Catalyst as well as preparation method and application thereof
By modifying the support-supported ruthenium catalyst through polyion liquid, the problem of high cost of heterogeneous catalysts and difficult to separate homogeneous catalysts is solved, and low-cost, high-activity and stable catalyst preparation is achieved, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202310565062.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-19
AI Technical Summary
The existing heterogeneous catalyst raw materials are relatively high, resulting in high cost of heterogeneous catalysts, which is not conducive to large-scale production and application, and homogeneous catalysts are difficult to separate and reuse.
The carrier modified with polyion liquid is used to support the ruthenium catalyst, and the dispersion and specific surface area of the ruthenium are improved by combining vinyl imidazole ionic liquid with SiO2 and Al2O3, thereby enhancing the catalytic activity and stability.
The preparation of low-cost catalysts is realized, which improves catalytic activity and stability, is suitable for large-scale production and reuse, and reduces the risk of ruthenium loss.
Smart Images

Figure BDA0004236469540000081 
Figure BDA0004236469540000083 
Figure BDA0004236469540000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalysis, and in particular relates to a catalyst and a preparation method and application thereof. Background Art
[0002] Carbon dioxide (CO2) is an important component of the atmosphere and the final oxidation / combustion product of carbon and carbon-containing compounds. With the development of society and the consumption of fossil energy, the current concentration of CO2 in the atmosphere is 147% higher than before industrialization, which has caused a series of major environmental problems such as global warming, sea level rise and ocean acidification. At the same time, CO2 is also an important C1 resource with the advantages of safety, non-toxicity, low cost, easy availability and renewability. The recycling of CO2 can promote the sustainable development of carbon resources. The directional conversion of CO2 into bulk and high value-added chemicals through catalytic technology can not only improve the predicament of human beings' long-term dependence on fossil energy, but also effectively reduce the content of CO2 in the air, which is conducive to alleviating the greenhouse effect caused by CO2.
[0003] N-formamides are a class of compounds widely used in organic synthesis, and can be used to synthesize high-value heterocycles, bio-intermediates and drugs. Among them, N,N-dimethylformamide is an important "universal solvent" and is also widely used in industrial production as an important intermediate in organic synthesis, pharmaceutical and pesticide industries. Based on the fact that CO2 is a cheap, non-toxic and renewable C1 resource, and hydrogen (H2) is the cleanest reducing agent, from the perspective of sustainable development, using a mixture of CO2 and H2 as a formylation agent to directly react with amines to prepare various N-formamides is undoubtedly a green and environmentally friendly approach. Although homogeneous N-formylation reactions have the characteristics of high activity, high selectivity and mild reaction conditions, homogeneous catalysts are difficult to separate and reuse, and ligand synthesis is relatively difficult. In contrast, catalysts in heterogeneous N-formylation reactions are easy to separate and recycle. Recently, heterogeneous nitrogen heterocyclic carbene iridium catalysts (Angew. Chem. Int. Ed., 2021, 60, 4125-4132, Highly Efficient and Selective N-Formylation of Amines with CO2 and H2 Catalyzed by Porous Organometallic Polymers; Chem. Asian J., 2018, 13, 3018–3021, N-Formylation of Amines with CO2 and H2 by Using NHC-Iridium Coordination Assemblies as Solid Molecular Catalysts; CN202010077178.1) and phosphine-containing polymer-supported ruthenium catalysts (Chem Sus Chem 2020, 13, 1735-1739, An Efficient and Practical System for the Synthesis of N,N-Dimethylformamide by CO2 Hydrogenation using a Heterogeneous Ru Catalyst: From Batch) have been reported. A method for preparing formamide compounds by hydrogenation of carbon dioxide catalyzed by continuous flow (CF) has been developed, and excellent catalytic activity has been achieved. However, the existing heterogeneous catalyst raw materials are relatively expensive, resulting in a relatively high cost of heterogeneous catalysts, which is not conducive to large-scale production applications. Summary of the invention
[0004] In view of this, the present invention provides a catalyst and a preparation method and application thereof. The catalyst provided by the present invention can catalyze the hydrogenation of carbon dioxide to prepare formamide compounds. At the same time, the cost of preparing the catalyst is low, which is conducive to large-scale production and application.
[0005] In order to solve the above technical problems, the present invention provides a catalyst, comprising a carrier modified with a polyionic liquid and ruthenium loaded on the surface of the carrier modified with the polyionic liquid;
[0006] The polyionic liquid is obtained by polymerization of vinyl imidazole ionic liquid;
[0007] The carrier is SiO2, Al2O3, TiO2, CeO2, Fe2O3, activated carbon or molecular sieve.
[0008] Preferably, the mass percentage of ruthenium in the catalyst is 0.5-10%.
[0009] The mass ratio of the vinyl imidazole ionic liquid to the carrier is 0.1-0.5:1.
[0010] Preferably, the vinyl imidazolium ionic liquid includes one or more of 1-vinyl-3-methylimidazolium bromide, 1-vinyl-3-ethylimidazolium bromide, 1-vinyl-3-butylimidazolium bromide, 1-vinyl-3-hexylimidazolium bromide, 1-vinyl-3-octylimidazole bromide, 1-vinyl-3-dodecylimidazolium bromide, 1-vinyl-3-carboxypropylimidazolium bromide, 1-vinyl-3-carboxymethylimidazolium bromide, 1-vinyl-3-butylimidazolium chloride, 1-vinyl-3-butylimidazolium hexafluorophosphate, 1-vinyl-3-butylimidazolium tetrafluoroborate, 1-vinyl-3-hexylimidazolium tetrafluoroborate and 1-vinyl-3-ethylimidazolium bis(trifluoromethylsulfonyl)imide.
[0011] The present invention also provides a method for preparing the catalyst described in the above technical solution, comprising the following steps:
[0012] The vinyl imidazole ionic liquid, a carrier, an organic solvent and an initiator are mixed to carry out a polymerization reaction to obtain a carrier modified with a polyionic liquid;
[0013] The carrier modified by the polyionic liquid, a ruthenium precursor, a precipitant, a reducing agent and water are mixed and sequentially subjected to deposition precipitation and reduction reaction to obtain the catalyst.
[0014] Preferably, the polymerization reaction temperature is 70-120° C. and the time is 12-36 hours.
[0015] Preferably, the organic solvent includes one or more of dimethyl sulfoxide, acetonitrile, N,N-dimethylformamide, methanol, ethanol, tetrahydrofuran, dioxane and isopropanol; the mass ratio of the organic solvent to the carrier is 2 to 20:1;
[0016] The initiator comprises 2,2'-azobisisobutyronitrile, dibenzoyl peroxide, di-tert-butyl peroxide or tert-butyl perbenzoate; the mass ratio of the initiator to the vinylimidazole ionic liquid monomer is 1 to 10:100.
[0017] Preferably, the ruthenium precursor includes one or more of ruthenium trichloride, potassium chlororuthenate, ruthenium acetylacetonate and ruthenium acetate.
[0018] Preferably, the precipitant comprises one or more of potassium carbonate solution, sodium carbonate solution, potassium hydroxide solution, sodium hydroxide solution and ammonia solution;
[0019] The temperature of the deposition precipitation is 25-100° C. and the time is 1-5 hours.
[0020] Preferably, the reducing agent is one or more of hydrazine hydrate aqueous solution, sodium borohydride aqueous solution and formaldehyde aqueous solution;
[0021] The temperature of the reduction reaction is 30-150° C. and the time is 1-5 hours.
[0022] The present invention also provides the use of the catalyst described in the above technical solution or the catalyst prepared by the preparation method described in the above technical solution in catalyzing the preparation of formamide compounds using amine, carbon dioxide and hydrogen as raw materials.
[0023] The present invention provides a catalyst, including a carrier modified by a polyionic liquid and ruthenium loaded on the surface of the carrier modified by the polyionic liquid; the polyionic liquid is obtained by polymerization of vinylimidazole ionic liquid; the carrier is SiO2, Al2O3, TiO2, CeO2, Fe2O3, activated carbon or molecular sieve. The present invention loads ruthenium on the carrier modified by the polyionic liquid to improve the dispersion of ruthenium, thereby increasing the specific surface area of ruthenium, increasing the catalytic active sites, and improving the catalytic activity of the catalyst. In the present invention, the nitrogen atoms in the polyionic liquid modified on the surface of the catalyst are conducive to the adsorption and activation of carbon dioxide molecules, thereby improving the catalytic activity of the catalyst; at the same time, the coordination between the functional groups of the polyionic liquid and the active component ruthenium avoids the loss of the active component ruthenium and improves the stability of the catalyst.
[0024] The present invention also provides a method for preparing the catalyst described in the above technical solution, comprising the following steps: mixing vinyl imidazole ionic liquid, a carrier, an organic solvent and an initiator for polymerization reaction to obtain a carrier modified by a polyionic liquid; mixing the carrier modified by the polyionic liquid, a ruthenium precursor, a precipitant, a reducing agent and water for deposition precipitation and reduction reaction in sequence to obtain the catalyst. The preparation method provided by the present invention has simple steps, strong controllability and practicality, low cost, and is suitable for large-scale production and application. DETAILED DESCRIPTION
[0025] The invention provides a catalyst, comprising a carrier modified by a polyionic liquid and ruthenium loaded on the surface of the carrier modified by the polyionic liquid.
[0026] In the present invention, the polyionic liquid is obtained by polymerization of vinyl imidazole ionic liquid; the vinyl imidazole ionic liquid preferably includes one or more of 1-vinyl-3-methyl imidazole bromide, 1-vinyl-3-ethyl imidazole bromide, 1-vinyl-3-butyl imidazole bromide, 1-vinyl-3-hexyl imidazole bromide, 1-vinyl-3-octyl imidazole bromide, 1-vinyl-3-dodecyl imidazole bromide, 1-vinyl-3-carboxypropyl imidazole bromide, 1-vinyl-3-carboxymethyl imidazole bromide, 1-vinyl-3-butyl imidazole chloride, 1-vinyl-3-butyl imidazole hexafluorophosphate, 1-vinyl-3-butyl imidazole tetrafluoroborate, 1-vinyl-3-hexyl imidazole tetrafluoroborate and 1-vinyl-3-ethyl imidazole bis(trifluoromethylsulfonyl)imide, more preferably 1-vinyl-3-methyl imidazole bromide, 1 1-vinyl-3-ethylimidazolium bromide, 1-vinyl-3-butylimidazolium bromide, 1-vinyl-3-hexylimidazolium bromide, 1-vinyl-3-octylimidazolium bromide, 1-vinyl-3-dodecylimidazolium bromide, 1-vinyl-3-carboxypropylimidazolium bromide, 1-vinyl-3-carboxymethylimidazolium bromide, 1-vinyl-3-butylimidazolium chloride, 1-vinyl-3-butylimidazolium hexafluorophosphate, 1-vinyl-3-butylimidazolium tetrafluoroborate, 1-vinyl-3-hexylimidazolium tetrafluoroborate or 1-vinyl-3-ethylimidazolium bistrifluoromethylsulfonyl imide, and more preferably 1-vinyl-3-butylimidazolium bromide, 1-vinyl-3-hexylimidazolium tetrafluoroborate, 1-vinyl-3-octylimidazolium bromide, 1-vinyl-3-carboxypropylimidazolium bromide or 1-vinyl-3-butylimidazolium hexafluorophosphate.
[0027] In the present invention, the carrier is SiO2, Al2O3, TiO2, CeO2, Fe2O3, activated carbon or molecular sieve, preferably SiO2, Al2O3, TiO2 or activated carbon. In the present invention, the molecular sieve is preferably MCM-41 molecular sieve.
[0028] In the present invention, the mass ratio of the vinylimidazole ionic liquid to the carrier is preferably 0.1 to 0.5:1, more preferably 0.2 to 0.4:1.
[0029] In the present invention, the mass percentage of ruthenium in the catalyst is preferably 0.5-10%, more preferably 1-5%.
[0030] The present invention also provides a method for preparing the catalyst described in the above technical solution, comprising the following steps:
[0031] The vinyl imidazole ionic liquid, a carrier, an organic solvent and an initiator are mixed to carry out a polymerization reaction to obtain a carrier modified with a polyionic liquid;
[0032] The carrier modified by the polyionic liquid, a ruthenium precursor, a precipitant, a reducing agent and water are mixed and sequentially subjected to deposition precipitation and reduction reaction to obtain the catalyst.
[0033] The present invention mixes vinyl imidazole ionic liquid, carrier, organic solvent and initiator for polymerization reaction to obtain a carrier modified with polyionic liquid. In the present invention, the organic solvent preferably includes one or more of dimethyl sulfoxide (DMSO), acetonitrile, N,N-dimethylformamide (DMF), methanol, ethanol, tetrahydrofuran, dioxane and isopropanol, and more preferably N,N-dimethylformamide, tetrahydrofuran or dioxane. In the present invention, when the organic solvent includes two or more of the above-mentioned specific substances, the present invention has no special requirements on the ratio of the specific substances, and any ratio can be used.
[0034] In the present invention, the mass ratio of the organic solvent to the carrier is preferably 2 to 20:1, more preferably 10 to 15:1.
[0035] In the present invention, the initiator preferably includes 2,2'-azobisisobutyronitrile (AIBN), dibenzoyl peroxide, di-tert-butyl peroxide or tert-butyl perbenzoate, more preferably 2,2'-azobisisobutyronitrile or dibenzoyl peroxide.
[0036] In the present invention, the mass ratio of the initiator to the vinylimidazole ionic liquid monomer is preferably 1 to 10:100, more preferably 8 to 10:100.
[0037] In the present invention, the mass ratio of the carrier to the vinylimidazole ionic liquid is preferably 1:0.1-0.5, more preferably 1:0.2-0.4.
[0038] In the present invention, the mixing is preferably carried out under stirring conditions, and the stirring time is preferably 0.4 to 0.6 hours, more preferably 0.5 hours. The present invention has no special requirements on the stirring speed, as long as the mixing is uniform.
[0039] In the present invention, the polymerization reaction temperature is preferably 70 to 120° C., more preferably 80 to 100° C.; the polymerization reaction time is preferably 12 to 36 hours, more preferably 24 to 48 hours.
[0040] In the present invention, the polymerization reaction is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen or an inert gas, more preferably nitrogen.
[0041] In the present invention, the vinyl imidazole ionic liquid self-polymerizes under the above polymerization conditions to form a polyionic liquid.
[0042] In the present invention, after the polymerization reaction, it is preferred that the method further comprises: subjecting the system after the polymerization reaction to solid-liquid separation, washing the solid obtained by the solid-liquid separation and then drying. In the present invention, the solid-liquid separation is preferably filtration; the present invention has no special requirements for the filtration, and the conventional method in the art can be used. In the present invention, the washing is preferably performed by acetone. In the present invention, the drying temperature is preferably 55 to 65°C, more preferably 60°C; the drying time is preferably 10 to 14h, more preferably 12h.
[0043] After obtaining the polyionic liquid modified carrier, the present invention mixes the polyionic liquid modified carrier, ruthenium precursor, precipitant, reducing agent and water to sequentially perform deposition precipitation and reduction reaction to obtain the catalyst. In the present invention, the mixing preferably includes the following steps:
[0044] dissolving a ruthenium precursor in a portion of water to obtain a ruthenium precursor solution;
[0045] first mixing the carrier modified with a polyionic liquid and the remaining water to obtain a dispersion of the carrier modified with a polyionic liquid;
[0046] The dispersion of the polyionic liquid-modified carrier and the ruthenium precursor solution are mixed for the second time to obtain a second mixed solution;
[0047] adding a precipitant dropwise to the second mixed solution for sedimentation;
[0048] The reducing agent is added dropwise to the sedimentation system to carry out a reduction reaction.
[0049] The present invention dissolves a ruthenium precursor in part of water to obtain a ruthenium precursor solution. In the present invention, the ruthenium precursor preferably includes one or more of ruthenium trichloride, potassium chlororuthenate, ruthenium acetylacetonate and ruthenium acetate, more preferably ruthenium trichloride, ruthenium acetylacetonate or ruthenium acetate. In the present invention, the mass concentration of the ruthenium precursor solution is preferably 4 to 6 mg / mL, more preferably 5 mg / mL.
[0050] The present invention has no particular limitation on the dissolution, as long as the dissolution is complete.
[0051] After obtaining the ruthenium precursor solution, the present invention first mixes the polyionic liquid-modified carrier and the remaining water to obtain a dispersion of the polyionic liquid-modified carrier. In the present invention, the mass ratio of the polyionic liquid-modified carrier to the remaining water is preferably 0.8 to 1.2:50, more preferably 1:50. In the present invention, the stirring time is preferably 8 to 12 minutes, more preferably 10 minutes. The present invention has no special requirements for the stirring speed, as long as it can be mixed evenly.
[0052] After obtaining the dispersion of the carrier modified by the polyionic liquid, the present invention secondly mixes the dispersion of the carrier modified by the polyionic liquid with the ruthenium precursor solution to obtain a second mixed solution. In the present invention, the volume ratio of the dispersion of the carrier modified by the polyionic liquid to the ruthenium precursor solution is preferably 48 to 52:1, more preferably 50:1. In the present invention, the second mixing is preferably carried out under stirring, and the stirring time is preferably 2 to 4 hours, more preferably 3 hours.
[0053] After obtaining the second mixed solution, the present invention drips a precipitant into the second mixed solution for sedimentation precipitation. In the present invention, the precipitant preferably includes one or more of potassium carbonate solution, sodium carbonate solution, potassium hydroxide solution, sodium hydroxide solution and ammonia water, more preferably sodium carbonate solution, sodium hydroxide solution or ammonia water. In the present invention, the mass concentration of the precipitant is preferably 5-50%, more preferably 10-20%. In the present invention, the pH value of the second mixed solution to which the precipitant is dripped is preferably 10-12, more preferably 11. The present invention has no special limitation on the amount of the precipitant, as long as the desired pH value can be reached.
[0054] In the present invention, the temperature of the deposition precipitation is preferably 25 to 100°C, more preferably 30 to 50°C; the time of the deposition precipitation is preferably 1 to 5 hours, more preferably 2 to 4 hours. In the present invention, the deposition precipitation is preferably accompanied by stirring. The present invention has no special requirements for the stirring, as long as the reaction can be completed. In the present invention, the ruthenium precursor and the precipitant react to generate a ruthenium precipitate attached to the surface of the carrier modified with the polyionic liquid.
[0055] After the deposition and precipitation, the present invention drips a reducing agent into the system after the deposition and precipitation to carry out a reduction reaction. In the present invention, the reducing agent is preferably one or more of a hydrazine hydrate aqueous solution, a sodium borohydride aqueous solution and a formaldehyde aqueous solution, and more preferably a sodium borohydride aqueous solution or a formaldehyde aqueous solution. In the present invention, the mass concentration of the reducing agent is preferably 5 to 40%, more preferably 10 to 20%. In the present invention, the molar ratio of the reducing component to ruthenium in the reducing agent is preferably 2 to 100:1, more preferably 10 to 50:1.
[0056] In the present invention, the temperature of the reduction reaction is preferably 30 to 150°C, more preferably 80 to 100°C; the time of the reduction reaction is preferably 1 to 5 hours, more preferably 2 to 4 hours. In the present invention, the reduction reaction is preferably accompanied by stirring. The present invention has no special requirements for the stirring, as long as the reaction can be completed.
[0057] The present invention reduces trivalent ruthenium in the ruthenium precipitate into simple ruthenium through reduction.
[0058] In the present invention, after the reduction reaction, it is preferred that the following steps are further performed: solid-liquid separation of the system after the reduction reaction, and the solid obtained by the solid-liquid separation is washed with water until it becomes neutral and then dried. In the present invention, the solid-liquid separation is preferably centrifugation; the speed of the centrifugation is preferably 7500-8500 r / min, more preferably 8000 r / min; the time of the centrifugation is preferably 0.8-1.2 min, more preferably 1 min. In the present invention, the water used for washing is preferably deionized water. In the present invention, the drying is preferably vacuum drying; the temperature of the vacuum drying is preferably 75-85°C, more preferably 80°C; the time of the vacuum drying is preferably 10-14 h, more preferably 12 h.
[0059] The present invention also provides the use of the catalyst described in the above technical solution or the catalyst prepared by the preparation method described in the above technical solution in catalyzing the preparation of formamide compounds using amine, carbon dioxide and hydrogen as raw materials. In the present invention, the method for preparing formamide compounds using amine, carbon dioxide and hydrogen as raw materials preferably includes the following steps:
[0060] Amine compounds, carbon dioxide, hydrogen, a catalyst and an organic solvent are mixed to carry out N-formylation reaction to obtain formamide compounds.
[0061] In the present invention, the amine compound preferably has a structure shown in Formula 1:
[0062]
[0063] In the present invention, R 1 Preferably, hydrogen, substituted or unsubstituted C1-C 20 Alkyl, substituted or unsubstituted C4-C 10 Cycloalkyl, substituted or unsubstituted C6-C 24 Aryl or heteroaryl, substituted or unsubstituted C7-C 25 Arylalkyl or heteroarylalkyl, -(CH2) n -OR 3 or -(CH2) n -NR 4 R 5; Wherein, n is any integer from 1 to 8.
[0064] In the present invention, R 2 Preferably, it is a substituted or unsubstituted C1-C 20 Alkyl, substituted or unsubstituted C4-C 10 Cycloalkyl, substituted or unsubstituted C6-C 24 Aryl or heteroaryl, substituted or unsubstituted C7-C 25 Arylalkyl or heteroarylalkyl, -(CH2) m -OR 3 or -(CH2) m -NR 4 R 5 , where m is any integer from 1 to 8.
[0065] In the present invention, R 1 With R 2 Can be linked to substituted or unsubstituted C4-C 10 Cycloalkyl.
[0066] In the present invention, R 3 , R 4 , R 5 Preferably independently: hydrogen, substituted or unsubstituted C1-C 20 Alkyl, substituted or unsubstituted C6-C 24 Aryl, substituted or unsubstituted C7-C 25 Arylalkyl or heteroaryl, where R 4 With R 5 Can be linked to substituted or unsubstituted C3-C 10 Cycloalkyl, C6-C 24 Aryl or heteroaryl.
[0067] In the present invention, the term "substituted" refers to that one or more hydrogen atoms in the group are replaced by a substituent selected from the group consisting of halogen, C1-C4 alkyl, C1-C4 haloalkyl, C2-C6 alkenyl, C2-C6 alkynyl, C1-C6 alkoxy, hydroxyl, amine or thiol.
[0068] In the present invention, the amine compound is preferably
[0069] In the present invention, the organic solvent is preferably one or more of N,N-dimethylformamide (DMF), tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, ethylene glycol dimethyl ether, tert-butyl methyl ether, benzene, toluene, xylene, methanol, ethanol, isopropanol and tert-butanol.
[0070] In the present invention, the molar ratio of the amine compound to the catalyst is preferably 1:0.01-0.5; the molar amount of the amine compound to the volume ratio of the organic solvent is preferably 0.01-1 mmol:1 mL.
[0071] In the present invention, the hydrogen pressure in the N-formylation reaction system is preferably 0.5-6 MPa, and the carbon dioxide pressure is preferably 0.5-6 MPa.
[0072] In the present invention, the temperature of the N-formylation reaction is preferably 80 to 200° C., more preferably 100 to 150° C.; the time of the N-formylation reaction is preferably 2 to 48 hours, more preferably 5 to 40 hours.
[0073] In the present invention, when the amine compound is dimethylamine or its equivalent dimethylamine carbon dioxide, the formamide compound is N,N-dimethylformamide.
[0074] In the present invention, after the catalytic reaction of the catalyst, it is preferred to perform solid-liquid separation on the system after the catalytic reaction, and the solid obtained by the solid-liquid separation is washed and dried to obtain a recovered catalyst. In the present invention, the solid-liquid separation is preferably centrifugal. The present invention has no special requirements for the centrifugation, as long as solid-liquid separation can be achieved. In the present invention, the washing preferably includes methanol washing and acetone washing in sequence. In the present invention, the number of methanol washings is preferably 2 to 4 times, more preferably 3 times; the volume of methanol used for each methanol washing is 8 mL. In the present invention, the number of acetone washings is preferably 1 to 2 times, more preferably 1 time; the volume of acetone used for each acetone washing is 8 mL. In the present invention, the drying is preferably exposed to air at room temperature to dry.
[0075] The catalyst provided by the present invention exhibits excellent catalytic performance and good cycle stability in the N-formylation reaction of amines with carbon dioxide and hydrogen, and can synthesize N-formamide compounds with a high yield. The catalyst provided by the present invention has the advantages of simple preparation method, low catalyst cost, large-scale operation, suitability for large-scale industrial production, high stability, excellent catalytic performance, strong practicality, etc., and the catalyst is easy to separate and can be reused.
[0076] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0077] Example 1
[0078] Under an inert atmosphere, 1.0 g of Al2O3, 0.2 g of 1-vinyl-3-butylimidazolium bromide, 20 mL of tetrahydrofuran and 16.4 mg of azobisisobutyronitrile were stirred in a hydrothermal reactor at 25° C. for 0.5 h; the polymerization reaction was carried out at 100° C. for 24 h and then filtered. The filtered solid was washed three times with 20 mL of tetrahydrofuran and then vacuum dried at 60° C. for 12 h to obtain a poly-1-vinyl-3-butylimidazolium bromide-modified alumina carrier;
[0079] 0.5 g of poly 1-vinyl-3-butylimidazole bromide modified alumina carrier was dispersed in 25 mL of deionized water and stirred for 10 min, then mixed with 0.5 mL of RuCl3 solution with a mass concentration of 5 mg / mL and stirred for 3 h to obtain a second mixed solution; a NaOH solution with a mass concentration of 15% was added dropwise to the second mixed solution to adjust the pH value of the system to 11, and precipitated at 25°C (with stirring) for 3 h; 0.25 mL of formaldehyde aqueous solution with a mass concentration of 15% was added dropwise to the system after precipitation, and after the addition was completed, a reduction reaction was carried out at 80°C (with stirring) for 4 h, and then centrifuged at a speed of 8000 r / min for 1 min, and the solid obtained by centrifugation was washed with deionized water, washed to neutrality, and then vacuum dried at 80°C for 12 h to obtain a polyionic liquid modified alumina supported ruthenium catalyst.
[0080] Example 2
[0081] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by SiO2.
[0082] Example 3
[0083] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by TiO2.
[0084] Example 4
[0085] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by CeO2.
[0086] Example 5
[0087] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by Fe2O3.
[0088] Example 6
[0089] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by activated carbon.
[0090] Example 7
[0091] The catalyst was prepared according to the method of Example 1, except that Al2O3 was replaced by MCM-41 molecular sieve.
[0092] Example 8
[0093] The catalyst was prepared according to the method of Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was replaced by 0.4 g of 1-vinyl-3-octylimidazolium bromide.
[0094] Example 9
[0095] The catalyst was prepared according to the method of Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was replaced by 0.3 g of 1-vinyl-3-carboxypropylimidazolium bromide.
[0096] Example 10
[0097] The catalyst was prepared according to the method of Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was replaced by 0.2 g of 1-vinyl-3-butylimidazolium hexafluorophosphate.
[0098] Embodiment 11
[0099] The catalyst was prepared according to the method of Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was replaced by 0.2 g of 1-vinyl-3-hexylimidazolium tetrafluoroborate.
[0100] Example 12
[0101] The catalyst was prepared according to the method of Example 1, except that the RuCl3 solution was replaced by an aqueous solution of ruthenium acetylacetonate.
[0102] Example 13
[0103] The catalyst was prepared according to the method of Example 1, except that the RuCl3 solution was replaced by a ruthenium acetate aqueous solution.
[0104] Embodiment 14
[0105] The catalyst was prepared according to the method of Example 1, except that the tetrahydrofuran organic solvent was replaced by N,N-dimethylformamide.
[0106] Embodiment 15
[0107] The catalyst was prepared according to the method of Example 1, except that the tetrahydrofuran organic solvent was replaced by dioxane.
[0108] Example 16
[0109] The catalyst was prepared according to the method of Example 1, except that the NaOH solution precipitant was replaced by a sodium carbonate aqueous solution.
[0110] Embodiment 17
[0111] The catalyst was prepared according to the method of Example 1, except that the NaOH solution precipitant was replaced by ammonia water with a mass concentration of 25%; and the formaldehyde aqueous solution reducing agent was replaced by sodium borohydride aqueous solution.
[0112] Embodiment 18
[0113] The catalyst was prepared according to the method of Example 1, except that the polymerization reaction conditions (100° C., 24 h) were replaced by 80° C., 48 h; and the azobisisobutyronitrile initiator was replaced by dibenzoyl peroxide.
[0114] Comparative Example 1
[0115] In Comparative Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was not added to modify the carrier and the polymerization reaction was not carried out, the rest of the implementation process was the same as that of Example 1. The obtained alumina-supported ruthenium catalytic material was recorded as Comparative Catalyst A.
[0116] Comparative Example 2
[0117] In Comparative Example 2, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was not added to modify the carrier and the polymerization reaction was not carried out, the rest of the implementation process was the same as that of Example 2. The obtained silica-supported ruthenium catalytic material was recorded as Comparative Catalyst B.
[0118] Comparative Example 3
[0119] In Example 1, except that 0.2 g of 1-vinyl-3-butylimidazolium bromide was not added to modify the carrier and the polymerization reaction was not carried out, the rest of the implementation process was the same as that of Example 3. The obtained titanium dioxide supported ruthenium catalytic material was recorded as comparative catalyst C.
[0120] The catalysts prepared in Examples 1 to 18 and Comparative Examples 1 to 3 were used to catalyze the N-formylation reaction with dimethylamine, carbon dioxide and hydrogen as raw materials to illustrate the catalytic performance of different catalysts; the specific steps were: 2.68 g (20 mmol, equivalent to 40 mmol dimethylamine) of dimethylammonium·dimethyl (DIMCARB), 40 mg of catalyst and 4 mL of methanol were added to a 100 mL high-pressure reactor equipped with a magnetic stirrer; after sealing the high-pressure reactor, it was replaced with carbon dioxide gas 3 times, and then filled with 3 MPa of carbon dioxide, and then 3 MPa of hydrogen was filled into the high-pressure reactor to a total pressure of 6 MPa; the reaction was carried out at 140° C. for 24 h to obtain N,N-dimethylformamide; after the reaction was completed, the reactor was cooled to room temperature and the pressure was slowly released, 20 mL of methanol was added, and then mesitylene (336 mg, 2 mmol) was added to the reaction system as 1 The internal standard of H NMR analysis was used to determine the yield. The catalytic performance data of different catalysts are shown in Table 1.
[0121] Table 1 Catalytic performance of the catalysts of Examples 1 to 18 and Comparative Examples 1 to 3
[0122]
[0123]
[0124] It can be seen from Table 1 that the catalyst provided by the present invention has good catalytic performance for preparing formamide compounds using amine, carbon dioxide and hydrogen as raw materials.
[0125] Taking the catalyst prepared in Example 1 as an example, the reusability of the ruthenium catalyst supported on a polyionic liquid modified carrier in catalyzing the N-formylation reaction of dimethylamine with CO2 / H2 was verified.
[0126] In a 100mL autoclave equipped with a magnetic stirrer, add 2.68g (20mmol, equivalent to 40mmol dimethylamine) of dimethylammonium·dimethyl (DIMCARB), 40mg of catalyst and 4mL of methanol; after sealing the autoclave, replace it with CO2 gas 3 times, fill it with 3MPa of CO2 and 3MPa of H2; react at 140℃ for 24h. After the reaction is completed, cool the autoclave to room temperature and slowly release the pressure. Add 20mL of methanol to dilute the reaction mixture, and then add 336mg (2mmol) of trimethoxybenzene as 1 The internal standard of H NMR analysis was used to determine the yield. The reaction solution was then transferred to a centrifuge tube and centrifuged to obtain the catalyst, which was washed three times with 8 mL of methanol and once with 8 mL of acetone. After being exposed to air at room temperature to dry, it was directly placed in a kettle for the next reuse. The reaction data of the catalyst reuse are shown in Table 2.
[0127] Table 2 Catalyst repeated catalytic performance of Example 1
[0128] Use times Product yield (%) first 98 Second time 98 The third time 98 Fourth 97 Fifth 97 Sixth 97 Seventh 96 Eighth 96 Ninth 95 The tenth time 95
[0129] It can be seen from Table 2 that the catalytic material prepared by the present invention can be recycled and reused, and after being reused ten times, it still has the same catalytic activity as when it was initially used.
[0130] According to the above method, 20 mmol of different amines were used to replace 40 mmol of dimethylammonium·dimethyl, and 20 mg of the catalyst prepared in Example 1 was used for catalysis to prepare formamide compounds. The specific types of amine compounds and prepared formamide compounds are listed in Table 3. The yield of formamide compounds was detected according to the above method, and the results are listed in Table 3.
[0131] Table 3 Catalytic performance of the catalyst of Example 1 in the N-formylation reaction of different amines with CO2 / H2
[0132]
[0133]
[0134] It can be seen from Table 3 that the catalyst prepared by the present invention can be applied to the N-formylation reaction of different amines with CO2 / H2, and all exhibit high catalytic activity.
[0135] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A catalyst, characterized in that It comprises a carrier modified by a polyionic liquid and ruthenium loaded on the surface of the carrier modified by the polyionic liquid; The polyionic liquid is obtained by polymerization of vinyl imidazole ionic liquid; The carrier is SiO2, Al2O3, TiO2, CeO2, Fe2O3, activated carbon or molecular sieve.
2. The catalyst according to claim 1, characterized in that The mass percentage of ruthenium in the catalyst is 0.5-10% The mass ratio of the vinyl imidazole ionic liquid to the carrier is 0.1-0.5:
1.
3. The catalyst according to claim 1, characterized in that The vinyl imidazolium ionic liquid includes one or more of 1-vinyl-3-methylimidazolium bromide, 1-vinyl-3-ethylimidazolium bromide, 1-vinyl-3-butylimidazolium bromide, 1-vinyl-3-hexylimidazolium bromide, 1-vinyl-3-octylimidazole bromide, 1-vinyl-3-dodecylimidazolium bromide, 1-vinyl-3-carboxypropylimidazolium bromide, 1-vinyl-3-carboxymethylimidazolium bromide, 1-vinyl-3-butylimidazolium chloride, 1-vinyl-3-butylimidazolium hexafluorophosphate, 1-vinyl-3-butylimidazolium tetrafluoroborate, 1-vinyl-3-hexylimidazolium tetrafluoroborate and 1-vinyl-3-ethylimidazolium bis(trifluoromethylsulfonyl)imide.
4. The method for preparing the catalyst according to any one of claims 1 to 3, comprising the following steps: The vinyl imidazole ionic liquid, a carrier, an organic solvent and an initiator are mixed to carry out a polymerization reaction to obtain a carrier modified with a polyionic liquid; The carrier modified by the polyionic liquid, a ruthenium precursor, a precipitant, a reducing agent and water are mixed and sequentially subjected to deposition precipitation and reduction reaction to obtain the catalyst.
5. The preparation method according to claim 4, characterized in that: The polymerization reaction temperature is 70-120° C. and the reaction time is 12-36 hours.
6. The preparation method according to claim 4 or 5, characterized in that: The organic solvent includes one or more of dimethyl sulfoxide, acetonitrile, N,N-dimethylformamide, methanol, ethanol, tetrahydrofuran, dioxane and isopropanol; the mass ratio of the organic solvent to the carrier is 2 to 20:1; The initiator comprises 2,2'-azobisisobutyronitrile, dibenzoyl peroxide, di-tert-butyl peroxide or tert-butyl perbenzoate; the mass ratio of the initiator to the vinylimidazole ionic liquid monomer is 1 to 10:
100.
7. The preparation method according to claim 4, characterized in that: The ruthenium precursor includes one or more of ruthenium trichloride, potassium chlororuthenate, ruthenium acetylacetonate and ruthenium acetate.
8. The preparation method according to claim 4, characterized in that: The precipitant comprises one or more of potassium carbonate solution, sodium carbonate solution, potassium hydroxide solution, sodium hydroxide solution and ammonia solution; The temperature of the deposition precipitation is 25-100° C. and the time is 1-5 hours.
9. The preparation method according to claim 4, characterized in that: The reducing agent is one or more of hydrazine hydrate aqueous solution, sodium borohydride aqueous solution and formaldehyde aqueous solution; The temperature of the reduction reaction is 30-150° C. and the time is 1-5 hours.
10. Use of the catalyst according to any one of claims 1 to 3 or the catalyst prepared by the preparation method according to any one of claims 4 to 9 in catalyzing the preparation of formamide compounds using amine, carbon dioxide and hydrogen as raw materials.
Citation Information
Patent Citations
Method for loading high-dispersion precious metals and alloy nanoparticles on surface of carbon nanotube
CN105771971A
Preparation and application of phenolic resin modified carrier loaded metal catalyst
CN109395784A
Ethylene carbonate hydrogenation heterogeneous catalyst as well as preparation method and application thereof
CN110975939A
Nitrogen-doped carbon-loaded ruthenium monatomic catalyst as well as preparation method and application thereof
CN112387295A