Carbon molecular sieve membrane as well as preparation method and application thereof
Through the high crosslinked molecular network structure of the carbon molecular sieve membrane, the problem that existing hydrogen separation technology is difficult to achieve ultra-pure hydrogen is solved, and efficient hydrogen separation and purification is achieved, and the hydrogen purity reaches 6N and above.
Patent Information
- Application Number
- CN202411019612.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
AI Technical Summary
Existing hydrogen separation technology is difficult to purify the mixed hydrogen gas to obtain ultrapure hydrogen.
Carbon molecular sieve membrane is prepared by carbonizing polymer crystalline materials, designing a high crosslinked molecular network, reducing the pore size of ultramicropores, improving the permeability of hydrogen, and mixing hydrogen through the carbon molecular sieve membrane as a permeation separation membrane The gas is separated and purified.
The purity of hydrogen is significantly improved, and it can be efficiently separated and purified in mixed hydrogen gases of different sources and volume concentrations. The hydrogen permeability coefficient is as high as 789GPU and the hydrogen purity can reach up to 6N.
Smart Images

Figure BDA0004967043170000081 
Figure BDA0004967043170000082 
Figure BDA0004967043170000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and in particular relates to a carbon molecular sieve membrane and a preparation method and application thereof. Background Art
[0002] Hydrogen energy is a clean secondary energy source and plays an important role in the future energy system. At present, the production of hydrogen includes technologies such as hydrogen production from fossil fuels, industrial by-product hydrogen, hydrogen production from water electrolysis, and hydrogen production from biomass. Due to different raw material compositions and processes, the purity and impurities of the hydrogen obtained are different, and all require further separation and purification. However, in many application fields, such as electronics, photovoltaics, and fuel cells, the demand for ultrapure hydrogen is becoming more and more urgent. Therefore, there is an urgent need for an efficient and feasible method to achieve one-step purification of ultrapure hydrogen. Summary of the invention
[0003] Technical problem solved by the present invention: It is difficult to purify mixed hydrogen gas to obtain ultra-pure hydrogen using the hydrogen separation technology in the prior art.
[0004] In view of the above technical problems, the present invention provides a carbon molecular sieve membrane and a preparation method and application thereof.
[0005] Specifically, the present invention provides the following technical solutions:
[0006] In a first aspect, the present invention provides a carbon molecular sieve membrane, wherein the carbon molecular sieve membrane is obtained by carbonizing a polymer material, wherein the polymer material is a high molecular crystalline material.
[0007] Preferably, the pore size of the carbon molecular sieve membrane is 0.35-0.8 nm.
[0008] More preferably, the pore size of the carbon molecular sieve membrane is 0.35 to 0.5 nm.
[0009] Preferably, the carbon molecular sieve membrane has a thickness of 0.1 to 30 μm.
[0010] More preferably, the carbon molecular sieve membrane has a thickness of 1 to 20 μm.
[0011] More preferably, the carbon molecular sieve membrane has a thickness of 1 to 10 μm.
[0012] In a second aspect, the present invention provides a method for preparing a carbon molecular sieve membrane, comprising the following steps:
[0013] (1) Preparation of polymer crystalline material: adding a phenolic compound, a carbonyl-containing compound and a non-cyclic amine compound to a solvent for reaction to obtain a polymer crystalline material;
[0014] (2) Preparation of a precursor: coating a polymer crystalline material on a carrier, aging the carrier, and using the aged polymer crystalline material as a precursor to obtain a carrier having a surface coated with the precursor;
[0015] (3) Preparation of carbon molecular sieve membrane: The precursor on the surface of the carrier is carbonized to obtain a carbon molecular sieve membrane.
[0016] Preferably, in step (1), the phenolic compound is selected from one or more of monophenolic compounds and substituted monophenolic compounds, diphenolic compounds and substituted diphenolic compounds, and triphenolic compounds and substituted triphenolic compounds.
[0017] Preferably, the substituent in the substituted monophenolic compound, substituted diphenolic compound or substituted triphenolic compound is selected from nitro, amino, methyl, ethyl, methoxy, carboxyl, formyl or formyloxy.
[0018] More preferably, the phenolic compound is selected from one or more of phenol, resorcinol, hydroquinone, pyrogallol, bisphenol A and 1-naphthol.
[0019] More preferably, the phenolic compound is selected from one or more of phenol, resorcinol, hydroquinone and 1-naphthol.
[0020] Preferably, in step (1), the carbonyl-containing compound is an aldehyde, an acid or a ketone.
[0021] Preferably, the aldehyde is selected from aromatic aldehydes and / or C 1-3 of fatty aldehydes.
[0022] More preferably, the aldehyde comprises one or more of formaldehyde, benzaldehyde, methyl, ethyl, hydroxyl, methoxy, acetylamino, dimethylamino or amino substituted benzaldehyde, salicylaldehyde and trimethylamino, nitro, cyano, sulfonic acid, aldehyde or carboxyl substituted salicylaldehyde.
[0023] Preferably, the acid is selected from one or more of isonicotinic acid, cyanuric acid, terephthalic acid and trimesic acid.
[0024] Preferably, the ketone is selected from one or more of cyclopropyl methyl ketone, methyl ethyl ketone, methyl heptenone, acetone and cyclohexanone.
[0025] Preferably, in step (1), the non-cyclic amine compound comprises one or more of aniline, methyl, ethyl, acetylamino or nitro-substituted aniline, N,N-methylenebisacrylamide, 4,4'-diaminodiphenylmethane and hexamethylenediamine.
[0026] Preferably, in step (1), the molar ratio of the phenolic compound to the carbonyl-containing compound is 1 to 4.5:1.
[0027] Preferably, the molar ratio of the phenolic compound to the carbonyl-containing compound is 1.5-4.5:1.
[0028] More preferably, the molar ratio of the phenolic compound to the carbonyl-containing compound is 1.5 to 4:1.
[0029] Preferably, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:1.5-20.
[0030] Preferably, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:3-20.
[0031] More preferably, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:4-20.
[0032] Preferably, in step (1), the solvent comprises one or more of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide.
[0033] Preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the acyclic amine compound is 1-35:5-30, wherein the unit of volume is mL and the unit of molar amount is mmol.
[0034] Preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the acyclic amine compound is 3-16:7-25, wherein the unit of volume is mL and the unit of molar amount is mmol.
[0035] More preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the acyclic amine compound is 3-10:8-23, wherein the unit of volume is mL and the unit of molar amount is mmol.
[0036] Preferably, in step (1), the volume ratio of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide is (0-6):(0-5):(0-5):(0-5):(0-4.5), wherein the volume ratios of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide are not 0 at the same time.
[0037] Preferably, in step (1), the reaction temperature is 25-100°C.
[0038] Preferably, in step (1), the reaction temperature is 45-70°C.
[0039] More preferably, in step (1), the reaction temperature is 60-70°C.
[0040] Preferably, in step (1), the reaction time is 6 to 30 hours.
[0041] Preferably, in step (1), the reaction time is 10 to 24 hours.
[0042] More preferably, in step (1), the reaction time is 13 to 24 hours.
[0043] Preferably, in step (1), the reaction speed is 400-700 rpm.
[0044] Preferably, in step (1), the reaction speed is 400-550 rpm.
[0045] Preferably, in step (2), the coating comprises the following steps: placing a reaction solution containing a polymer crystalline material on a carrier and aging it.
[0046] Preferably, in step (2), the aging temperature is 20 to 120° C., and the aging time is 0.5 to 24 h.
[0047] Preferably, the carrier is a porous material.
[0048] Preferably, the carrier is selected from one or more of anodized aluminum, porous glass, stainless steel mesh and phenolic resin.
[0049] Preferably, the coating is performed by a scraping method, which comprises the following steps: placing a reaction solution containing a polymer crystalline material on a carrier, then adjusting and fixing the height difference between a scraper and the carrier, scraping in the same direction, and aging.
[0050] Preferably, the height difference between the scraper and the carrier is 5-100 μm.
[0051] More preferably, the height difference between the scraper and the carrier is 10 to 50 μm.
[0052] Preferably, the aging temperature is 60-120°C; preferably, the aging temperature is 80-110°C; more preferably, the aging temperature is 80-100°C; and / or, the aging time is 0.5-10h; preferably, the aging time is 2-8h; and / or, the aging pressure is 0.1-0.5MPa.
[0053] Preferably, the coating is a casting method, which includes the following steps: adjusting the viscosity of the reaction solution containing the polymer crystalline material to 10-20 Pa·s, then casting it on a carrier and aging it; preferably, the aging temperature is 25-50°C, and / or the aging time is 12-24h.
[0054] Preferably, the coating is a spin coating method, which includes the following steps: adjusting the viscosity of the reaction liquid containing the polymer crystalline material to 10-20 Pa·s, then fixing the carrier on a rotating device, adjusting the rotation speed, so that the reaction liquid is dispersed on the carrier, and aging; preferably, the rotation speed is 10000-15000rpm; more preferably, the aging temperature is 50-90°C; and / or the aging time is 6-12h.
[0055] Preferably, in step (3), the carbonization conditions are: a heating rate of 0.1 to 5°C / min; a carbonization temperature of 600 to 1000°C, preferably, a carbonization temperature of 600 to 950°C; and / or a carbonization time of 2 to 22 hours, preferably, a carbonization time of 2 to 18 hours.
[0056] Preferably, the atmosphere of the carbonization process is an inert atmosphere, a hydrogen atmosphere or a nitrogen atmosphere.
[0057] More preferably, the inert atmosphere is argon.
[0058] Preferably, the carbon molecular sieve membrane is prepared by the carbon molecular sieve membrane preparation method.
[0059] In a third aspect, the present invention provides an application of the carbon molecular sieve membrane in separating or purifying hydrogen.
[0060] In a fourth aspect, the present invention provides a method for separating and purifying hydrogen from a hydrogen-mixed gas, comprising the following steps:
[0061] The carbon molecular sieve membrane is used as a permeation separation membrane, the mixed hydrogen gas is introduced into one side of the membrane assembly, and pressure is applied on the side of the mixed hydrogen gas to make the mixed hydrogen gas permeate through the carbon molecular sieve membrane and enter the other side of the membrane assembly to obtain hydrogen separation gas.
[0062] Preferably, the hydrogen-mixed gas is hydrogen and one or a combination of two or more of the following gases: methane, nitrogen, oxygen, carbon dioxide, ethane, ethylene, propane, propylene, butane, isobutane, butylene and isobutylene.
[0063] More preferably, the volume ratio of hydrogen in the hydrogen mixed gas is 1% to 80%.
[0064] More preferably, the pressure difference between the two sides of the membrane is 0.1-3 MPa.
[0065] Beneficial Effects of the Invention
[0066] (1) The present invention carbonizes a polymer crystalline material to prepare a carbon molecular sieve membrane. The present invention changes the inherent defects in the original polymer-derived carbon molecular sieve membrane by designing a highly cross-linked molecular network, reduces the pore size of the ultra-micropores, provides gas transmission and diffusion, and improves the permeation selectivity of hydrogen in different hydrogen-mixed gases.
[0067] (2) The carbon molecular sieve membrane of the present invention uses a polymer crystalline material as a precursor, has a simple preparation process, is easy to control the conditions, has good repeatability, reduces separation and process operation costs, and the prepared carbon molecular sieve membrane significantly improves the purity of the separated hydrogen.
[0068] (3) The carbon molecular sieve membrane of the present invention can be used for separation and purification of mixed hydrogen gases of different sources and volume concentrations. The hydrogen permeability coefficient is as high as 789GPU and the maximum hydrogen purity can reach 6N. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 This is an optical image of the polymer crystalline material in Example 3.
[0070] Figure 2 This is the infrared spectrum of the polymer crystalline material in Example 9.
[0071] Figure 3 This is the X-ray diffraction spectrum of the polymer crystalline material in Example 5.
[0072] Figure 4 Schematic diagram of membrane assembly and testing device.
[0073] Figure 5 This is the micropore distribution diagram of the carbon molecular sieve membrane in Example 3.
[0074] Figure 6 This is a scanning electron microscope image of the carbon molecular sieve membrane in Example 5.
[0075] Figure 7 This is an optical image of the carbon molecular sieve membrane in Example 7.
[0076] Figure 8 This is an optical image of the carbon molecular sieve membrane in Example 11.
[0077] Fig. 9 This is a diagram of the actual separation performance of the carbon molecular sieve membrane in Example 3. DETAILED DESCRIPTION
[0078] As mentioned above, the object of the present invention is to provide a carbon molecular sieve membrane and a preparation method and application thereof.
[0079] At present, the separation processes for hydrogen with a purity below 5N (purity of 99.9995%) mainly include adsorption, cryogenic separation, and metal hydride separation. These hydrogen separation technologies are difficult to purify mixed hydrogen to ultrapure hydrogen (6N and above) because it is difficult to remove ppm-level impurities. As an emerging separation material, carbon molecular sieve membranes have a unique pore structure and excellent separation performance, making them a promising candidate material for ultrapure hydrogen purification. Compared with traditional membrane separation technology, carbon molecular sieve membranes have the characteristics of high permeability and good selectivity. They can effectively separate impurities in hydrogen and further improve its purity. However, research on the use of carbon molecular sieve membranes for one-step purification of ultrapure hydrogen is still in its infancy. A Chinese patent (CN107376661A) discloses a palladium composite carbon membrane with a high hydrogen permeability. The results of the H2 / N2 single gas test show that the H2 permeability is 41.8m 3 ·m -2 ·h -1 , H2 purity is 99.98%, which has improved the separation efficiency of hydrogen to a certain extent, but has not yet achieved one-step purification of ultra-pure hydrogen. The journal Nat. Commun. 2021, 12, 268. discloses a carbon molecular sieve membrane for H2 / N2 separation, with an H2 permeability coefficient of 444.6 Barrer and an H2 purity of 99.992%. It is not yet possible to purify H2 to 6N or above in one step.
[0080] In the present invention, the carbon atom content of various carbon-hydrogen-containing structural parts is represented by prefixes with the minimum and maximum carbon atom numbers, i.e., the prefix C i~j The number of carbon atoms in the moiety is from an integer "i" to an integer "j" (including i and j). Thus, for example, C 1~3 The aliphatic aldehyde refers to an aliphatic aldehyde having 1 to 3 carbon atoms (including 1 and 3), such as formaldehyde, acetaldehyde, propionaldehyde or isopropionaldehyde.
[0081] The term "substituted" refers to the possibility of substitution at any available attachment point on the structure.
[0082] The term "polymer crystalline material" refers to a flaky polymer crystalline material prepared from phenolic compounds, carbonyl-containing compounds and non-cyclic amines through Mannich reaction and condensation reaction. The XRD spectrum of the polymer material of the present invention has a sharp diffraction peak, indicating that the present invention has successfully obtained a polymer crystalline material.
[0083] In the present invention, the first purpose is to provide a carbon molecular sieve membrane, which is obtained by carbonizing a polymer material, wherein the polymer material is a high molecular crystalline material, the pore size of the carbon molecular sieve membrane is 0.35 to 0.8 nm, and the thickness of the carbon molecular sieve membrane is 0.1 to 30 μm.
[0084] In the present invention, the second object is to provide a method for preparing a carbon molecular sieve membrane, comprising the following steps:
[0085] (1) Preparation of polymer crystalline material: adding a phenolic compound, a carbonyl-containing compound and a non-cyclic amine to a solvent for reaction, stirring at a speed of 400 to 700 rpm, a temperature of 25 to 100° C., and a time of 6 to 30 hours to obtain a polymer crystalline material; wherein the molar ratio of the phenolic compound, the carbonyl-containing compound and the non-cyclic amine compound is 1 to 4.5:1:1.5 to 20;
[0086] (2) Preparation of a precursor: coating a polymer crystalline material on a carrier, aging the material, and using the aged polymer crystalline material as a precursor to obtain a carrier having a surface coated with the precursor;
[0087] (3) Preparation of carbon molecular sieve membrane: The precursor is carbonized in an inert atmosphere, nitrogen atmosphere or hydrogen atmosphere, with a heating rate of 0.1 to 5°C / min, a temperature of 600 to 1000°C, and a time of 2 to 22 hours to obtain a carbon molecular sieve membrane.
[0088] The carbonyl-containing compound of the present invention refers to an aldehyde compound, a ketone compound or an acid compound containing a carbonyl group.
[0089] The non-cyclic amine compound of the present invention refers to an amine compound that does not contain a ring in the structural formula of the compound.
[0090] Preferably, the combination of the phenolic compound, the carbonyl-containing compound and the non-cyclic amine is selected from the combination of resorcinol, benzaldehyde and 4,4'-diaminodiphenylmethane, the combination of 1-naphthol, formaldehyde and hexamethylenediamine, the combination of hydroquinone, formaldehyde and 4,4'-diaminodiphenylmethane, the combination of resorcinol, benzaldehyde and hexamethylenediamine, and the combination of phenol, isonicotinic acid or N,N-methylenebisacrylamide.
[0091] In the present invention, the height difference between the scraper and the carrier is related to the thickness of the sieve layer in the carbon molecular sieve membrane after carbonization.
[0092] In the present invention, the carrier is a porous material with high strength and high porosity, wherein high strength refers to a compressive strength of 16-17 MPa, and high porosity refers to a porosity of 50%-80%. The porosity refers to the percentage of the pore volume of the material to the total volume of the material.
[0093] In the present invention, the purpose of the aging is to increase the cross-linking degree of the high molecular polymer, which is beneficial to obtain a carbon membrane with separation performance.
[0094] In the present invention, the pressure difference refers to the difference between the pressure on the mixed hydrogen gas side and the pressure on the argon gas side. ΔP = P1-P2. ΔP: pressure difference; P1: pressure on the mixed hydrogen gas side (retentate side); P2: pressure on the argon gas side (permeate side).
[0095] The third object of the present invention is to provide a method for separating and purifying hydrogen from a mixed hydrogen gas, comprising the following steps:
[0096] The carbon molecular sieve membrane is used to prepare a membrane assembly, and the ambient temperature around the membrane assembly is regulated; a mixed hydrogen gas is introduced into one side of the membrane assembly, and argon gas with the same volume fraction is introduced into the other side, and pressure is applied to one side of the mixed hydrogen gas to make the mixed hydrogen gas permeate through the carbon molecular sieve membrane to obtain hydrogen separation gas, and the purity of the obtained hydrogen can reach above 6N.
[0097] Unless otherwise specified, the various reagents / instruments used in the examples of the present invention are conventional commercially available products.
[0098] The mixed hydrogen gas permeation experiment used the Wicke-Kallenbach method. Figure 4 This is a schematic diagram of the test device. The mixed hydrogen gas is mixed by a mass flow controller (MFC, Sevenstar D07-7) and then enters the membrane pool. Part of the hydrogen passes through the carbon molecular sieve membrane into the permeate side to obtain hydrogen separation gas. The non-permeated gas in the mixed gas is retained by the carbon molecular sieve membrane on the retentate side. The gas composition on the permeate side is analyzed by an online 7900B gas chromatograph and mass spectrometer.
[0099] The gas permeation calculation formula is as follows:
[0100]
[0101] Among them, Q A is the permeation of gas A (in GPU), Δp is the transmembrane pressure (in bar), T is the temperature near the membrane (ambient temperature) (in °C), p0 is the local atmospheric pressure (in bar), p atm is the standard atmospheric pressure (in bar), dVA / dt is the flow rate of gas A on the permeate side (in cm 3 ·s -1 ). Wherein, gas A is hydrogen.
[0102] The calculation formula of H2 gas selectivity is as follows:
[0103]
[0104] Yi,perm and Yj,perm are the volume ratios of gases i and j on one side of the membrane (permeate side), Xi,feed and Xj,feed are the volume ratios of gases i and j on one side of the membrane (retentate side), i represents hydrogen, and j represents other gases except hydrogen in the mixed hydrogen gas.
[0105] The calculation formula of H2 purity is as follows:
[0106]
[0107] Among them, Q H2 is the hydrogen permeation rate, Q j It is the sum of the permeation of other gases in the mixed hydrogen gas.
[0108] The carbon molecular sieve membrane material and its preparation method and application described in the present invention are further illustrated by specific examples below.
[0109] Example 1
[0110] Resorcinol (1.5 mmol), formaldehyde (1 mmol) and 4,4'-diaminodiphenylmethane (20 mmol) in a molar ratio of 1.5:1:20 were added to 5 mL of methanol, the reaction stirring rate was 400 rpm, the reaction temperature was 45°C, the reaction time was 10 h, and a reaction solution containing a polymer crystalline material was obtained.
[0111] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 10 μm, and the scraper is coated in the same direction. Then, the substrate is aged for 8 hours at a normal pressure and a temperature of 80° C. to obtain a carrier with a precursor coated on the surface.
[0112] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 800°C at 0.1°C / min for 2h, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 15μm.
[0113] Example 2
[0114] Phenol (4.5 mmol), benzaldehyde (1.0 mmol) and hexamethylenediamine (1.5 mmol) in a molar ratio of 4.5:1:1.5 were added to 5 mL of ethanol. The reaction stirring rate was 420 rpm, the reaction temperature was 50°C, and the reaction time was 12 h to obtain a reaction solution containing a polymer crystalline material.
[0115] Then, the reaction solution containing the polymer crystalline material is placed on the porous glass by scraping. The height difference between the scraper and the porous glass is adjusted and fixed to 20 μm, and scraping is carried out in the same direction. Then, the substrate is aged for 2 hours at a normal pressure and a temperature of 81°C to obtain a carrier with the precursor scraped on the surface.
[0116] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 800°C at 1°C / min for 22 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 10μm.
[0117] Example 3
[0118] Resorcinol (3 mmol), benzaldehyde (1 mmol) and 4,4'-diaminodiphenylmethane (15 mmol) in a molar ratio of 3:1:15 were added to 4.5 mL of benzyl alcohol. The reaction stirring rate was 410 rpm, the reaction temperature was 60°C, and the reaction time was 13 h to obtain a reaction solution containing a polymer crystalline material. Figure 1 This is an optical image of the polymer crystalline material in the reaction solution. It can be seen from the image that the flake polymer material has been successfully synthesized. The flake polymer material has a length of about 14.17 μm and a width of about 4.91 μm.
[0119] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 30 μm, and scraped in the same direction. Then, the substrate is aged for 5 hours at a normal pressure and a temperature of 90° C. to obtain a carrier with a precursor scraped on the surface.
[0120] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 800°C at 1°C / min for 2h, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 1μm. Figure 5 This is the micropore distribution diagram of the carbon molecular sieve membrane in Example 3. The pore size of the carbon molecular sieve membrane is concentrated at 0.35 nm. Fig. 9 3 is a graph of the actual separation performance of the carbon molecular sieve membrane in Example 3. It can be seen from the graph that after the mixed gas of H2, N2 and CH4 is treated by the carbon molecular sieve membrane obtained in Example 3, hydrogen with a concentration of 6N can be obtained.
[0121] Example 4
[0122] 1-Naphthol (2 mmol), formaldehyde (1 mmol) and hexamethylenediamine (5 mmol) in a molar ratio of 2:1:5 were added to 4 mL of DMF. The reaction stirring rate was 450 rpm, the reaction temperature was 60°C, and the reaction time was 15 h to obtain a reaction solution containing a polymer crystalline material.
[0123] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the carrier is aged for 8 hours under normal pressure and temperature of 90° C. to obtain a carrier with a precursor scraped on the surface.
[0124] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 900°C at 1°C / min for 4 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 3μm.
[0125] Example 5
[0126] Resorcinol (1.5 mmol), benzaldehyde (1 mmol) and hexamethylenediamine (20 mmol) in a molar ratio of 1.5:1:20 were added to a mixed solvent of 5 mL of methanol, 1 mL of ethanol, 1 mL of deionized water and 3 mL of DMF. The reaction stirring rate was 460 rpm, the reaction temperature was 60°C, the reaction time was 24 h, and a reaction solution containing a polymer crystalline material was obtained. Figure 3 This is the X-ray diffraction spectrum of the polymer crystalline material in the reaction solution of Example 5. It can be seen from the figure that the polymer material has a sharp diffraction peak, which means that the obtained polymer material is a polymer crystalline material.
[0127] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 12 μm, and the scraper is coated in the same direction. Then, the substrate is aged for 8 hours at a normal pressure and a temperature of 80° C. to obtain a carrier with a precursor scraped on the surface.
[0128] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 950°C at 1°C / min for 5 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 5μm. Figure 6 This is a scanning electron microscope image of the carbon molecular sieve membrane in Example 5. It can be seen from the image that the surface of the carbon molecular sieve membrane is dense and has no defects over a large area.
[0129] Example 6
[0130] Bisphenol A (1.5 mmol), salicylaldehyde (1 mmol) and N,N-methylenebisacrylamide (13 mmol) in a molar ratio of 1.5:1:13 were added to a mixed solvent of 5 mL of methanol, 2 mL of ethanol and 3 mL of DMF. The reaction stirring rate was 500 rpm, the reaction temperature was 60°C, the reaction time was 24 h, and a reaction solution containing a polymer crystalline material was obtained.
[0131] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 35 μm, and scraped in the same direction. Then, the carrier is aged for 8 hours under normal pressure and temperature of 83°C to obtain a carrier with a precursor scraped on the surface.
[0132] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 1000°C at 5°C / min for 8 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 6μm.
[0133] Example 7
[0134] 1-Naphthol (2 mmol), isonicotinic acid (1 mmol) and hexamethylenediamine (12 mmol) in a molar ratio of 2:1:12 were added to a mixed solvent of 5 mL of methanol and 1 mL of DMF. The reaction stirring rate was 530 rpm, the reaction temperature was 60°C, and the reaction time was 24 h to obtain a reaction solution containing a polymer crystalline material.
[0135] Then, the reaction solution containing the polymer crystalline material is placed on the porous glass by scraping. The height difference between the scraper and the porous glass is adjusted and fixed to 34 μm, and scraping is carried out in the same direction. Then, the substrate is aged for 8 hours at a normal pressure and a temperature of 110° C. to obtain a carrier with the precursor scraped on the surface.
[0136] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 1000°C at 1°C / min for 9 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 13μm. Figure 7 This is an optical image of the carbon molecular sieve membrane in Example 7. It can be seen from the image that the surface of the obtained carbon molecular sieve membrane is smooth, but it still has defects and cannot obtain infinite separation selectivity.
[0137] Example 8
[0138] Hydroquinone (2.5 mmol), formaldehyde (1 mmol) and 4,4'-diaminodiphenylmethane (5.5 mmol) in a molar ratio of 2.5:1:5.5 were added to a mixed solvent of 5 mL of methanol, 3 mL of ethanol, 1 mL of deionized water and 1 mL of DMF. The reaction stirring rate was 510 rpm, the reaction temperature was 70°C, the reaction time was 24 h, and a reaction solution containing a polymer crystalline material was obtained.
[0139] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the carrier is aged for 8 hours under normal pressure and temperature of 82° C. to obtain a carrier with a precursor scraped on the surface.
[0140] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 800°C at 1°C / min for 10 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 10μm.
[0141] Example 9
[0142] Resorcinol (4 mmol), benzaldehyde (1 mmol) and hexamethylenediamine (4.5 mmol) in a molar ratio of 4:1:4.5 were added to a mixed solvent of 1 mL of benzyl alcohol, 1 mL of deionized water and 1 mL of DMF. The reaction stirring rate was 500 rpm, the reaction temperature was 60°C, and the reaction time was 24 h to obtain a reaction solution containing a polymer crystalline material. Figure 2 This is the infrared spectrum of the polymer crystalline material in the reaction solution of Example 9. It can be seen from the figure that C=O and C=N bonds are found in the infrared spectrum, indicating that the obtained flaky polymer material has undergone Mannich reaction and condensation reaction.
[0143] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the carrier is aged for 3 hours under normal pressure and temperature of 84°C to obtain a carrier with a precursor scraped on the surface.
[0144] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 900°C at 0.5°C / min for 12 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 8μm.
[0145] Example 10
[0146] Phenol (1.5 mmol), isonicotinic acid (1 mmol) and N,N-methylenebisacrylamide (9.5 mmol) in a molar ratio of 1.5:1:9.5 were added to a mixed solvent of 2 mL of ethanol and 3 mL of deionized water. The reaction stirring rate was 550 rpm, the reaction temperature was 65°C, and the reaction time was 20 h to obtain a reaction solution containing a polymer crystalline material.
[0147] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 34 μm, and scraped in the same direction. Then, the substrate is aged for 6 hours at a normal pressure and a temperature of 89° C. to obtain a carrier with a precursor scraped on the surface.
[0148] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 600°C at 1°C / min for 18 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 7μm.
[0149] Embodiment 11
[0150] Pyrogallol (1.5 mmol), benzaldehyde (1 mmol) and 4,4'-diaminodiphenylmethane (16.5 mmol) in a molar ratio of 1.5:1:16.5 were added to a mixed solvent of 1 mL of ethanol and 2 mL of DMF. The reaction stirring rate was 500 rpm, the reaction temperature was 50°C, and the reaction time was 21 h to obtain a reaction solution containing a polymer crystalline material.
[0151] Then, the reaction solution containing the polymer crystalline material is placed on the porous glass by scraping. The height difference between the scraper and the porous glass is adjusted and fixed to 36 μm, and scraping is carried out in the same direction. Then, the substrate is aged for 4 hours at a normal pressure and a temperature of 110° C. to obtain a carrier with the precursor scraped on the surface.
[0152] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 700°C at 3°C / min for 20 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 5μm. Figure 8 This is an optical photograph of the carbon molecular sieve membrane in Example 11. The carbon molecular sieve membrane obtained in Example 11 has a smooth surface, but still has defects and cannot obtain infinite separation selectivity.
[0153] Example 12
[0154] 1-Naphthol (1.5 mmol), isonicotinic acid (1 mmol) and hexamethylenediamine (20 mmol) in a molar ratio of 1.5:1:20 were added to a mixed solvent of 5 mL of methanol and 1 mL of ethanol. The reaction stirring rate was 450 rpm, the reaction temperature was 55°C, and the reaction time was 22 h to obtain a reaction solution containing a polymer crystalline material.
[0155] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 38 μm, and scraped in the same direction. Then, the substrate is aged for 4 hours at a normal pressure and a temperature of 80° C. to obtain a carrier with a precursor scraped on the surface.
[0156] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 1000°C at 0.5°C / min for 16 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 6μm.
[0157] Example 13
[0158] Resorcinol (4.5 mmol), salicylaldehyde (1 mmol) and N,N-methylenebisacrylamide (3.5 mmol) in a molar ratio of 4.5:1:3.5 were added to a mixed solvent of 5 mL of methanol, 2 mL of deionized water and 1 mL of DMF. The reaction stirring rate was 400 rpm, the reaction temperature was 65°C, the reaction time was 21 h, and a reaction solution containing a polymer crystalline material was obtained.
[0159] Then, the reaction solution containing the polymer crystalline material is placed on a stainless steel wire mesh by a scraper coating method. The height difference between the scraper and the stainless steel wire mesh is adjusted and fixed to 45 μm, and scraped in the same direction. Then, the reaction solution is aged for 4 hours at a normal pressure and a temperature of 110°C to obtain a carrier with a precursor scraped on the surface.
[0160] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 600°C at 1°C / min for 17h, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 5μm.
[0161] Embodiment 14
[0162] Phenol (4.5 mmol), benzaldehyde (1 mmol) and hexamethylenediamine (19.5 mmol) in a molar ratio of 4.5:1:19.5 were added to a mixed solvent of 3 mL of methanol, 1 mL of ethanol, 3 mL of deionized water and 1 mL of DMF. The reaction stirring rate was 420 rpm, the reaction temperature was 50°C, the reaction time was 23 h, and a reaction solution containing a polymer crystalline material was obtained.
[0163] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the substrate is aged for 5 hours at a normal pressure and a temperature of 89° C. to obtain a carrier with a precursor scraped on the surface.
[0164] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 800°C at 0.5°C / min for 15h, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 10μm.
[0165] Embodiment 15
[0166] Bisphenol A (1.5 mmol), isonicotinic acid (1 mmol) and hexamethylenediamine (5.5 mmol) in a molar ratio of 1.5:1:5.5 were added to a mixed solvent of 5 mL of methanol and 4 mL of DMF. The reaction stirring rate was 450 rpm, the reaction temperature was 65°C, and the reaction time was 24 h to obtain a reaction solution containing a polymer crystalline material.
[0167] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 10 μm, and scraped in the same direction. Then, the carrier is aged for 4 hours under normal pressure and temperature of 110°C to obtain a carrier with a precursor scraped on the surface.
[0168] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 700°C at 1°C / min for 20 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 12μm.
[0169] Example 16
[0170] 1-Naphthol (2.5 mmol), salicylaldehyde (1 mmol) and N,N-methylenebisacrylamide (16.5 mmol) in a molar ratio of 2.5:1:16.5 were added to a mixed solvent of 5 mL of methanol and 4.5 mL of deionized water. The reaction stirring rate was 550 rpm, the reaction temperature was 70°C, and the reaction time was 11 h to obtain a reaction solution containing a polymer crystalline material.
[0171] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 16 μm, and scraped in the same direction. Then, the substrate is aged for 6 hours at a normal pressure and a temperature of 90° C. to obtain a carrier with a precursor scraped on the surface.
[0172] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 1000°C at 0.3°C / min for 16 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 11μm.
[0173] Embodiment 17
[0174] Bisphenol A (1.5 mmol), cyclopropyl methyl ketone (1 mmol) and N,N-methylenebisacrylamide (15 mmol) in a molar ratio of 1.5:1:15 were added to a mixed solvent of 5 mL of methanol, 2.5 mL of ethanol, 4.5 mL of deionized water and 4 mL of DMF. The reaction stirring rate was 540 rpm, the reaction temperature was 60°C, the reaction time was 15 h, and a reaction solution containing a polymer crystalline material was obtained.
[0175] Then, the reaction solution containing the polymer crystalline material is placed on a stainless steel wire mesh by a scraper coating method. The height difference between the scraper and the stainless steel wire mesh is adjusted and fixed to 19 μm, and scraped in the same direction. Then, the reaction solution is aged for 6 hours at a normal pressure and a temperature of 90°C to obtain a carrier with a precursor scraped on the surface.
[0176] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 900°C at 5°C / min for 20 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 15μm.
[0177] Embodiment 18
[0178] Phenol (2 mmol), isonicotinic acid (1 mmol) and hexamethylenediamine (14 mmol) in a molar ratio of 2:1:14 were added to a mixed solvent of 2 mL of methanol and 2 mL of ethanol. The reaction stirring rate was 520 rpm, the reaction temperature was 65°C, and the reaction time was 16 h to obtain a reaction solution containing a polymer crystalline material.
[0179] Then, the reaction liquid containing the polymer crystalline material is placed on the molded phenolic resin by a scraper coating method. The height difference between the scraper and the molded phenolic resin is adjusted and fixed to 25 μm, and scraped in the same direction. Then, the carrier is aged for 4 hours under normal pressure and temperature of 110°C to obtain a carrier with a precursor scraped on the surface.
[0180] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: H2 gas atmosphere, heating from 25°C to 600°C at 5°C / min for 3h, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.35nm, and the thickness of the carbon molecular sieve membrane was 15μm.
[0181] Embodiment 19
[0182] Phenol (4.5 mmol) and benzaldehyde (1 mmol) in a molar ratio of 4.5:1 were added to 4.5 mL of benzyl alcohol. The reaction stirring rate was 550 rpm, the reaction temperature was 70° C., and the reaction time was 23 h to obtain a reaction solution containing a polymer crystalline material.
[0183] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the substrate is aged for 8 hours at a normal pressure and a temperature of 110° C. to obtain a carrier with a precursor scraped on the surface.
[0184] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 1000°C at 1°C / min for 3 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 20μm.
[0185] Embodiment 20
[0186] Phenol (4.5 mmol), benzaldehyde (1 mmol) and 1,3-cyclohexanediamine (15 mmol) in a molar ratio of 4.5:1:15 were added to 4.5 mL of benzyl alcohol. The reaction stirring rate was 550 rpm, the reaction temperature was 70°C, and the reaction time was 23 h to obtain a reaction solution containing a polymer crystalline material.
[0187] Then, the reaction solution containing the polymer crystalline material is placed on the anodized aluminum by a scraper coating method. The height difference between the scraper and the anodized aluminum is adjusted and fixed to 50 μm, and scraped in the same direction. Then, the substrate is aged for 8 hours at a normal pressure and a temperature of 110° C. to obtain a carrier with a precursor scraped on the surface.
[0188] Finally, the precursor coated on the surface of the carrier was carbonized to obtain a carbon molecular sieve membrane. The carbonization conditions were: Ar gas atmosphere, heating from 25°C to 1000°C at 1°C / min for 3 hours, and cooling. The pore size of the obtained carbon molecular sieve membrane was 0.5nm, and the thickness of the carbon molecular sieve membrane was 15μm.
[0189] Application Examples
[0190] The carbon molecular sieve membrane obtained in the example is used to purify the hydrogen component. Figure 4 It is a schematic diagram of the membrane assembly and the test method. The "sieve layer" in the figure refers to the carbon molecular sieve membrane described in the present invention; the "substrate" refers to the carrier described in the present invention, such as anodized aluminum, porous glass, stainless steel wire mesh or molded phenolic resin, etc.; the "permeate side" refers to the side where the material passes through the membrane during the membrane separation of mixed gases; the "residue side" refers to the side opposite to the permeate side, that is, the side where the material does not pass through the membrane and is retained. The carbon molecular sieve membrane is placed horizontally, and the mixed gas flows along Figure 4 The direction of the middle arrow passes through the carbon molecular sieve membrane from the retentate side to the permeate tester, wherein hydrogen passes through the carbon molecular sieve membrane to the permeate side, and a mass spectrometer and a chromatograph are used to detect the purity of hydrogen in the permeate side gas.
[0191] The application process is as follows: the ambient temperature of the membrane assembly carrying the carbon molecular sieve membrane is controlled at -30 to 200°C, the mixed hydrogen gas component is introduced into one side of the membrane assembly (the retentate side), and the argon gas with the same volume fraction is introduced into the other side (the permeate side), with a pressure difference of 0.1-3MPa as the driving force (by adjusting the back pressure valve on the inlet side to change the transmembrane pressure difference), the mixed gas permeates through the carbon molecular sieve membrane, and after being diluted with argon gas (purge gas), the components are analyzed by chromatography to calculate the purity of the hydrogen. Among them, the volume percentage of the hydrogen component in the mixed hydrogen gas is 1-80%. The details are shown in Table 2.
[0192] Table 2 Separation performance evaluation results of carbon molecular sieve membranes prepared in various embodiments
[0193]
[0194]
[0195] Note: The unit of hydrogen permeation is GPU, 1GPU = 3.35×10 -10 mol·m -2 ·s -1 ·Pa -1; Hydrogen permeation is a direct indicator of the processing capacity of carbon molecular sieve membranes; high permeation means large processing capacity, indicating that carbon molecular sieve membranes have the potential for industrial application; hydrogen permeation is related to the type of carrier, the proportion of hydrogen in the mixed gas, the transmembrane pressure difference and the test temperature. The larger the H2 selectivity value, the higher the H2 purity, indicating a better separation effect.
[0196] It can be seen from Table 2 that the carbon molecular sieve membranes prepared in Examples 1-20 can separate and purify hydrogen in mixed hydrogen gas in one step, and the purity of the obtained hydrogen is above 99%. Among them, the carbon molecular sieve membranes prepared in Examples 3-5 and Examples 8-10 can separate and purify the hydrogen in the mixed hydrogen gas to 6N, i.e., 99.9999%.
[0197] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.
Claims
1. A carbon molecular sieve membrane, It is characterized in that The carbon molecular sieve membrane is obtained by carbonizing a polymer material, and the polymer material is a high molecular crystalline material.
2. The carbon molecular sieve membrane according to claim 1, It is characterized in that The polymer crystalline material is aged and coated on a carrier as a precursor, and the precursor is carbonized to obtain a carbon molecular sieve membrane.
3. The carbon molecular sieve membrane according to claim 1 or 2, It is characterized in that The polymer crystalline material is obtained by adding a phenol compound, a carbonyl-containing compound and a non-cyclic amine compound into a solvent for reaction.
4. The carbon molecular sieve membrane according to any one of claims 1 to 3, It is characterized in that The pore size of the carbon molecular sieve membrane is 0.35 to 0.8 nm; preferably, the pore size of the carbon molecular sieve membrane is 0.35 to 0.5 nm; And / or, the carbon molecular sieve membrane has a thickness of 0.1 to 30 μm; preferably, the carbon molecular sieve membrane has a thickness of 1 to 20 μm; more preferably, the carbon molecular sieve membrane has a thickness of 1 to 10 μm.
5. A method for preparing the carbon molecular sieve membrane according to any one of claims 1 to 4, It is characterized in that The steps include: (1) Preparation of polymer crystalline material: adding a phenolic compound, a carbonyl-containing compound and a non-cyclic amine compound to a solvent for reaction to obtain a polymer crystalline material; (2) Preparation of a precursor: coating a polymer crystalline material on a carrier, aging the carrier, and using the aged polymer crystalline material as a precursor to obtain a carrier having a surface coated with the precursor; (3) Preparation of carbon molecular sieve membrane: The precursor on the surface of the carrier is carbonized to obtain a carbon molecular sieve membrane.
6. The preparation method according to claim 5, It is characterized in that In step (1), the phenolic compound is selected from one or more of monophenolic compounds and substituted monophenolic compounds, diphenolic compounds and substituted diphenolic compounds, and triphenolic compounds and substituted triphenolic compounds; Preferably, the substituent in the substituted monophenolic compound, substituted diphenolic compound or substituted triphenolic compound is selected from nitro, amino, methyl, ethyl, methoxy, carboxyl, formyl or formyloxy; More preferably, the phenolic compound is selected from one or more of phenol, resorcinol, hydroquinone, pyrogallol, bisphenol A and 1-naphthol; More preferably, the phenolic compound is selected from one or more of phenol, resorcinol, hydroquinone and 1-naphthol.
7. The preparation method according to claim 5 or 6, It is characterized in that In step (1), the carbonyl-containing compound is an aldehyde, an acid or a ketone; Preferably, the aldehyde is selected from aromatic aldehydes and / or C 1-3 of fatty aldehydes; More preferably, the aldehyde comprises one or more of formaldehyde, benzaldehyde, methyl, ethyl, hydroxyl, methoxy, acetylamino, dimethylamino or amino substituted benzaldehyde, salicylaldehyde and trimethylamino, nitro, cyano, sulfonic acid, aldehyde or carboxyl substituted salicylaldehyde; And / or, preferably, the acid is selected from one or more of isonicotinic acid, cyanuric acid, terephthalic acid and trimesic acid; And / or, preferably, the ketone is selected from one or more of cyclopropyl methyl ketone, methyl ethyl ketone, methyl heptenone, acetone and cyclohexanone.
8. The preparation method according to any one of claims 5 to 7, It is characterized in that In step (1), the non-cyclic amine compound includes one or more of aniline, methyl, ethyl, acetylamino or nitro substituted aniline, N,N-methylenebisacrylamide, 4,4'-diaminodiphenylmethane and hexamethylenediamine.
9. The preparation method according to any one of claims 5 to 8, It is characterized in that In step (1), the molar ratio of the phenolic compound to the carbonyl-containing compound is 1 to 4.5:1; Preferably, the molar ratio of the phenolic compound to the carbonyl-containing compound is 1.5 to 4.5:1; More preferably, the molar ratio of the phenolic compound to the carbonyl-containing compound is 1.5 to 4:1; and / or, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:1.5-20; Preferably, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:3 to 20; More preferably, the molar ratio of the carbonyl-containing compound to the non-cyclic amine compound is 1:4-20.
10. The preparation method according to any one of claims 5 to 9, It is characterized in that In step (1), the solvent includes one or more of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide; Preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the non-cyclic amine compound is 1-35:5-30, wherein the unit of volume is mL and the unit of molar amount is mmol; Preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the acyclic amine compound is 3-16:7-25, wherein the unit of volume is mL and the unit of molar amount is mmol; More preferably, the ratio of the volume of the reaction solvent to the total molar amount of the phenolic compound, the carbonyl-containing compound and the acyclic amine compound is 3-10:8-23, wherein the unit of volume is mL and the unit of molar amount is mmol.
11. The preparation method according to claim 10, It is characterized in that In step (1), the volume ratio of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide is (0-6):(0-5):(0-5):(0-5):(0-4.5), wherein the volume ratios of methanol, ethanol, benzyl alcohol, water and N,N-dimethylformamide are not 0 at the same time.
12. The preparation method according to any one of claims 5 to 11, It is characterized in that In step (1), the reaction temperature is 25 to 100° C.; preferably, the reaction temperature is 45 to 70° C.; more preferably, the reaction temperature is 60 to 70° C.; And / or, the reaction time is 6 to 30 hours; preferably, the reaction time is 10 to 24 hours; more preferably, the reaction time is 13 to 24 hours; And / or, the reaction speed is 400-700 rpm; preferably, the reaction speed is 400-550 rpm.
13. The preparation method according to any one of claims 5 to 12, It is characterized in that In step (2), the coating comprises the following steps: placing a reaction solution containing a polymer crystalline material on a carrier and aging it; preferably, the aging temperature is 20 to 120° C. and the aging time is 0.5 to 24 hours; And / or, the carrier is a porous material; preferably, the carrier is selected from one or more of anodized aluminum, porous glass, stainless steel mesh and phenolic resin.
14. The preparation method according to claim 13, It is characterized in that The coating is performed by a scraping method, which includes the following steps: placing a reaction solution containing a polymer crystalline material on a carrier, then adjusting and fixing the height difference between a scraper and the carrier, scraping and coating in the same direction, and aging; Preferably, the height difference between the scraper and the carrier is 5 to 100 μm; more preferably, the height difference between the scraper and the carrier is 10 to 50 μm; And / or, preferably, the aging temperature is 60-120°C; more preferably, the aging temperature is 80-110°C; further preferably, the aging temperature is 80-100°C; and / or, the aging time is 0.5-10h; preferably, the aging time is 2-8h; and / or, the aging pressure is 0.1-0.5MPa.
15. The preparation method according to claim 13, It is characterized in that The coating is a casting method, which includes the following steps: adjusting the viscosity of the reaction solution containing the polymer crystalline material to 10-20 Pa·s, then casting it on the carrier, and aging; preferably, the aging temperature is 25-50° C., and / or the aging time is 12-24 hours; Alternatively, the coating is a spin coating method, which includes the following steps: adjusting the viscosity of the reaction liquid containing the polymer crystalline material to 10-20 Pa·s, then fixing the carrier on a rotating device, adjusting the rotation speed, so that the reaction liquid is dispersed on the carrier, and aging; preferably, the rotation speed is 10000-15000rpm; more preferably, the aging temperature is 50-90°C; and / or the aging time is 6-12h.
16. The preparation method according to any one of claims 5 to 15, It is characterized in that In step (3), the carbonization conditions are: a heating rate of 0.1 to 5°C / min; a carbonization temperature of 600 to 1000°C, preferably 600 to 950°C; and / or a carbonization time of 2 to 22 hours, preferably 2 to 18 hours; And / or, the atmosphere of the carbonization process is an inert atmosphere, a hydrogen atmosphere or a nitrogen atmosphere; preferably, the inert atmosphere is argon.
17. A carbon molecular sieve membrane, It is characterized in that The carbon molecular sieve membrane is prepared by the method for preparing a carbon molecular sieve membrane according to any one of claims 5 to 16.
18. Use of the carbon molecular sieve membrane according to any one of claims 1 to 4 or the carbon molecular sieve membrane according to claim 17 in separating or purifying hydrogen.
19. A method for separating hydrogen from a hydrogen-mixed gas, It is characterized in that The steps include: Using the carbon molecular sieve membrane described in any one of claims 1 to 4 or the carbon molecular sieve membrane described in claim 17 as a permeation separation membrane, passing the mixed hydrogen gas into one side of the membrane assembly, and applying pressure on the side of the mixed hydrogen gas to make the mixed hydrogen gas permeate through the carbon molecular sieve membrane into the other side of the membrane assembly to obtain hydrogen separation gas; Preferably, the hydrogen-mixed gas is hydrogen and one or a combination of two or more of the following gases: methane, nitrogen, oxygen, carbon dioxide, ethane, ethylene, propane, propylene, butane, isobutane, butylene and isobutylene; More preferably, the volume ratio of hydrogen in the hydrogen mixed gas is 1% to 80%; More preferably, the pressure difference between the two sides of the membrane is 0.1-3 MPa.
Citation Information
Patent Citations
Preparation method of palladium-base composite membrane
CN107376661A
Fluorine-containing silicon low-surface-energy material for nano-imprinting and preparation method thereof
CN101750896A
Main chain benzoxazine copolymer oligomer, copolymer resin and preparation method thereof
CN108641055A
Monoamine-terminated ultrahigh-frequency low-dielectric main chain benzoxazine copolymer oligomer, copolymer resin and preparation method thereof
CN110818868A
Phenolic aldehyde-based unsupported mesoporous-microporous carbon membrane as well as preparation method and application thereof
CN115970512A