Preparation method of flaky metal composite catalyst

By preparing sheet metal composite catalysts, using pore-forming agents and ultrasonic modification technology to form rich pore structures, combined with rare earth metal compounds, the problems of high cost and difficulty in recycling of precious metal catalysts are solved, and efficient CO removal and long-life catalysts are achieved. Suitable for industrial applications.

CN118988333APending Publication Date: 2024-11-22PINGXIANG HUAXING ENVIRONMENTAL PROTECTION ENG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411031533.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing precious metal catalysts have high cost and are difficult to recycle during the CO oxidation process, which makes them unsuitable for industrial production and difficult to fully stimulate the activity of the catalyst.

Method used

Using the preparation method of sheet metal composite catalyst, a rich pore structure is formed by adding pore-forming agent, ultrasonic modification and hydrothermal reaction to the metal salt solution, and combining the excessive impregnation of rare earth metal compounds, good catalytic activity and Easy-to-recycle catalyst.

Benefits of technology

It realizes the efficient CO removal capability and long-lasting service life of the catalyst, reduces production costs, and has no secondary pollution throughout the process, which is green and environmentally friendly, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988333A_ABST
    Figure CN118988333A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalysts, in particular to a preparation method of a flaky metal composite catalyst, which comprises the following steps: (1) adding a certain amount of metal compound into an organic solvent, and stirring to completely dissolve the metal compound to obtain a metal salt solution A, adding a pore-forming agent into the metal salt solution A, stirring at a first preset temperature, and fully dissolving to obtain a mixed solution A; (2) adding alkali A and a high polymer A into the mixed solution A, and uniformly stirring; (3) performing ultrasonic modification on the solution uniformly stirred in the step (2) under certain conditions, and then transferring the solution into a high-temperature reaction kettle for hydrothermal reaction to obtain a mixed solution B; (4) filtering the mixed solution B, drying filter residues to obtain a catalyst precursor, and roasting the catalyst precursor to obtain a catalyst carrier; and (5) excessively impregnating the rare earth metal compound and the catalyst carrier according to a certain ratio.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of catalysts, and in particular to a method for preparing a flaky metal composite catalyst. Background Art

[0002] Hydrogen is an ideal clean energy. Its use can optimize the existing energy structure and effectively reduce carbon emissions. It is an important carrier for achieving the "dual carbon" goal. At present, hydrogen is mainly produced by processing primary fossil energy such as coal, oil and natural gas. The production process will release a large amount of CO, NO x and SO x Polluting gases such as CO2 cause irreversible damage to the environment and affect people's life and health, which has attracted widespread attention from academia and industry at home and abroad. Among them, the development of efficient CO oxidation catalysts is one of the current hot issues in catalysis.

[0003] At present, the methods for removing CO mainly include adsorption, combustion and catalytic oxidation. Among them, the catalytic oxidation method is widely used in clean energy development research due to its advantages such as high catalytic efficiency and no secondary pollution risk. For example, the patent with patent number ZL2024100889495 discloses a low-load Pt-based catalyst and its preparation method and application. The preparation method has the advantages of mild conditions, simple operation and environmental protection. The low-load Pt-based catalyst preferentially oxidizes CO in a H2-rich atmosphere, has a wide CO conversion temperature window in the reaction, and can achieve complete elimination of formaldehyde at room temperature. However, precious metal catalysts often have the problems of being expensive and difficult to recycle, and are not suitable for industrial production processes.

[0004] For example, the patent number ZL2023101371328 discloses a copper-iron alloy catalyst and its preparation and application. The catalyst has good catalytic activity, high CO product selectivity and stability, and the MgO carrier can promote the adsorption of carbon dioxide and improve the carbon dioxide conversion rate. However, the copper species may have clustering problems during the catalyst synthesis process, resulting in the hiding of the active crystal surface and active sites of the catalyst. It is difficult to fully stimulate the catalytic activity without effective treatment. Therefore, it is urgent to develop a catalyst with high catalytic activity and easy to reuse. Summary of the invention

[0005] In view of the shortcomings and existing problems of the prior art, the present disclosure provides a method for preparing a flaky metal composite catalyst. The catalyst prepared by the method is easy to recover and has a good catalytic effect.

[0006] The technical solution adopted by the present disclosure to solve the above technical problems is: a method for preparing a flaky metal composite catalyst, comprising the following steps:

[0007] (1) adding a certain amount of a metal compound to an organic solvent, stirring to completely dissolve the metal compound, to obtain a metal salt solution A, then adding a pore-forming agent to the metal salt solution A and stirring at a first preset temperature to obtain a mixed solution A after the metal compound is fully dissolved;

[0008] (2) adding base A and polymer A to the mixed solution A and stirring evenly;

[0009] (3) The solution stirred evenly in step (2) is ultrasonically modified under certain conditions, and then transferred to a high-temperature reactor for hydrothermal reaction to obtain a mixed solution B;

[0010] (4) filtering the mixed solution B and drying the filter residue to obtain a catalyst precursor, and calcining the catalyst precursor to obtain a catalyst carrier;

[0011] (5) The rare earth metal compound and the catalyst carrier are impregnated in excess according to a certain ratio, stirred to allow the rare earth metal compound to contact and react with the catalyst carrier, and then filtered, dried and calcined in sequence to obtain a sheet-like metal composite catalyst.

[0012] Wherein, in step (1), the metal compound is a first metal compound and a second metal compound, the first metal compound is one or more of copper nitrate, copper chloride, copper sulfate and copper acetate; the second metal compound is one or more of ferric nitrate, ferric chloride, ferric sulfate, ferric acetate, cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt acetate, manganese nitrate, manganese chloride, manganese sulfate, manganese acetate, zinc nitrate, zinc chloride, zinc sulfate and zinc acetate; the mass ratio of the first metal compound to the second metal compound is 10:1 to 2:1 in terms of oxide.

[0013] In step (1), the organic solvent is N,N-dimethylformamide, acetone, toluene or chloroform; and the mass ratio of the metal compound to the organic solvent is 0.05:1 to 0.3:1.

[0014] In step (1), the pore former is one of ammonium bicarbonate, ammonium bisulfate and carbon amide, and the mass ratio of the pore former to the solvent is 0.01:1 to 0.1:1. The pore former selected in the present disclosure uses the escaped ammonia gas as the pore-forming unit. Compared with the existing ammonium chloride and zinc salt, the pore former involved in the present disclosure is low in price, the pore-forming unit is easier to overflow, and more and more uniform pores can be generated during the pore development process. In addition, the amount of pore former should be moderate. If the amount of pore former is too small, the catalyst pores will not be fully formed, affecting the pollutant purification effect; if the amount of pore former is too much, it may cause adjacent pores to connect, some pores to collapse, and the specific surface area to decrease, which is not conducive to the exposure of active sites.

[0015] The first preset temperature is 40-80°C. The main purpose of heating is to accelerate the dissolution rate of the material. Low temperature and long stirring time may cause the base functional group to react with the metal after hydrolysis to form a precipitate. If the temperature is too high, part of the organic solvent will evaporate, resulting in distortion of the active ingredient load value and increased high temperature energy consumption. The stirring time is 2-5h.

[0016] Among them, in step (2), alkali A is first added to the mixed solution A to stabilize the liquid phase environment to ensure the smooth progress of the pore development process, and then polymer A is added to adjust the viscosity of the mixed solution; the addition rate of alkali A and polymer A is 0.1-1g / min. In the present disclosure, the material addition rate is mainly to ensure the smooth progress of the dissolution process. If the addition rate is too slow, the feeding time will be extended and the energy consumption will increase; if the feeding rate is too fast, it may cause agglomeration during the mixing process with the metal, affecting the effective dispersion of the active ingredients. The feeding rate involved in the present disclosure can avoid the agglomeration of active components while maintaining low energy consumption.

[0017] In step (2), the base A is one or more of sodium hydroxide, sodium carbonate and sodium bicarbonate, and the base A is added to adjust the pH so that the pH range of the mixed solution A is 8 to 10 to ensure the smooth progress of the pore development process.

[0018] In step (2), the polymer A is one of polyacrylonitrile (PAN), polyvinyl pyrrolidone (PVP), polymethyl methacrylate (PMMA) and polyacrylamide (PAM), and the polymer A is added to adjust the viscosity so that the viscosity of the mixed solution A is in the range of 800 to 2000 cps. This viscosity range is to ensure that the components of the catalyst can adhere to each other and there is no problem of scattered distribution. The polymer A acts as a bridge. If the viscosity is too low, the metal components cannot form a whole, and if the viscosity is too high, it is not conducive to the dispersion of the components.

[0019] In step (3), the conditions for ultrasonic modification of the mixed solution A are: ultrasonic power of 20-50 kW, ultrasonic temperature of 40-80° C., ultrasonic time of 1-5 h, and ultrasonic frequency of 20-100 KHz. Too low ultrasonic frequency will reduce the penetration of sound waves and fail to effectively optimize the performance of the catalyst. Too high ultrasonic frequency will cause the structure of the catalyst to collapse and the movement of active molecules to be too disordered, resulting in changes in the performance of the catalyst.

[0020] The purpose of increasing the temperature during ultrasound is to speed up the movement frequency of molecules so that they can be better dispersed into the solution. If the temperature is too low, the effective ingredients will disperse slowly and local agglomeration problems may occur. If the temperature is too high, the volatilization of the organic solvent will be accelerated, which will increase the viscosity and be unfavorable for the uniform migration of the ingredients in the liquid phase. Multiple experimental studies have proved that the temperature range disclosed in this disclosure can ensure the realization of the ultrasound goal.

[0021] Ultrasonic modification is a critical step in the catalyst preparation process. The action of ultrasonic sound waves on metal atoms will promote their movement, making them more evenly dispersed in the catalyst system, which is conducive to the exposure of active sites. The action of ultrasonic sound waves on the catalyst skeleton will optimize the structure of the catalyst due to the transfer of energy.

[0022] In step (3), the temperature of the hydrothermal reaction is 100-200°C. In the present disclosure, if the hydrothermal temperature is too low, the self-assembly process of the raw materials is restricted, the metal composite cannot be smoothly generated, and it is difficult to form a lamellar porous structure after aging; if the temperature is too high, the high-pressure reaction has safety risks and wastes energy. At the same time, the generated metal composite may further migrate and destroy the overall structure of the catalyst; the reaction time is 12-36h.

[0023] Hydrothermal reaction is a key step in the catalyst preparation process. This is due to the hydrothermal self-assembly process of the raw materials. The raw materials migrate autonomously under a specific temperature and pressure environment, and are arranged one by one in sequence to form an ordered metal complex skeleton. The use of hydrothermal reaction can ensure the regularity of the structure of the generated material. Compared with the current traditional temperature aging method, the hydrothermal process is easier to control, and the generated catalyst structure is more regular, without problems such as overlapping channels, which affects the exposure of the active crystal surface.

[0024] In step (4), after the mixed solution B is filtered, the filter residue is repeatedly washed with deionized water until the filtrate is neutral, and then dried.

[0025] Furthermore, the drying temperature is 80-150°C.

[0026] Furthermore, the calcination is carried out in a tubular furnace, and the calcination is carried out under anaerobic conditions, the purpose of which is to remove excess organic matter on the basis of stabilizing the carbon skeleton. The calcination temperature is 300-500°C. The main purpose of the calcination in this step is to remove the organic matter remaining on the catalyst precursor. Too low a temperature will result in incomplete removal of impurities, affecting the catalytic performance; too high a temperature may cause the catalyst structure to collapse; the heating rate is 1-5°C / min, and the calcination time is 2-5h. The heating rate should not be too fast, which is not conducive to the complete transformation of the catalyst structure, that is, local sintering will occur; the protective gas during calcination is one of nitrogen, helium and argon, and the air intake rate of the protective gas is 100-200mL / min.

[0027] Wherein, in step (5), the solvent used for excessive impregnation is deionized water; and the rare earth metal compound is one or more of cerium nitrate, cerium chloride, cerium sulfate, lanthanum nitrate, lanthanum chloride and lanthanum sulfate.

[0028] Furthermore, the mass ratio of the rare earth metal compound to the catalyst carrier is 0.05:1 to 0.3:1.

[0029] Furthermore, the stirring rate is 300-600 rpm, and the time is 6-12 h.

[0030] Furthermore, the drying temperature is 80-150°C.

[0031] Furthermore, the calcination is carried out in a muffle furnace, and the calcination is aerobic calcination. The calcination in this step is to remove carbon from the catalyst, and the aerobic conditions can ensure the complete conversion of carbon. The calcination temperature is 600-800°C, the heating rate is 1-5°C / min, and the calcination time is 2-5h. If the temperature is too low, incomplete conversion of carbon species will cover some active sites and reduce the catalytic performance; if the temperature is too high, the pore space of the composite catalyst may collapse, and it will also cause a waste of resources. The calcination in this step is an enhancement of the calcination in the previous step, removing carbon and strengthening the interconnection between metal composites.

[0032] Compared with the prior art, the present invention first adds a pore-forming agent to the metal salt solution A for pore formation, then ultrasonically modifies the pores to maintain stability, then hydrothermally reacts to orderly distribute the pore structure of the composite metal, and finally calcines to finalize the shape, so that the prepared flaky metal composite catalyst has a rich pore structure, micropores, mesopores and macropores, can provide more abundant active sites, and enhance the pollutant removal ability; in the process of preparing the flaky metal composite catalyst by the method of the present invention, there is no secondary pollution throughout the process, which is green and environmentally friendly; the prepared flaky metal composite catalyst has good CO poisoning resistance and a longer service life, and has great potential in industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present application will be further described in detail below in conjunction with the accompanying drawings and preferred embodiments, but those skilled in the art will appreciate that these drawings are drawn only for the purpose of explaining the preferred embodiments and therefore should not be used as a limitation on the scope of the present application. In addition, unless otherwise specified, the drawings are only schematically representing the composition or structure of the described objects and may contain exaggerated displays, and the drawings are not necessarily drawn to scale.

[0034] Figure 1 The CO conversion rate data of the catalysts prepared in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present disclosure under the same reaction conditions;

[0035] Figure 2 is the CO conversion rate and selectivity data of the catalyst prepared in Example 1 of the present disclosure;

[0036] Figure 3 is a scanning electron microscope image of the catalyst prepared in Example 1 of the present disclosure. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is described in detail, clearly and completely in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the present disclosure.

[0038] Example 1

[0039] A method for preparing a flaky metal composite catalyst comprises the following steps:

[0040] (1) adding copper nitrate and ferric nitrate to an N,N-dimethylamide solution, wherein the mass ratio of copper nitrate to ferric nitrate is 10:1 (calculated as oxides), and the mass ratio of the total mass of copper nitrate and ferric nitrate to N,N-dimethylamide is 0.1:1, stirring at room temperature to completely dissolve the copper nitrate and ferric nitrate to obtain a metal salt solution A, and then using carbonamide as a pore-forming agent, according to the mass ratio of carbonamide to N,N-dimethylamide of 0.01:1, adding carbonamide to the metal salt solution A, and stirring at 40°C for 2 hours, and obtaining a mixed solution A after being fully dissolved;

[0041] (2) adding sodium bicarbonate to the mixed solution A at a rate of 0.1 g / min and stirring to adjust the pH of the mixed solution A to 8, adding polyvinyl pyrrolidone to the mixed solution A at a rate of 0.1 g / min and stirring to adjust the viscosity of the mixed solution A to 1000 cps;

[0042] (3) After the pH and viscosity of the mixed solution A are adjusted, the mixed solution A is placed in an ultrasonic device and ultrasonicated at 40° C. for 2 h under the conditions of 40 kW and 50 kHz. The ultrasonicated liquid is then transferred to a high-temperature reactor and reacted at 150° C. for 12 h. After the reaction is completed, the reactor is taken out and naturally cooled to room temperature to obtain a catalyst precursor.

[0043] (4) The catalyst precursor is repeatedly washed with deionized water until the filtrate is neutral, and then the filter residue is dried at 100°C to obtain a catalyst precursor, and the catalyst precursor is transferred to a tube furnace for calcination. In a nitrogen atmosphere with an air intake of 100 mL / min, the temperature is increased to 300°C at a rate of 2°C / min, and the temperature is kept constant for 2 hours, and then naturally cooled to room temperature to obtain a catalyst carrier;

[0044] (5) Cerium nitrate and the catalyst carrier were added to an excess of deionized water at a mass ratio of 0.1:1, and the mixture was stirred at a rate of 300 rpm for 6 h. The mixed suspension was then filtered, and the filter residue was dried at 100 °C. The dried solid was then transferred to a muffle furnace for calcination, and the temperature was increased to 600 °C at a rate of 2 °C / min and kept constant for 2 h. When the temperature dropped to room temperature, a flaky metal composite catalyst was obtained.

[0045] Depend on Figure 2 It can be seen that the catalyst synthesized in this example absorbs CO under the following reaction conditions: CO concentration is 1%, H2 concentration is 50%, N2 is the balance gas, the mixed gas flow rate is 50mL / min, and the reaction temperature is 30-300°C. The results show that in the lower temperature window (<200°C), CO maintains 100% removal effect, CO selectivity is maintained at more than 80%, and has good thermal stability. No catalytic effect decline is detected within 50h, and 100% CO conversion rate is still maintained at 50h. In addition, by Figure 3 It can be seen that the catalyst prepared in this example is a lamellar structure, and the interior of the material is filled with many pore structures of different sizes, which can provide abundant active sites and enhance the CO removal capability.

[0046] Example 2

[0047] A method for preparing a flaky metal composite catalyst comprises the following steps:

[0048] (1) adding copper chloride, copper sulfate, cobalt chloride and manganese sulfate to an acetone solution, wherein the total mass ratio of copper chloride and copper sulfate to the total mass ratio of cobalt chloride and manganese sulfate is 8:1 (calculated as oxides), and the mass ratio of the total mass of copper chloride, copper sulfate, cobalt chloride and manganese sulfate to acetone is 0.05:1, stirring at room temperature to completely dissolve copper chloride, copper sulfate, cobalt chloride and manganese sulfate to obtain a metal salt solution A, and then using ammonium bicarbonate as a pore-forming agent, according to the mass ratio of ammonium bicarbonate to acetone of 0.02:1, adding ammonium bicarbonate to the metal salt solution A, and stirring at 50° C. for 3 hours, and obtaining a mixed solution A after being fully dissolved;

[0049] (2) adding sodium carbonate to the mixed solution A at a rate of 0.2 g / min and stirring to adjust the pH of the mixed solution A to 9, adding polyacrylonitrile to the mixed solution A at a rate of 0.2 g / min and stirring to adjust the viscosity of the mixed solution A to 800 cps;

[0050] (3) After the pH and viscosity of the mixed solution A are adjusted, the mixed solution A is placed in an ultrasonic device and ultrasonicated at 50° C. for 1 h under the conditions of 20 kW and 20 kHz. The ultrasonicated liquid is then transferred to a high-temperature reactor and reacted at 100° C. for 24 h. After the reaction is completed, the reactor is taken out and naturally cooled to room temperature to obtain a catalyst precursor.

[0051] (4) The catalyst precursor is repeatedly washed with deionized water until the filtrate is neutral, and then the filter residue is dried at 80°C to obtain a catalyst precursor, and the catalyst precursor is transferred to a tube furnace for calcination. In an argon atmosphere with an air intake of 120 mL / min, the temperature is increased to 350°C at a rate of 1°C / min, and the temperature is kept constant for 3 hours, and then naturally cooled to room temperature to obtain a catalyst carrier;

[0052] (5) Cerium chloride, lanthanum nitrate and catalyst carrier were added to excess deionized water at a mass ratio of 0.05:1, and stirred at a rate of 400 rpm for 8 h. The mixed suspension was filtered and the filter residue was dried at 80 °C. The dried solid was then transferred to a muffle furnace for calcination, and the temperature was increased to 650 °C at a rate of 1 °C / min and kept constant for 3 h. When the temperature dropped to room temperature, a flaky metal composite catalyst was obtained.

[0053] The catalyst synthesized in this example absorbs CO under the following reaction conditions: CO concentration is 1%, H2 concentration is 50%, N2 is the balance gas, the mixed gas flow rate is 50mL / min, and the reaction temperature is 30-300°C. The results show that in the lower temperature window (<200°C), CO maintains a 100% removal effect, the CO selectivity is maintained at about 78%, and has good thermal stability. No catalytic effect is detected within 50 hours, and the CO conversion rate is still maintained at 99.4% at 50 hours.

[0054] Example 3

[0055] A method for preparing a flaky metal composite catalyst comprises the following steps:

[0056] (1) copper nitrate, copper acetate and zinc acetate are added to a toluene solution, wherein the mass ratio of the total mass of copper nitrate and copper acetate to zinc acetate is 5:1 (calculated as oxide), and the mass ratio of the total mass of copper nitrate, copper acetate and zinc acetate to toluene is 0.15:1, and the copper nitrate, copper acetate and zinc acetate are completely dissolved at room temperature to obtain a metal salt solution A, and then ammonium bisulfate is used as a pore-forming agent, and the mass ratio of ammonium bisulfate to toluene is 0.05:1, and ammonium bisulfate is added to the metal salt solution A, and stirred at 60° C. for 4 hours to obtain a mixed solution A after being fully dissolved;

[0057] (2) adding sodium hydroxide to the mixed solution A at a rate of 0.5 g / min and stirring to adjust the pH of the mixed solution A to 10, adding polymethyl methacrylate to the mixed solution A at a rate of 0.5 g / min and stirring to adjust the viscosity of the mixed solution A to 1200 cps;

[0058] (3) After the pH and viscosity of the mixed solution A are adjusted, the mixed solution A is placed in an ultrasonic device and ultrasonicated at 60° C. for 3 h under the conditions of 30 kW and 60 kHz. The ultrasonicated liquid is then transferred to a high-temperature reactor and reacted at 120° C. for 36 h. After the reaction is completed, the reactor is taken out and naturally cooled to room temperature to obtain a catalyst precursor.

[0059] (4) The catalyst precursor is repeatedly washed with deionized water until the filtrate is neutral, and then the filter residue is dried at 120° C. to obtain a catalyst precursor, and the catalyst precursor is transferred to a tube furnace for calcination, and the temperature is increased to 400° C. at a rate of 3° C. / min in a helium atmosphere with an air intake of 150 mL / min, and the temperature is kept constant for 4 hours, and then naturally cooled to room temperature to obtain a catalyst carrier;

[0060] (5) Lanthanum sulfate, lanthanum chloride and the catalyst carrier were added to an excess of deionized water at a mass ratio of 0.05:1, and the mixture was stirred at a rate of 500 rpm for 10 h. The mixed suspension was then filtered, and the filter residue was dried at 120 °C. The dried solid was then transferred to a muffle furnace for calcination, and the temperature was increased to 700 °C at a rate of 3 °C / min and kept constant for 4 h. When the temperature dropped to room temperature, a flaky metal composite catalyst was obtained.

[0061] The catalyst synthesized in this example absorbs CO under the following reaction conditions: CO concentration is 1%, H2 concentration is 50%, N2 is the balance gas, the mixed gas flow rate is 50mL / min, and the reaction temperature is 30-300°C. The results show that in the lower temperature window (<200°C), CO maintains a 100% removal effect, the selectivity of CO is maintained at about 70%, and has good thermal stability. No significant decrease in the catalytic effect is detected within 50 hours, and the conversion rate of CO is 97.2% at 50 hours.

[0062] Example 4

[0063] A method for preparing a flaky metal composite catalyst comprises the following steps:

[0064] (1) copper nitrate, copper sulfate, copper chloride, ferric chloride, ferric acetate and manganese sulfate are added to a chloroform solution, wherein the total mass ratio of copper nitrate, copper sulfate and copper chloride to the total mass ratio of ferric chloride, ferric acetate and manganese sulfate is 3:1 (calculated as oxides), and the mass ratio of copper nitrate, copper sulfate, copper chloride, ferric chloride, ferric acetate and manganese sulfate to chloroform is 0.2:1, stirring at room temperature to completely dissolve copper nitrate, copper sulfate, copper chloride, ferric chloride, ferric acetate and manganese sulfate to obtain a metal salt solution A, and then using carbonamide as a pore-forming agent, according to the mass ratio of carbonamide to chloroform of 0.08:1, adding carbonamide to the metal salt solution A, and stirring at 70°C for 5 hours, after fully dissolving, to obtain a mixed solution A;

[0065] (2) adding sodium hydroxide and sodium bicarbonate (the mass ratio of sodium hydroxide to sodium bicarbonate is 2:1) to the mixed solution A at a rate of 0.8 g / min and stirring, adjusting the pH of the mixed solution A to 10, adding polyacrylamide to the mixed solution A at a rate of 0.8 g / min and stirring, adjusting the viscosity of the mixed solution A to 1500 cps;

[0066] (3) After the pH and viscosity of the mixed solution A are adjusted, the mixed solution A is placed in an ultrasonic device and ultrasonicated at 70° C. for 4 h under the conditions of 50 kW and 100 kHz. The ultrasonicated liquid is then transferred to a high-temperature reactor and reacted at 180° C. for 12 h. After the reaction is completed, the reactor is taken out and naturally cooled to room temperature to obtain a catalyst precursor.

[0067] (4) The catalyst precursor is repeatedly washed with deionized water until the filtrate is neutral, and then the filter residue is dried at 150° C. to obtain a catalyst precursor, and the catalyst precursor is transferred to a tube furnace for calcination. In a nitrogen atmosphere with an air intake of 180 mL / min, the temperature is increased to 450° C. at a rate of 4° C. / min, and the temperature is maintained for 5 h, and then naturally cooled to room temperature to obtain a catalyst carrier;

[0068] (5) Cerium nitrate, cerium chloride and lanthanum nitrate and the catalyst carrier were added to an excess of deionized water in a mass ratio of 0.2:1, and stirred at a rate of 600 rpm for 12 hours. The mixed suspension was then filtered, and the filter residue was dried at 150°C. The dried solid was then transferred to a muffle furnace for calcination, and the temperature was increased to 750°C at a rate of 4°C / min and kept constant for 5 hours. When the temperature dropped to room temperature, a flaky metal composite catalyst was obtained.

[0069] The catalyst synthesized in this example absorbs CO under the following reaction conditions: CO concentration is 1%, H2 concentration is 50%, N2 is the balance gas, the mixed gas flow rate is 50mL / min, and the reaction temperature is 30-300°C. The results show that in the lower temperature window (<200°C), CO maintains a 100% removal effect, the selectivity of CO is maintained at about 73%, and has good thermal stability. No significant decrease in the catalytic effect is detected within 50 hours, and the conversion rate of CO is 98.8% at 50 hours.

[0070] Example 5

[0071] A method for preparing a flaky metal composite catalyst comprises the following steps:

[0072] (1) Add copper nitrate, copper chloride, copper sulfate, copper acetate, ferric nitrate, cobalt sulfate and zinc chloride to an N,N-dimethylamide solution, wherein the total mass ratio of copper nitrate, copper chloride, copper sulfate and copper acetate to the total mass ratio of ferric nitrate, cobalt sulfate and zinc chloride is 2:1 (calculated as oxides), and the mass ratio of copper nitrate, copper chloride, copper sulfate, copper acetate, ferric nitrate, cobalt sulfate and zinc chloride to N,N-dimethylamide is 0.3:1, and stir at room temperature to completely dissolve copper nitrate, copper chloride, copper sulfate, copper acetate, ferric nitrate, cobalt sulfate and zinc chloride to obtain a metal salt solution A, and then use ammonium bicarbonate as a pore-forming agent, according to the mass ratio of ammonium bicarbonate to N,N-dimethylamide of 0.1:1, add ammonium bicarbonate to the metal salt solution A, and stir at 80°C for 5 hours to obtain a mixed solution A after sufficient dissolution;

[0073] (2) adding sodium carbonate and sodium bicarbonate (the mass ratio of sodium carbonate to sodium bicarbonate is 5:1) to the mixed solution A at a rate of 1 g / min and stirring, adjusting the pH of the mixed solution A to 9, adding polyvinyl pyrrolidone to the mixed solution A at a rate of 1 g / min and stirring, adjusting the viscosity of the mixed solution A to 2000 cps;

[0074] (3) After the pH and viscosity of the mixed solution A are adjusted, the mixed solution A is placed in an ultrasonic device and ultrasonicated at 80° C. for 5 h under the conditions of 50 kW and 80 kHz. The ultrasonicated liquid is then transferred to a high-temperature reactor and reacted at 200° C. for 24 h. After the reaction is completed, the reactor is taken out and naturally cooled to room temperature to obtain a catalyst precursor.

[0075] (4) The catalyst precursor is repeatedly washed with deionized water until the filtrate is neutral, and then the filter residue is dried at 150°C to obtain a catalyst precursor, and the catalyst precursor is transferred to a tube furnace for calcination. In an argon atmosphere with an air intake of 200 mL / min, the temperature is increased to 500°C at a rate of 5°C / min, and the temperature is maintained for 5 hours, and then naturally cooled to room temperature to obtain a catalyst carrier;

[0076] (5) Cerium sulfate, lanthanum chloride, lanthanum sulfate and catalyst carrier were added to excess deionized water at a mass ratio of 0.3:1, and stirred at a rate of 300 rpm for 12 hours. The mixed suspension was filtered, and the filter residue was dried at 150°C. The dried solid was then transferred to a muffle furnace for calcination, and the temperature was increased to 800°C at a rate of 5°C / min and kept constant for 5 hours. When the temperature dropped to room temperature, a flaky metal composite catalyst was obtained.

[0077] The catalyst synthesized in this example absorbs CO under the following reaction conditions: the CO concentration is 1%, the H2 concentration is 50%, N2 is the balance gas, the flow rate of the mixed gas is 50 mL / min, and the reaction temperature is 30 - 300 °C. The results show that in the lower temperature window (<200 °C), the removal rate of CO remains 100%, the selectivity of CO is maintained at about 62%, and it has good thermal stability. No obvious decrease in the catalytic effect is detected within 50 h, and the conversion rate of CO at 50 h is 93.6%.

[0078] Comparative Example 1

[0079] The difference between this comparative example and Example 1 is that no pore-forming agent is added in step (1), and the other steps and parameter settings are the same as those in Example 1.

[0080] The catalyst synthesized in this comparative example absorbs CO under the following reaction conditions: the CO concentration is 1%, the H2 concentration is 50%, N2 is the balance gas, the flow rate of the mixed gas is 50 mL / min, and the reaction temperature is 30 - 300 °C. The results show that in the lower temperature window (150 °C < T < 200 °C), the removal rate of CO remains 100%, the selectivity of CO is maintained at about 57%, and its thermal stability is poorer than that of Example 1. The conversion rate of CO at 50 h is 71.2%.

[0081] Comparative Example 2

[0082] The difference between this comparative example and Example 1 is that ultrasonic treatment is not used in step (3), and the other steps and parameter settings are the same as those in Example 1.

[0083] The catalyst synthesized in this comparative example absorbs CO under the following reaction conditions: the CO concentration is 1%, the H2 concentration is 50%, N2 is the balance gas, the flow rate of the mixed gas is 50 mL / min, and the reaction temperature is 30 - 300 °C. The results show that in the lower temperature window (100 °C < T < 200 °C), the removal rate of CO remains 100%, the selectivity of CO is maintained at about 53%, and its thermal stability is poorer than that of Example 1. The conversion rate of CO at 50 h is 85.3%.

[0084] Comparative Example 3

[0085] The difference between this comparative example and Example 1 is that in step (3), hydrothermal reaction is not used, but isothermal heating is carried out (which means aging is carried out at the same temperature as the hydrothermal heating temperature, i.e., 150 °C. The specific operation is to transfer the ultrasonicated liquid to a beaker, seal the beaker mouth (to prevent the solution from volatilizing too fast), and place it in an oven at 150 °C for 12 h), and the other steps and parameter settings are the same as those in Example 1.

[0086] The catalyst synthesized in this comparative example absorbs CO under the following reaction conditions: the CO concentration is 1%, the H2 concentration is 50%, N2 is the balance gas, the flow rate of the mixed gas is 50 mL / min, and the reaction temperature is 30 - 300 °C. The results show that in the lower temperature window (150 °C < T < 200 °C), the removal rate of CO remains 100%, the selectivity of CO is maintained at about 56%, the thermal stability is poorer than that of Example 1, and the conversion rate of CO at 50 h is 74.4%.

[0087] It can be seen from Figure 1 that under the reaction conditions: the CO concentration is 1%, the H2 concentration is 50%, N2 is the balance gas, the flow rate of the mixed gas is 50 mL / min, and the reaction temperature is 0 - 300 °C, the CO conversion rate of the catalyst prepared in Example 1 is basically 100% in the temperature range of 80 - 300 °C, while the CO conversion rate of the catalysts prepared in Comparative Example 1 and Comparative Example 3 reaches 100% at about 150 °C. The CO conversion rates of the catalysts prepared in Comparative Example 1, Comparative Example 2 and Comparative Example 3 start to drop sharply at about 200 °C, and the CO conversion rate at 300 °C is only about 20%.

[0088] The above has introduced this application in detail. Specific examples are used in this article to elaborate on the principle and implementation manner of this application. The description of the above examples is only used to help understand this application and its core idea. It should be pointed out that for those of ordinary skill in the art of this technology, without departing from the principle of this application, several improvements and modifications can be made to this application, and these improvements and modifications also fall within the protection scope of the claims of this application.

Claims

1. A method for preparing a flaky metal composite catalyst, It is characterized in that The steps include: (1) adding a certain amount of a metal compound to an organic solvent, stirring to completely dissolve the metal compound, to obtain a metal salt solution A, then adding a pore-forming agent to the metal salt solution A and stirring at a first preset temperature to obtain a mixed solution A after the metal compound is fully dissolved; (2) adding base A and polymer A to the mixed solution A and stirring evenly; (3) The solution stirred evenly in step (2) is ultrasonically modified under certain conditions, and then transferred to a high-temperature reactor for hydrothermal reaction to obtain a mixed solution B; (4) filtering the mixed solution B and drying the filter residue to obtain a catalyst precursor, and calcining the catalyst precursor to obtain a catalyst carrier; (5) The rare earth metal compound and the catalyst carrier are impregnated in excess according to a certain ratio, stirred to allow the rare earth metal compound to contact and react with the catalyst carrier, and then filtered, dried and calcined in sequence to obtain a sheet-like metal composite catalyst.

2. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (1), the metal compound is a first metal compound and a second metal compound, the first metal compound is one or more of copper nitrate, copper chloride, copper sulfate and copper acetate; the second metal compound is one or more of ferric nitrate, ferric chloride, ferric sulfate, ferric acetate, cobalt nitrate, cobalt chloride, cobalt sulfate, cobalt acetate, manganese nitrate, manganese chloride, manganese sulfate, manganese acetate, zinc nitrate, zinc chloride, zinc sulfate and zinc acetate; the mass ratio of the first metal compound to the second metal compound as oxide is 10:1 to 2:

1.

3. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (1), the organic solvent is N,N-dimethylformamide, acetone, toluene or chloroform; and the mass ratio of the metal compound to the organic solvent is 0.05:1 to 0.3:

1.

4. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (1), the pore-forming agent is one of ammonium bicarbonate, ammonium bisulfate and carbonamide, and the mass ratio of the pore-forming agent to the solvent is 0.01:1 to 0.1:1; the first preset temperature is 40 to 80°C, and the stirring time is 2 to 5 hours.

5. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (2), the addition rate of alkali A and polymer A is 0.1-1 g / min; the alkali A is one or more of sodium hydroxide, sodium carbonate and sodium bicarbonate, and the alkali A is added to adjust the pH so that the pH range of the mixed solution A is 8-10; the polymer A is one of polyacrylonitrile, polyvinyl pyrrolidone, polymethyl methacrylate and polyacrylamide, and the polymer A is added to adjust the viscosity so that the viscosity range of the mixed solution A is 800-2000 cps.

6. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (3), the conditions for ultrasonic modification of the mixed solution A are: ultrasonic power of 20-50 kW, ultrasonic temperature of 40-80° C., ultrasonic time of 1-5 h, and ultrasonic frequency of 20-100 KHz.

7. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (3), the temperature of the hydrothermal reaction is 100-200°C, and the reaction time is 12-36h.

8. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (4), after the mixed solution B is filtered, the filter residue is repeatedly washed with deionized water until the filtrate is neutral, and then dried; the drying temperature is 80 to 150°C.

9. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (4), calcination is carried out in a tubular furnace under anaerobic conditions, with a calcination temperature of 300 to 500° C., a heating rate of 1 to 5° C. / min, and a calcination time of 2 to 5 h; the protective gas during calcination is one of nitrogen, helium and argon, and the protective gas intake rate is 100 to 200 mL / min.

10. The method for preparing the flaky metal composite catalyst according to claim 1, It is characterized in that In step (5), the solvent used for excessive impregnation is deionized water; the rare earth metal compound is one or more of cerium nitrate, cerium chloride, cerium sulfate, lanthanum nitrate, lanthanum chloride and lanthanum sulfate; the mass ratio of the rare earth metal compound to the catalyst carrier is 0.05:1-0.3:1; the stirring rate is 300-600rpm, and the time is 6-12h; the drying temperature is 80-150°C; the calcination is carried out in a muffle furnace, the calcination is aerobic calcination, the calcination temperature is 600-800°C, the heating rate is 1-5°C / min, and the calcination time is 2-5h.

Citation Information

Patent Citations

  • Copper-iron alloy catalyst and preparation and application thereof

    CN116060009A

  • Low-load Pt-based catalyst as well as preparation method and application thereof

    CN117797830A