;
[0045] Figure 2 This is a test diagram of the processability of the coating film prepared in Example 2;
[0046] Figure 3 This is a test diagram of the processability of the coating film prepared in Example 3;
[0047] Figure 4 This is a test diagram of the processability of the coating film prepared in Comparative Example 1;
[0048] Figure 5 This is a processability test diagram of the coating film prepared in Comparative Example 2. DETAILED DESCRIPTION
[0049] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the present invention is further explained below with reference to specific diagrams and figures.
[0050] The following terms should also be explained in this invention:
[0051] Aging process: During the use of polymer materials or products, due to the influence of external factors such as heat, oxidation by oxidants, and light, the surface of the materials or products gradually changes, such as discoloration, hardening, brittleness, cracks, etc. At the same time, its characteristics and performance are seriously affected, mechanical properties decrease, air permeability increases, etc., causing them to be destroyed and lose their use value.
[0052] Antioxidants: A class of chemical substances that, when present in small amounts in a polymer system, can delay or inhibit the oxidation process of the polymer, thereby preventing the aging of the polymer and extending its service life. They are also called "antioxidants". In a broad sense, most weak reducing agents are antioxidants, but the appropriate ones are selected according to different industrial uses. Weak reducing agents with high chemical and physical stability or low toxicity can be cleverly used in formulations as antioxidants. Polymer materials such as plastics, synthetic fibers and rubber are prone to thermal oxidation degradation reactions. Adding antioxidants can maintain the excellent properties of polymer materials and extend their service life.
[0053] Commonly used plastic antioxidants are generally divided into five categories according to their molecular structure and mechanism of action: hindered phenols, phosphites, thiols, composites and hindered amines (HALS).
[0054] Commonly used heat stabilizers are mainly epoxidized oils and esters, which also have certain plasticizer functions.
[0055] The application of green and environmentally friendly plasticizers, heat stabilizers and antioxidants can reduce pollutant emissions in industrial production processes, reduce resource consumption, and improve production efficiency, thereby achieving sustainable development and environmentally friendly production.
[0056] The coating film in the present invention adopts the technology disclosed in the coating machine with application number ZL201810750341.9 and titled "Continuous body coating device and coating method for tablets". According to the above-mentioned disclosed technology, the coating film is first bubbled, and then the coating film is bubbled around the tablet, and then heat-sealed.
[0057] Example 1
[0058] A method for preparing a coating film for tablets comprises the following steps:
[0059] 90g of cellulose diacetate was placed in a blast drying oven for the first time and dried for 48h to remove water, 12g of solid polyethylene glycol was melted in a water bath at 85°C, and then 30g of citrate and 1.5g of epoxidized soybean oil were added and mixed for 30min (speed ratio 63), and then placed in a vacuum drying oven for heat treatment at 60°C for 48h, and then extruded into granules (3-5mm) at 180°C by a twin-screw extruder, and cast into a film at 200°C by a single-screw casting machine to obtain a coating film for tablet drugs (such as Figure 1 shown).
[0060] Example 2
[0061] This example is basically the same as Example 1, except that the epoxidized soybean oil in Example 1 is replaced with pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and the final product is as follows: Figure 2 The tablet drug shown is coated with a film.
[0062] Example 3
[0063] This example is basically the same as Example 1, except that the epoxy soybean oil in Example 1 is replaced with didodecyl thiodipropionate, and the final product is as follows Figure 3 The tablet drug shown is coated with a film.
[0064] Comparative Example 1
[0065] This comparative example is basically the same as Example 1, except that the stabilizer and antioxidant are not heated in this comparative example, and the final product is as follows Figure 4 The tablet drug shown is coated with a film.
[0066] Comparative Example 2
[0067] This comparative example is basically the same as Example 1, except that this comparative example contains only cellulose acetate and no other additives. Figure 5 The shape shown means that a coating film cannot be prepared.
[0068] test
[0069] The following tests were performed on Examples 1-3 and Comparative Examples 1 and 2, respectively. The test results are shown in Table 1.
[0070] Table 1
[0071]
[0072] (1) Adding a heat stabilizer or an antioxidant can increase the thermal decomposition temperature of the coating film. In Example 1, after adding a heat stabilizer, the thermal decomposition temperature of the coating film is higher than that of the coating film without adding a heat stabilizer by (251.43-234.68) / 234.68*100%=7.14%. In Example 3, after adding an antioxidant, the thermal decomposition temperature of the coating film is the highest than that of the coating film without adding an antioxidant, and can reach (245.43-234.68) / 234.68*100%=4.58%. Therefore, it can be shown that the coating film has high heat resistance.
[0073] (2) Adding a heat stabilizer or an antioxidant can also reduce the yellowness index of the coating film. In Example 1, after adding a heat stabilizer, the yellowness index of the coating film is lower than that of the coating film without adding a heat stabilizer by (31.4-12.4) / 31.4*100%=60.51%; after adding an antioxidant in Example 2, the yellowness index of the coating film is lower than that of the coating film without adding a heat stabilizer by (31.4-23.13) / 31.4*100%=26.34%. Therefore, it can be explained that the coating film has high heat resistance and high aesthetics; and will not affect the light transmittance and drug sustained release time of the coating film.
[0074] (3) Adding a heat stabilizer will increase the melt index. Compared with Comparative Example 1, Example 1 has a melt index increased by (43.59-33.96) / 33.96*100%=28.36%, which indicates that the fluidity of the melt after hot melting is improved and it is easy to process into a film, but it will not affect the film-forming property;
[0075] (4) The addition of heat stabilizer and antioxidant respectively enhances the toughness of the coating film, namely, judging from the tensile strength and elongation at break in Table 1, the enhanced toughness is beneficial to the subsequent coating process.
[0076] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A coating film for tablets, characterized in that: By weight, it includes the following components: 80-90 parts of cellulose acetate, 20-30 parts of plasticizer; Porogen; The porogen accounts for 5-10% of the total weight of the cellulose acetate and the plasticizer; Heat stabilizers or antioxidants may also be included.
2. The coating film according to claim 1, characterized in that The heat stabilizer or antioxidant accounts for 0.1-2% of the total weight of the cellulose acetate and the plasticizer.
3. A tablet coating film according to claim 1, characterized in that: The plasticizer is one or more of citrate esters, polyvinyl alcohols, glycerol, and propylene glycol; The porogen is one or more of mannitol, sucrose, polyethylene glycols, and sodium chloride; The heat stabilizer is one or more of sucrose acetate isobutyrate, epoxy soybean oil, and cyclohexane-1,2-dicarboxylic acid diisononyl ester; the antioxidant is one or more of didodecyl thiodipropionate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and dimethyltin dithioacetate.
4. A tablet coating film according to claim 3, characterized in that: The plasticizer is a citric acid ester; the porogen is solid polyethylene glycol; the heat stabilizer is epoxidized soybean oil; or the antioxidant is one of didodecyl thiodipropionate and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
5. A tablet coating film according to claim 4, characterized in that: The coating film for tablet medicine comprises the following components by weight: 90 parts of cellulose acetate, 30 parts of citrate esters, 12 parts of solid polyethylene glycol, and 1.5 parts of epoxidized soybean oil.
6. A tablet coating film according to claim 4, characterized in that: The coating film for tablet medicine comprises the following components by weight: 90 parts of cellulose acetate, 30 parts of citrate, 12 parts of solid polyethylene glycol, and 1.5 parts of didodecyl thiodipropionate or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate.
7. A tablet coating film according to claim 1, characterized in that: The cellulose acetate is cellulose diacetate, with an acetylation degree of 38-42% and an esterification degree of 220-270.
8. The method for preparing a tablet coating film according to any one of claims 1 to 7, characterized in that: The cellulose acetate is mixed with a plasticizer, a pore-forming agent, a heat stabilizer or an antioxidant in proportion, and the mixture is dried, granulated and cast to obtain the cellulose acetate.
9. The method for preparing a tablet coating film according to claim 8, characterized in that: The drying after mixing is carried out in a vacuum drying oven, wherein the drying power is 800-1000W, the drying time is 24-48h, the mixing is carried out in a mixer, and the mixing time is 15-45min, the rotation speed during mixing is 60-65r / min, the drying time after mixing is 24-48h, the granulation adopts a twin-screw particle size process, wherein the granulation temperature is 160-190°C, the particle size is 3-5mm, the twin-screw rotation speed is 100-300rpm, and the casting adopts a single-screw casting process, wherein the casting temperature is 190-220°C, and the single-screw rotation speed is 50-100rpm.
Citation Information
Patent Citations
Continuous fitted coating device and a coating method
CN108888514A
Cited By
Thermoplastic acetate fiber coating film as well as preparation and application thereof
CN121606704A