Adsorbent as well as preparation method and application thereof
By using an adsorbent composed of activated carbon support and metal single atoms to catalyze the decomposition of free chlorine in hydrochloric acid at low temperature, the problem of insufficient removal of free chlorine in hydrochloric acid is solved, and high efficiency, low energy consumption, hydrochloric acid purity and environmental safety are achieved. improve.
Patent Information
- Application Number
- CN202411280170.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
AI Technical Summary
The removal method of free chlorine in hydrochloric acid in industrialization consumes a lot of energy and is insufficient, affecting the purity and safety of hydrochloric acid and poses a risk of environmental pollution.
Adsorbent composed of activated carbon support and metal single atoms (Zn, Fe, Al, Cu) are used to catalyze the free chlorine in hydrochloric acid at low temperature, and high catalytic activity and stability are prepared by specific preparation methods. adsorbent.
It achieves efficient removal of free chlorine in hydrochloric acid, improves the purity of hydrochloric acid, reduces energy consumption, and enhances the stability and safety of adsorbents.
Smart Images

Figure CN118988250A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an adsorbent and a preparation method and application thereof, belonging to the technical field of adsorbents. Background Art
[0002] The HCl oxidation method is used industrially to convert the HCl produced as a by-product during the phosgenation reaction into liquid chlorine for recycling. During the chlorine production process, some hydrogen chloride gas cannot be completely converted. It is captured by water absorption and made into hydrochloric acid for sale. However, since some chlorine is mixed in the hydrogen chloride gas, the produced hydrochloric acid contains a small amount of free chlorine. This free chlorine not only affects the widespread use of hydrochloric acid, but also causes chlorine to escape during the storage of hydrochloric acid, causing harm to human health and generating environmental pollution.
[0003] At present, the industrial removal of free chlorine in hydrochloric acid mainly adopts the gas stripping method, that is, the hydrochloric acid is purged with inert gas and heated with steam. This method not only consumes a lot of energy, but also the free chlorine in the hydrochloric acid after gas stripping fluctuates greatly due to the influence of temperature, the free chlorine is not fully removed, and the purity of the treated hydrochloric acid is not high. Summary of the invention
[0004] The invention provides an adsorbent, which can catalyze the decomposition of free chlorine in hydrochloric acid at low temperature, thereby improving the adsorption efficiency of the free chlorine in the hydrochloric acid.
[0005] The invention provides a method for preparing the adsorbent, which is simple to operate and suitable for wide promotion and application.
[0006] The present invention provides a method for removing free chlorine from hydrochloric acid. The above-mentioned adsorbent or the adsorbent prepared by the above-mentioned preparation method is used to perform adsorption treatment on hydrochloric acid to remove free chlorine from the hydrochloric acid. The removal method is simple to operate, and the free chlorine can be fully removed, so that hydrochloric acid with higher purity can be obtained.
[0007] The present invention provides an adsorbent, wherein the adsorbent comprises an activated carbon carrier and metal single atoms located in at least part of the pores and / or the surface of the activated carbon carrier;
[0008] The metal single atom includes at least one of Zn, Fe, Al, and Cu;
[0009] In the adsorbent, the mass percentage of metal single atoms is 10-15%.
[0010] The adsorbent as described above, wherein the particle size of the adsorbent is 200 to 600 nm.
[0011] The present invention provides a method for preparing the adsorbent as described above, which comprises the following steps:
[0012] 1) after dispersing an activated carbon source and a thiol in a solvent, an aging treatment, a first drying treatment and a first calcination treatment are sequentially performed to form an activated carbon carrier;
[0013] 2) using a metal salt solution to sequentially perform an impregnation treatment, a second drying treatment, and a second calcination treatment on the activated carbon carrier to obtain the adsorbent;
[0014] The metal element in the metal salt solution includes at least one of Zn, Fe, Al and Cu.
[0015] The preparation method as described above, wherein before step 1), further comprises grinding the activated carbon source to make the particle size of the activated carbon source be 200-600 nm.
[0016] The preparation method as described above, wherein, in the aging treatment, the temperature is 80-90° C. and the time is 3-7 h; and / or,
[0017] In the first drying process, the temperature is 100-150° C. and the time is 2-4 hours; and / or,
[0018] In the first calcination treatment, the temperature is 300-500° C. and the time is 17-25 hours.
[0019] The preparation method as described above, wherein the immersion treatment is carried out at a temperature of 25 to 40° C. for a time of 1 to 2 hours; and / or,
[0020] In the second drying process, the temperature is 80-100°C and the time is 2-5h; and / or,
[0021] In the second calcination treatment, the temperature is 200-300° C. and the time is 12-15 hours.
[0022] In the preparation method as described above, the mass ratio of the thiol, the solvent and the activated carbon source is 1:(500-900):(120-300).
[0023] The preparation method as described above, wherein the thiol is selected from at least one of 1-propanethiol, ethanethiol, ethanedithiol and cysteine; and / or,
[0024] The solvent comprises an alcohol solvent, and the alcohol solvent is selected from at least one of methanol, ethanol and isopropanol.
[0025] The present invention provides a method for removing free chlorine from hydrochloric acid, wherein the hydrochloric acid to be treated is subjected to adsorption treatment using the adsorbent as described above; or,
[0026] The adsorbent prepared by the preparation method described above is used to adsorb the hydrochloric acid to be treated.
[0027] The removal method as described above, wherein in the adsorption treatment, the temperature is 25-40°C, the pressure is normal pressure, and the residence time is 0.01-0.08h -1 and / or,
[0028] The content of free chlorine in the hydrochloric acid to be treated is 1000-5000ppm.
[0029] The adsorbent of the present invention comprises an activated carbon carrier and metal single atoms located in at least part of the pores and / or the surface of the activated carbon carrier, wherein the metal single atoms comprise at least one of Zn, Fe, Al and Cu; in the adsorbent, the mass percentage of the metal single atoms is 10-15%. The adsorbent has a high loading amount of metal single atoms, high catalytic activity, and excellent stability. When used to remove free chlorine in hydrochloric acid, the free chlorine in the hydrochloric acid can be removed efficiently, thereby improving the purity of the hydrochloric acid.
[0030] The preparation method of the adsorbent of the present invention can prepare the above-mentioned adsorbent, and the preparation method is simple to operate and suitable for wide promotion and application.
[0031] The method for removing free chlorine from hydrochloric acid of the present invention uses the above-mentioned adsorbent or the adsorbent prepared by the above-mentioned preparation method to adsorb hydrochloric acid to remove free chlorine from the hydrochloric acid. The removal method is simple to operate, and the free chlorine is fully removed, so that hydrochloric acid with higher purity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the following briefly introduces the drawings required for use in the embodiments of the present invention or related technologies. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 Graph showing the pore size distribution of the adsorbent in some embodiments of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] A first aspect of the present invention provides an adsorbent, the adsorbent comprising an activated carbon carrier and metal single atoms located in at least part of the pores and / or the surface of the activated carbon carrier;
[0036] The metal element in the metal single atom includes at least one of Zn, Fe, Al, and Cu;
[0037] The mass percentage of the metal element in the adsorbent is 10-15%.
[0038] In the present invention, the metal single atom may be located in the entire pores of the activated carbon carrier, or in part of the pores of the activated carbon carrier; and / or, the metal single atom may be located in the entire surface of the activated carbon carrier, or in part of the surface of the activated carbon carrier.
[0039] In the adsorbent of the present invention, the loading amount of the metal element in the metal single atom is relatively high, which can improve the catalytic activity of the adsorbent, and the metal single substance in the adsorbent and the activated carbon carrier have excellent binding force, which can improve the stability of the adsorbent. When the adsorbent is used to remove free chlorine in hydrochloric acid, the removal efficiency of free chlorine in hydrochloric acid can be improved, thereby obtaining high-purity hydrochloric acid.
[0040] Figure 1 Figure 2 is a particle size distribution diagram of the adsorbent in some embodiments of the present invention. Figure 1 As shown, in some embodiments of the present invention, the particle size of the adsorbent is 200 to 600 nm. In the present invention, the particle size of the adsorbent is the same as the particle size of the activated carbon carrier. When the particle size of the adsorbent is within the above range, the adsorbent has higher catalytic activity and stability.
[0041] The second aspect of the present invention provides a method for preparing the adsorbent of the first aspect, comprising the following steps:
[0042] 1) after dispersing an activated carbon source and a thiol in a solvent, an aging treatment, a first drying treatment and a first calcination treatment are sequentially performed to form an activated carbon carrier;
[0043] 2) using a metal salt solution to sequentially perform an impregnation treatment, a second drying treatment, and a second calcination treatment on the activated carbon carrier to obtain an adsorbent;
[0044] The metal element in the metal salt solution includes at least one of Zn, Fe, Al and Cu.
[0045] In the present invention, the activated carbon source refers to a material used to form an activated carbon carrier, which may be granular or powdery. Exemplarily, the activated carbon source may be at least one of wood activated carbon, coconut shell, bamboo charcoal, and coal. The metal salt solution may be a solution formed by a salt including at least one of Zn, Fe, Al, and Cu, for example, the metal salt solution may be a solution formed by chlorides of zinc, aluminum, iron, and copper metals.
[0046] The preparation method of the present invention specifically comprises: 1) uniformly dispersing an activated carbon source and a thiol in a solvent, and then performing an aging treatment to allow the activated carbon source and the thiol to fully react, wherein the oxygen-containing functional groups (e.g., carboxyl groups) on the surface of the activated carbon source undergo a carboxyl-sulfide exchange reaction with the sulfhydryl groups in the thiol to form an acylsulfide intermediate; then performing a first drying treatment to remove the solvent; and then performing a first calcination treatment to form an activated carbon carrier including a thiol ester compound;
[0047] 2) The activated carbon carrier is impregnated with a metal salt solution so that the metal salt fills at least part of the pores of the activated carbon carrier or is located on at least part of the surface of the activated carbon carrier. During the impregnation process, the thiol carboxyl group of the acylsulfide intermediate has a strong metal affinity and can form a stable coordination bond with the metal ion, thereby increasing the loading amount of the metal ion and the binding force between the metal ion and the activated carbon carrier; then a second drying treatment is performed to remove the liquid phase in the metal salt solution, and finally a second calcination treatment is performed to obtain an activated carbon carrier and metal single atoms located in at least part of the pores and / or the surface of the activated carbon carrier.
[0048] In some embodiments, in step 1), after the activated carbon source and the thiol are dispersed in the solvent, stirring treatment can be performed for 1-2 hours to allow the activated carbon source and the thiol to be more fully dispersed in the solvent.
[0049] In the preparation method of the adsorbent of the present invention, thiol is used to react with an activated carbon source, so that the oxygen-containing functional group carboxyl group on the surface of the carbon powder undergoes a carboxylsulfide exchange reaction with the thiol, thereby obtaining an acylsulfide intermediate. In the subsequent metal salt impregnation treatment, since the thiol carboxyl group in the acylsulfide intermediate has a strong metal affinity, it can form a stable coordination bond with the loaded metal ion, thereby improving the stability of the adsorbent, and can also increase the loading amount of the metal ion, further improving the catalytic activity of the adsorbent.
[0050] In some embodiments of the present invention, before step 1), the activated carbon source is further ground to make the particle size of the activated carbon source be 200-600 nm.
[0051] Specifically, the activated carbon source is ground to a particle size of 200-600 nm, and then the activated carbon source of 200-600 nm and thiol are dispersed in a solvent, and then an aging treatment, a first drying treatment and a first calcination treatment are performed in sequence to form an activated carbon carrier.
[0052] The present invention does not particularly limit the specific process of the grinding process, as long as an activated carbon source with a particle size of 200-600nm can be formed. In some embodiments, the grinding process can be carried out in a high-energy grinder, specifically, the high-energy grinder can be a vibrating ball mill. In other embodiments, a grinding aid and a grinding ball can be added during the grinding process to promote the grinding process, wherein the grinding aid can be zinc stearate and the grinding ball can be a zirconium oxide ball.
[0053] The present invention grinds the activated carbon source before step 1) to obtain an activated carbon source with a specific particle size, which can promote the subsequent reaction between the activated carbon source and thiol, thereby improving the efficiency of the impregnation treatment and obtaining an adsorbent with high catalytic activity and better stability.
[0054] The present invention does not particularly limit the thiol, and may be any thiol commonly used in the art. For example, the thiol may be selected from at least one of 1-propanethiol, ethanethiol, ethanedithiol and cysteine.
[0055] The solvent of the present invention is not particularly limited and can be a commonly used solvent in the art. In some embodiments of the present invention, when the solvent includes an alcohol solvent, the thiol and the activated carbon source can be more fully dispersed, and the alcohol solvent is easily volatilized during the subsequent drying and roasting process, thereby improving the catalytic activity and stability of the adsorbent and improving the preparation efficiency of the adsorbent. In some embodiments, the alcohol solvent is selected from at least one of methanol, ethanol and isopropanol.
[0056] The inventors found in the study that the specific parameters of the aging treatment, the first drying treatment and the first calcination treatment can be limited to obtain an activated carbon carrier containing more acylsulfide intermediates, thereby promoting the subsequent impregnation treatment and improving the catalytic activity and stability of the adsorbent. Exemplarily, in some embodiments of the present invention, when the temperature is 80-90°C and the time is 3-7h during the aging treatment, the activated carbon source and the mercaptan can undergo a more complete carboxylsulfide exchange reaction to form more acylsulfide intermediates, promote the subsequent impregnation treatment, and improve the catalytic activity and stability of the adsorbent;
[0057] When the temperature in the first drying treatment is 100-150°C and the time is 2-4h, the solvent can be removed more fully while saving energy, thereby improving the catalytic activity and stability of the adsorbent;
[0058] When the temperature in the first roasting treatment is 300-500°C and the time is 17-25h, an activated carbon carrier with excellent performance can be obtained while saving energy, which is helpful for the subsequent impregnation treatment.
[0059] The inventors also found that by selecting the specific processes of the impregnation treatment, the second drying treatment and the second calcination treatment, the catalytic activity and stability of the adsorbent can be further improved. For example, in some embodiments of the present invention, during the impregnation treatment, the temperature is 25 to 40°C and the time is 1 to 2 hours; and / or,
[0060] In the second drying process, the temperature is 80-100°C and the time is 2-5h; and / or,
[0061] In the second calcination treatment, the temperature is 200-300°C and the time is 12-15h.
[0062] In the present invention, the first calcination treatment and the second calcination treatment may be performed in a muffle furnace.
[0063] In some embodiments of the present invention, when the mass ratio of thiol, solvent and activated carbon source is 1: (500-900): (120-300), the thiol and the activated carbon source can be more fully dispersed in the solvent, and the thiol can better undergo carboxylsulfide exchange reaction with the activated carbon source to obtain an activated carbon carrier containing more acylsulfide intermediates, thereby promoting the subsequent impregnation treatment and improving the catalytic activity and stability of the adsorbent.
[0064] The third aspect of the present invention provides a method for removing free chlorine from hydrochloric acid, using the adsorbent of the first aspect to adsorb the hydrochloric acid to be treated; or,
[0065] The adsorbent prepared by the preparation method of the second aspect is used to adsorb the hydrochloric acid to be treated.
[0066] The present invention does not specifically limit the hydrochloric acid to be treated, and any hydrochloric acid containing free chlorine is within the protection scope of the present invention. The present invention uses the adsorbent of the first aspect or the adsorbent prepared by the preparation method of the second aspect to adsorb the hydrochloric acid to be treated, and the adsorbent can catalytically decompose the free chlorine in the hydrochloric acid to be treated, remove the free chlorine in the hydrochloric acid to be treated, and obtain hydrochloric acid with higher purity.
[0067] The removal method of the present invention is not only simple to operate, but also can fully remove free chlorine in hydrochloric acid, thereby obtaining hydrochloric acid with higher purity, and is suitable for wide promotion and application.
[0068] In some embodiments of the present invention, specific parameters of the adsorption treatment can be selected to further improve the efficiency of the adsorption treatment and obtain higher purity hydrochloric acid. For example, in the adsorption treatment, the temperature is 25-40°C, the pressure is normal pressure, and the residence time is 0.01-0.08h. -1 .
[0069] The inventors have also found that the adsorption treatment of the present invention has an excellent adsorption effect on the hydrochloric acid to be treated with a free chlorine content of 1000-5000 ppm.
[0070] In some embodiments, the adsorbent can be filled in the adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column and is adsorbed in the adsorption column, and the residence time of the hydrochloric acid to be treated in the adsorption column is controlled to be 0.01-0.08h. -1 , so that the treated hydrochloric acid is extracted from the bottom of the adsorption column.
[0071] The technical solution of the present invention will be further described below in conjunction with specific embodiments.
[0072] Example 1
[0073] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0074] 1) adding commercially available wood activated carbon zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 260 nm;
[0075] Weigh 3 g of 1-propanethiol, 1500 g of methanol, and 380 g of an activated carbon source, mix them, stir for 1 h, stand at 80 ° C for 4 h for aging, then perform a first drying treatment at 120 ° C for 2 h, and then place them in a muffle furnace at 300 ° C for a first calcination treatment for 17 h to obtain an activated carbon carrier;
[0076] 2) Weigh a zinc chloride salt solution, add an activated carbon carrier according to a 10 wt% loading amount, and perform an immersion treatment at 30° C. for 2 h, followed by a second drying treatment at 80° C. for 3 h, and place the solution in a muffle furnace at 300° C. for a second calcination treatment for 13 h to obtain an adsorbent.
[0077] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0078] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0079] During the adsorption treatment, the temperature was 40°C, the pressure was normal pressure, and the residence time was 0.03h. -1 ;
[0080] The free chlorine content in the hydrochloric acid to be treated is 1600 ppm, and the free chlorine content in the hydrochloric acid after adsorption treatment is 120 ppm. The removal efficiency of free chlorine in the hydrochloric acid is 92%.
[0081] Example 2
[0082] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0083] 1) adding commercially available wood activated carbon, zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 600 nm;
[0084] Weigh 2 g of 1-propanethiol, 1600 g of methanol, and 500 g of an activated carbon source, mix them, stir for 1 h, stand at 85 ° C for 5 h for aging, then perform a first drying treatment at 110 ° C for 3 h, and then place them in a muffle furnace at 400 ° C for a first calcination treatment for 24 h to obtain an activated carbon carrier;
[0085] 2) Weigh the ferrous chloride solution, add the activated carbon carrier according to the 13 wt% loading amount, and immerse it at 28° C. for 1 hour, then perform a second drying treatment at 85° C. for 5 hours, and place it in a muffle furnace at 240° C. for a second calcination treatment for 14 hours to obtain an adsorbent.
[0086] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0087] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0088] During the adsorption treatment, the temperature was 32°C, the pressure was normal, and the residence time was 0.04h. -1 ;
[0089] The free chlorine content in the hydrochloric acid to be treated is 1300 ppm, and the free chlorine content in the hydrochloric acid after adsorption treatment is 150 ppm. The removal efficiency of free chlorine in the hydrochloric acid is 88%.
[0090] Example 3
[0091] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0092] 1) adding commercially available wood activated carbon, zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 480 nm;
[0093] Weigh 3 g of 1-propanethiol, 1800 g of methanol, and 600 g of an activated carbon source, mix them, stir for 2 h, stand at 90 ° C for 7 h for aging, then perform a first drying treatment at 100 ° C for 4 h, and then place them in a muffle furnace at 430 ° C for a first calcination treatment for 21 h to obtain an activated carbon carrier;
[0094] 2) Weigh aluminum chloride salt solution, add activated carbon carrier according to 12 wt% loading, immerse at 32° C. for 2 h, perform a second drying treatment at 88° C. for 5 h, place in a muffle furnace at 270° C. for a second calcination treatment for 15 h, and obtain an adsorbent.
[0095] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0096] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0097] During the adsorption treatment, the temperature was 25°C, the pressure was normal pressure, and the residence time was 0.05h. -1 ;
[0098] The free chlorine content in the hydrochloric acid to be treated is 1400 ppm, and the free chlorine content in the hydrochloric acid after adsorption treatment is 130 ppm. The removal efficiency of free chlorine in the hydrochloric acid is 91%.
[0099] Example 4
[0100] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0101] 1) adding commercially available wood activated carbon, zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 450 nm;
[0102] Weigh 2 g of 1-propanethiol, 1200 g of methanol, and 250 g of an activated carbon source, mix them, stir for 2 h, stand at 88 ° C for 6 h for aging, then perform a first drying treatment at 130 ° C for 4 h, and then place them in a muffle furnace at 340 ° C for a first calcination treatment for 19 h to obtain an activated carbon carrier;
[0103] 2) Weigh aluminum chloride salt solution, add activated carbon carrier according to 15 wt% loading, immerse at 36°C for 2 h, then perform a second drying treatment at 100°C for 3 h, place in a muffle furnace at 290°C for a second calcination treatment for 12 h, and obtain an adsorbent.
[0104] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0105] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0106] During the adsorption treatment, the temperature was 33°C, the pressure was normal, and the residence time was 0.08h. -1 ;
[0107] The free chlorine content in the hydrochloric acid to be treated is 1500ppm, the free chlorine content in the hydrochloric acid after adsorption treatment is 150ppm, and the removal efficiency of free chlorine in the hydrochloric acid is 90%.
[0108] Example 5
[0109] The preparation method of the adsorbent in this embodiment is basically the same as that in Example 1, except that:
[0110] 1) Obtain an activated carbon source with a particle size of 800 nm.
[0111] The method for removing free chlorine from hydrochloric acid in this embodiment is basically the same as that in Example 1, except that:
[0112] The adsorbent in this example was used for adsorption treatment. After the adsorption treatment, the free chlorine content in the hydrochloric acid was 220 ppm, and the removal efficiency of the free chlorine in the hydrochloric acid was 86%.
[0113] Example 6
[0114] The preparation method of the adsorbent in this embodiment is basically the same as that in Example 1, except that:
[0115] 1) During the aging treatment, the temperature is 50°C and the time is 8h;
[0116] In the first drying treatment, the temperature was 90°C and the time was 1 h;
[0117] In the second calcination treatment, the temperature was 600° C. and the time was 10 h.
[0118] The method for removing free chlorine from hydrochloric acid in this embodiment is basically the same as that in Example 1, except that:
[0119] The adsorbent in this example was used for adsorption treatment. After the adsorption treatment, the free chlorine content in the hydrochloric acid was 450 ppm, and the removal efficiency of the free chlorine in the hydrochloric acid was 76%.
[0120] Example 7
[0121] The preparation method of the adsorbent in this embodiment is basically the same as that in Example 1, except that:
[0122] 2) During the immersion treatment, the temperature is 60°C and the time is 3h;
[0123] In the second drying treatment, the temperature was 120°C and the time was 4 h;
[0124] In the second calcination treatment, the temperature was 350° C. and the time was 8 h.
[0125] The method for removing free chlorine from hydrochloric acid in this embodiment is basically the same as that in Example 1, except that:
[0126] The adsorbent in this example was used for adsorption treatment. After the adsorption treatment, the free chlorine content in the hydrochloric acid was 380 ppm, and the removal efficiency of the free chlorine in the hydrochloric acid was 77%.
[0127] Example 8
[0128] The preparation method of the adsorbent in this embodiment is basically the same as that in Example 1, except that:
[0129] 1) Weigh 1000 g of methanol and 400 g of activated carbon source.
[0130] The method for removing free chlorine from hydrochloric acid in this embodiment is basically the same as that in Example 1, except that:
[0131] The adsorbent of this embodiment was used for adsorption treatment. After the adsorption treatment, the free chlorine content in the hydrochloric acid was 280 ppm, and the removal efficiency of the free chlorine in the hydrochloric acid was 83%.
[0132] Example 9
[0133] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0134] 1) adding commercially available wood activated carbon, zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 500 nm;
[0135] Weigh 1 g of ethyl mercaptan, 800 g of methanol, and 130 g of an activated carbon source, mix them, stir for 1 h, stand at 85 ° C for 6 h for aging, then perform a first drying treatment at 100 ° C for 4 h, and then place them in a muffle furnace at 480 ° C for a first calcination treatment for 25 h to obtain an activated carbon carrier;
[0136] 2) Weigh a zinc chloride salt solution, add an activated carbon carrier according to a loading amount of 11 wt%, and perform an impregnation treatment at 32° C. for 1 h, then perform a second drying treatment at 90° C. for 3 h, and place the activated carbon carrier in a muffle furnace at 290° C. for a second calcination treatment for 12 h to obtain an adsorbent.
[0137] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0138] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0139] During the adsorption treatment, the temperature was 28°C, the pressure was normal, and the residence time was 0.06h. -1 ;
[0140] The free chlorine content in the hydrochloric acid to be treated is 4000 ppm, and the free chlorine content in the hydrochloric acid after adsorption treatment is 390 ppm. The removal efficiency of free chlorine in the hydrochloric acid is 91%.
[0141] Example 10
[0142] The adsorbent of this embodiment is prepared by a method comprising the following steps:
[0143] 1) adding commercially available wood activated carbon, zirconium oxide balls and zinc stearate into a vibration ball mill and grinding them to obtain an activated carbon source with a particle size of 500 nm;
[0144] Weigh 1 g of ethyl mercaptan, 800 g of methanol, and 130 g of an activated carbon source, mix them, stir for 1 h, stand at 85 ° C for 6 h for aging, then perform a first drying treatment at 100 ° C for 4 h, and then place them in a muffle furnace at 480 ° C for a first calcination treatment for 25 h to obtain an activated carbon carrier;
[0145] 2) Weigh a zinc chloride salt solution, add an activated carbon carrier according to a loading amount of 11 wt%, and perform an impregnation treatment at 32° C. for 1 h, then perform a second drying treatment at 90° C. for 3 h, and place the activated carbon carrier in a muffle furnace at 290° C. for a second calcination treatment for 12 h to obtain an adsorbent.
[0146] The method for removing free chlorine from hydrochloric acid of the present embodiment comprises:
[0147] The adsorbent of this embodiment is filled in an adsorption column, so that the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and the adsorption treatment is performed in the adsorption column, so that the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0148] During the adsorption treatment, the temperature was 60°C, the pressure was normal, and the residence time was 0.09h. -1 ;
[0149] The free chlorine content in the hydrochloric acid to be treated is 4000ppm, and the free chlorine content in the hydrochloric acid after adsorption treatment is 600ppm, and the removal efficiency of free chlorine in the hydrochloric acid is 85%.
[0150] Comparative Example 1
[0151] The adsorbent in this comparative example is commercially available activated carbon.
[0152] The method for removing free chlorine in the hydrochloric acid of this comparative example comprises:
[0153] The adsorbent of this comparative example is filled in an adsorption column, and the hydrochloric acid to be treated enters the adsorption column from the top of the adsorption column, and is adsorbed in the adsorption column, and the hydrochloric acid after the adsorption treatment is extracted from the bottom of the adsorption column;
[0154] During the adsorption treatment, the temperature was 40°C, the pressure was normal, and the residence time was 0.06h. -1 ;
[0155] The free chlorine content in the hydrochloric acid to be treated is 1100ppm, the free chlorine content in the hydrochloric acid after adsorption treatment is 450ppm, the C content is 2000ppm, the removal efficiency of free chlorine in the hydrochloric acid is 60%, and the carbon powder in the activated carbon will be lost during the adsorption treatment.
[0156] Comparative Example 2
[0157] The preparation method of the adsorbent in this comparative example is basically the same as that in Example 1, except that:
[0158] 1) No 1-propanethiol is added;
[0159] 2) The actual Zn content of the obtained adsorbent was measured to be 2 wt%.
[0160] The method for removing free chlorine in hydrochloric acid in this comparative example is basically the same as that in Example 1, except that:
[0161] The adsorbent of this comparative example was filled into an adsorption column for adsorption treatment. After the adsorption treatment, the free chlorine content in the hydrochloric acid was 460 ppm, and the removal efficiency of the free chlorine in the hydrochloric acid was 72%. The loss of carbon powder was observed during the adsorption process.
[0162] Table 1 shows the metal content, adsorption efficiency, adsorption treatment temperature and adsorbent stability of the adsorbent in different embodiments and comparative examples;
[0163] Table 1
[0164]
[0165] It can be seen from Table 1 that when the adsorbent of the embodiment of the present invention is used to remove free chlorine in hydrochloric acid, the removal efficiency of free chlorine is high, and there is no loss of activated carbon during the removal process, indicating that the adsorbent of the present invention has excellent catalytic activity and stability.
[0166] Further, it can be seen from Example 1 and Comparative Example 1 that by reacting thiol with an activated carbon source and performing metal salt impregnation treatment, an adsorbent with high adsorption efficiency and stability can be obtained. It can be seen from Example 1 and Comparative Example 2 that only performing metal salt impregnation treatment has limited improvement on the adsorption efficiency of the adsorbent. By reacting thiol with an activated carbon source and then performing metal salt impregnation treatment, an adsorbent with both excellent adsorption efficiency and stability can be obtained.
[0167] It can be seen from Examples 1 and 5 that by selecting the particle size of the activated carbon source, the obtained adsorbent has a higher adsorption efficiency when used for adsorption treatment;
[0168] It can be seen from Example 1 and Example 6 that by selecting the specific processes of the aging treatment, the first drying treatment and the first calcination treatment in the preparation process of the activated carbon carrier, an adsorbent with higher adsorption efficiency can be obtained;
[0169] It can be seen from Example 1 and Example 7 that the adsorption efficiency of the adsorbent can be further improved by selecting the specific processes of the impregnation treatment, the second drying treatment, and the second calcination treatment;
[0170] It can be seen from Example 1 and Example 8 that the adsorption efficiency of the adsorbent can be further improved by selecting the content of each raw material in the preparation process of the activated carbon carrier.
[0171] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. The above are only preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are included in the scope of protection of the present invention.
Claims
1. An adsorbent, characterized in that: The adsorbent includes an activated carbon carrier and metal single atoms located in at least part of the pores and / or the surface of the activated carbon carrier; The metal single atom includes at least one of Zn, Fe, Al, and Cu; In the adsorbent, the mass percentage of metal single atoms is 10-15%.
2. The adsorbent according to claim 1, characterized in that The particle size of the adsorbent is 200-600 nm.
3. A method for preparing the adsorbent according to claim 1 or 2, characterized in that: The following steps are involved: 1) after dispersing an activated carbon source and a thiol in a solvent, an aging treatment, a first drying treatment and a first calcination treatment are sequentially performed to form an activated carbon carrier; 2) using a metal salt solution to sequentially perform an impregnation treatment, a second drying treatment, and a second calcination treatment on the activated carbon carrier to obtain the adsorbent; The metal element in the metal salt solution includes at least one of Zn, Fe, Al and Cu.
4. The preparation method according to claim 3, characterized in that: Before step 1), the method further includes grinding the activated carbon source to make the particle size of the activated carbon source be 200-600 nm.
5. The preparation method according to claim 3 or 4, characterized in that: During the aging treatment, the temperature is 80-90°C and the time is 3-7h; and / or, In the first drying process, the temperature is 100-150° C. and the time is 2-4 hours; and / or, In the first calcination treatment, the temperature is 300-500° C. and the time is 17-25 hours.
6. The preparation method according to any one of claims 3 to 5, characterized in that: During the immersion treatment, the temperature is 25-40° C. and the time is 1-2 hours; and / or, In the second drying process, the temperature is 80-100°C and the time is 2-5h; and / or, In the second calcination treatment, the temperature is 200-300° C. and the time is 12-15 hours.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The mass ratio of the thiol, the solvent and the activated carbon source is 1:(500-900):(120-300).
8. The preparation method according to any one of claims 3 to 7, characterized in that: The thiol is selected from at least one of 1-propanethiol, ethanethiol, ethanedithiol and cysteine; and / or, The solvent comprises an alcohol solvent, and the alcohol solvent is selected from at least one of methanol, ethanol and isopropanol.
9. A method for removing free chlorine from hydrochloric acid, characterized in that: Using the adsorbent according to claim 1 or 2 to adsorb the hydrochloric acid to be treated; or, The hydrochloric acid to be treated is adsorbed by the adsorbent prepared by the preparation method according to any one of claims 3 to 8.
10. The removal method according to claim 9, characterized in that: In the adsorption treatment, the temperature is 25-40°C, the pressure is normal pressure, and the residence time is 0.01-0.08h -1 and / or, The content of free chlorine in the hydrochloric acid to be treated is 1000-5000ppm.
Citation Information
Patent Citations
Preparation method and application of cyclic mercaptan-modified activated carbon
CN109589952A
Method for oxidizing and repairing polluted soil by using activated carbon-based monatomic iron catalyst
CN114308036A
Monoatomic dispersed palladium-based catalyst as well as preparation method and application thereof
CN115445636A
Removal of chlorine or chlorine compound and apparatus therefor
JP1999128675A
Cited By
Monatomic iron-loaded granular active carbon composite material as well as preparation method and application thereof
CN120920041A
A granular activated carbon composite material loaded with single-atom iron, its preparation method and its application