Method for preparing catalyst from landfill leachate and copper anode slime

A highly efficient catalyst was prepared by calcining sulfuric acid solution with copper anode mud and reacting it with landfill leachate and red mud, which solved the problem of landfill leachate and copper anode mud treatment, and achieved efficient removal of pollutants and resource utilization.

CN118988417APending Publication Date: 2024-11-22CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411103570.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the effective treatment and resource utilization of landfill leachate and copper anode sludge, resulting in environmental pollution and high treatment costs.

Method used

A highly efficient catalyst was prepared by mixing and roasting sulfuric acid solution with copper anode mud, mixing landfill leachate with roasted anode mud, and then reacting it with red mud to form a multi-component mixture, followed by hydrothermal treatment.

Benefits of technology

The prepared catalyst can efficiently remove COD, total phosphorus and ammonia nitrogen pollutants from landfill leachate, reduce treatment costs, and realize the resource utilization of waste and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988417A_ABST
    Figure CN118988417A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a catalyst from landfill leachate and copper anode slime, and the method effectively solves the problem of treatment of the two wastes by converting the landfill leachate and the copper anode slime into the catalyst. The pollution of the waste to the environment can be reduced, the waste treatment cost can be reduced, and contribution is made to the environmental protection cause. According to the method, the preparation process is simple, only the copper anode mud, the red mud and the landfill leachate are needed as raw materials, useful components in waste are fully utilized, and input of the raw materials is reduced. The prepared catalyst can be applied to various chemical reactions, the reaction efficiency is improved, the energy consumption is reduced, greater economic benefits are brought to enterprises, and beneficial reference is provided for resource utilization of other wastes. The prepared catalytic material can efficiently remove COD (Chemical Oxygen Demand), ammonia nitrogen and total phosphorus pollutants in the concentrated landfill leachate in a photocatalytic environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of waste resource utilization, and in particular relates to a method for preparing a catalyst by utilizing garbage leachate and copper anode mud. Background Art

[0002] With the rapid development of society, waste treatment has become an important issue in the field of environmental protection. As two common wastes, the treatment and resource utilization of landfill leachate and copper anode mud have always attracted much attention. Landfill leachate is a liquid waste generated during landfill or incineration, which contains a large amount of organic pollutants and salt. Copper anode mud is a solid waste generated during the electrolytic copper refining process, which is rich in precious metals and other valuable elements. If these two types of waste are not properly handled, they will cause serious pollution to the environment. By converting landfill leachate and copper anode mud into catalysts, a resource recycling model of turning waste into treasure is realized. This model can not only reduce dependence on limited natural resources, but also reduce production costs and promote sustainable development. This also provides a useful reference for the resource utilization of other types of waste.

[0003] Both landfill leachate and copper anode mud contain abundant metal elements and compounds, which can be used as active components or carriers in the catalyst preparation process. Through reasonable preparation processes, such as impregnation method, coprecipitation method, etc., these substances can be converted into catalysts with high catalytic activity. Transition metal oxides show high catalytic activity in many chemical reactions, and copper anode mud is rich in copper, silver and other metal elements, which are typical representatives of transition metals. These metal elements can form metal oxides with high catalytic activity after proper treatment. Organic and inorganic substances in landfill leachate can also provide abundant active sites for catalysts, thereby enhancing their catalytic performance. Summary of the invention

[0004] Purpose of the invention: The first purpose of the present invention is to provide a method for preparing a catalyst using landfill leachate and copper anode mud. The second purpose of the present invention is to provide the application of the catalyst prepared by the above method.

[0005] Technical solution: The present invention provides a method for preparing a catalyst using landfill leachate and copper anode mud, comprising the following steps:

[0006] (1) mixing sulfuric acid solution and copper anode mud, stirring evenly, to obtain sulfuric acid mixed with anode mud;

[0007] (2) roasting the sulfuric acid-mixed anode mud to obtain roasted anode mud;

[0008] (3) mixing the landfill leachate and the roasted anode mud, stirring them evenly to obtain leachate slurry;

[0009] (4) mixing the red mud and the leachate slurry and stirring them evenly to obtain a red mud leachate slurry;

[0010] (5) drying the red mud percolation slurry and then roasting it to obtain activated mud;

[0011] (6) grinding the activated clay into powder, mixing water and the activated clay powder, and granulating to obtain activated clay granules;

[0012] (7) Adding the activated mud particles into a reactor for hydrothermal reaction to obtain a catalyst.

[0013] Furthermore, the liquid-to-solid ratio of the sulfuric acid solution and the copper anode mud in step (1) is 0.15-0.45:1 mL / g, and the concentration of the sulfuric acid solution is 4-16 M.

[0014] Furthermore, the calcination time in step (2) is 0.5 to 4.5 hours, and the calcination temperature is 550 to 750°C.

[0015] Furthermore, the liquid-to-solid ratio of the landfill leachate and the roasted anode mud in step (3) is 2 to 6:1 mL / g, and the stirring time is 0.25 to 2.75 hours.

[0016] Furthermore, the mass ratio of the red mud to the leachate slurry in step (4) is 15 to 45:100.

[0017] Furthermore, the calcination temperature in step (5) is 550-850° C., and the calcination time is 0.5-4.5 hours.

[0018] Furthermore, the liquid-to-solid ratio of water and activated mud powder in step (6) is 0.25-0.55:1 mL / g.

[0019] Furthermore, the temperature of the hydrothermal reaction in step (7) is 180 to 360° C., and the hydrothermal reaction time is 1 to 5 hours.

[0020] The present invention also provides an application of the catalyst prepared by the above method in the treatment of landfill leachate.

[0021] Furthermore, the application is to remove one or more of COD, total phosphorus and ammonia nitrogen in landfill leachate.

[0022] Reaction mechanism: The sulfuric acid-doped anode mud is roasted, and the sulfides, selenides, tellurides, and oxides of metals such as gold, silver, copper, and nickel in the sulfuric acid-doped anode mud react with sulfuric acid and are converted into water-soluble sulfates. The selenides are oxidized to selenium dioxide and selenate, and selenium dioxide and silver chloride are separated from the solid by sublimation and volatilization. The landfill leachate and the roasted anode mud are mixed, and the water-soluble metal sulfates in the roasted anode mud are dissolved into the landfill leachate and react with organic pollutants, ammonia nitrogen, phosphates and other pollutants in the landfill leachate to form a mixed slurry containing metal organic complexes, metal ammonium sulfate salts, and metal phosphates (precipitates). The red mud and leachate slurry are mixed, and the alkaline substances and minerals containing aluminum, titanium, iron, silicon, and calcium in the red mud are adsorbed and react with metal organic complexes, metal ammonium sulfate salts, and metal phosphates (precipitates) to form a multi-component mixture. The red mud leachate is dried and then roasted. During the roasting process, organic pollutants are pyrolyzed to form carbon-based materials, while ammonia nitrogen pollutants are oxidized. The inorganic salts introduced into the landfill leachate induce the multi-component mixture to further undergo oxidation reaction and phase transformation on the surface of the carbon-based material to form activated mud containing a variety of catalytic materials such as gold, copper, silver, iron, tellurium, and titanium. The activated mud particles are added to the reactor for hydrothermal reaction. The aluminosilicates in the red mud combine with inorganic salts such as sodium, calcium, and magnesium to undergo geopolymerization self-excitation reaction to form geopolymer gel, which fully wraps the multi-component mixed catalytic material. At the same time, the free radical active substances generated during the hydrothermal reaction can further enhance the catalytic activity of the catalytic material.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following outstanding and significant advantages: The present invention effectively solves the treatment problem of garbage leachate and copper anode mud by converting these two types of waste into catalysts. It can not only reduce the pollution of waste to the environment, but also reduce the cost of waste treatment, and contribute to the cause of environmental protection. This method has a simple preparation process, and the required raw materials are only copper anode mud, red mud, and garbage leachate. It makes full use of the useful components in the waste and reduces the input of raw materials. The prepared catalyst can be used in various chemical reactions to improve reaction efficiency, reduce energy consumption, bring greater economic benefits to enterprises, and provide a useful reference for the resource utilization of other wastes. The catalytic material prepared by the present invention can efficiently remove COD, ammonia nitrogen and total phosphorus pollutants in concentrated garbage leachate under a photocatalytic environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figure is a flow chart of the processing method of the present invention. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0026] Landfill leachate: The landfill leachate used in the experiment was obtained from Zhuji Sanfeng Environmental Protection Energy Co., Ltd. The COD mass concentration of this batch of landfill leachate was 3639 mg / L, the total phosphorus concentration was 294 mg / L, and the ammonia nitrogen concentration was 1062 mg / L.

[0027] Red mud: provided by Shandong Zibo Zhengheng Aluminum Co., Ltd., the main components include: 38.52% Fe 2 O 3 、27.83%Al 2 O 3 、12.49%SiO 2 、11.36%Na 2 O, 5.61% TiO 2 , 0.57% CaO, 0.34% SO 3 and other components (inevitable impurities and loss on ignition);

[0028] Copper anode mud: The copper anode mud was taken from Yunnan Copper Co., Ltd. The XRF analysis results of the elemental composition of the copper anode mud are as follows: 26.72% O, 20.46% Cu, 7.58% Pb, 7.02% Se, 5.54% S, 5.32% Ag, 4.47% As, 4.08% Sb, 4.02% Sn, 3.75% Ba, 2.64% Te, 1.75% Bi, 1.51% Cl, 1.12% Ni, 0.82% Zn, 0.24% Mg, 0.17% Si, 0.15% Au and other components (unavoidable ignition loss).

[0029] Example 1 Effect of the liquid-to-solid ratio of sulfuric acid solution and copper anode mud on the performance of the prepared catalyst

[0030] Sulfuric acid solution and copper anode mud are mixed according to a liquid-solid ratio of 0.075:1mL / g, 0.1:1mL / g, 0.125:1mL / g, 0.15:1mL / g, 0.3:1mL / g, 0.45:1mL / g, 0.50:1mL / g, 0.55:1mL / g, and 0.60:1mL / g, and stirred evenly to obtain sulfuric acid-doped anode mud, wherein the concentration of the sulfuric acid solution is 4M. The sulfuric acid-doped anode mud is roasted to obtain roasted anode mud, wherein the roasting time is 0.5 hours and the roasting temperature is 550°C. The landfill leachate and the roasted anode mud are mixed according to a liquid-solid ratio of 2:1mL / g, stirred for 0.25 hours, and the leachate slurry is obtained. Red mud and leachate slurry are mixed according to a mass ratio of 15:100, stirred evenly, and red mud leachate slurry is obtained. The red mud percolation slurry is dried and then roasted to obtain activated mud, wherein the roasting temperature is 550°C and the roasting time is 0.5 hours. The activated mud is ground into powder, and water and the activated mud powder are mixed at a liquid-solid ratio of 0.25:1 mL / g, and granulated to obtain activated mud particles. The activated mud particles are added to a reactor for hydrothermal reaction to obtain a catalyst, wherein the hydrothermal reaction temperature is 180°C and the hydrothermal reaction time is 1 hour.

[0031] Photocatalytic removal test: 5g of catalyst was added to 1L of landfill leachate, stirred at 120rpm and irradiated with UV light for 120min, then centrifuged at 5000rpm to separate solid and liquid. The concentration of different pollutants in the separated liquid was tested and the removal rate was calculated. The specific test and calculation are as follows.

[0032] COD concentration detection and calculation of COD removal rate: The COD concentration of the leachate was determined according to the national standard "Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method" (GB 11914-1989). The COD removal rate was calculated according to formula (1), where R COD is the COD removal rate, c COD0 and c CODt They are the COD concentrations (mg / L) of domestic waste leachate before and after treatment, respectively.

[0033]

[0034] Total phosphorus concentration detection and total phosphorus removal rate calculation: The total phosphorus concentration of the leachate was determined according to the standard "Water quality determination of phosphate and total phosphorus - continuous flow - ammonium molybdate spectrophotometry" (HJ 670-2013). The total phosphorus removal rate was calculated according to formula (2), where R TP is the total phosphorus removal rate, c TP0 and c TPt They are the total phosphorus concentrations (mg / L) of domestic waste leachate before and after treatment.

[0035]

[0036] Ammonia nitrogen concentration detection and ammonia nitrogen removal rate calculation: The ammonia nitrogen concentration of the leachate is determined according to the "Determination of ammonia nitrogen in water quality - salicylic acid spectrophotometry" (HJ536-2009). The ammonia nitrogen removal rate is calculated according to formula (3), where R N is the ammonia nitrogen removal rate, c N0 is the initial concentration of ammonia nitrogen in the leachate before treatment (mg / L), c Nt is the residual concentration of ammonia nitrogen in the treated leachate (mg / L).

[0037]

[0038] The test results of this embodiment are shown in Table 1.

[0039] Table 1 Effect of liquid-to-solid ratio of sulfuric acid solution and copper anode mud on the performance of the prepared catalyst

[0040]

[0041]

[0042] It can be seen from Table 1 that when the liquid-to-solid ratio of sulfuric acid solution to copper anode mud is less than 0.15:1 mL / g (such as in Table 1, the liquid-to-solid ratio of sulfuric acid solution to copper anode mud = 0.125:1 mL / g, 0.1:1 mL / g, 0.075:1 mL / g and lower ratios not listed in Table 1), less sulfuric acid solution is added, and the sulfuric acid solution and copper anode mud do not react fully during the roasting process, resulting in the removal rates of COD, total phosphorus and ammonia nitrogen by the prepared catalyst being significantly reduced as the liquid-to-solid ratio of sulfuric acid solution to copper anode mud decreases. When the liquid-solid ratio of sulfuric acid solution to copper anode mud is equal to 0.15-0.45:1 mL / g (as in Table 1, the liquid-solid ratio of sulfuric acid solution to copper anode mud = 0.15:1 mL / g, 0.3:1 mL / g, 0.45:1 mL / g), the sulfuric acid-doped anode mud is roasted, and the sulfides, selenides, tellurides, and oxides of metals such as gold, silver, copper, and nickel in the sulfuric acid-doped anode mud react with sulfuric acid and are converted into water-soluble sulfates, and selenides are oxidized to selenium dioxide and selenate, and selenium dioxide and silver chloride are separated from the solid by sublimation and volatilization. Finally, the prepared catalyst has a COD removal rate of more than 87%, a total phosphorus removal rate of more than 81%, and an ammonia nitrogen removal rate of more than 86%. When the liquid-solid ratio of sulfuric acid solution to copper anode mud is greater than 0.45:1 mL / g (such as in Table 1, the liquid-solid ratio of sulfuric acid solution to copper anode mud = 0.50:1 mL / g, 0.55:1 mL / g, 0.60:1 mL / g and higher ratios not listed in Table 1), excessive sulfuric acid solution is added, and the reaction of sulfuric acid solution and copper anode mud is unbalanced during the roasting process, resulting in the removal rate of COD, total phosphorus and ammonia nitrogen by the prepared catalyst significantly decreasing with the further increase of the liquid-solid ratio of sulfuric acid solution to copper anode mud. In summary, combining benefits and costs, when the liquid-solid ratio of sulfuric acid solution to copper anode mud is equal to 0.15-0.45:1 mL / g, it is most conducive to improving the performance of the prepared catalyst.

[0043] Example 2 Effect of liquid-to-solid ratio of landfill leachate and roasted anode mud on the performance of the prepared catalyst

[0044] Sulfuric acid solution and copper anode mud are mixed at a liquid-solid ratio of 0.45:1mL / g, stirred evenly, and sulfuric acid-doped anode mud is obtained, wherein the concentration of the sulfuric acid solution is 12M. Sulfuric acid-doped anode mud is roasted to obtain roasted anode mud, wherein the roasting time is 2.5 hours and the roasting temperature is 650°C. Leachate and roasted anode mud are mixed at a liquid-solid ratio of 1.25:1mL / g, 1.5:1mL / g, 1.75:1mL / g, 2:1mL / g, 4:1mL / g, 6:1mL / g, 6.5:1mL / g, 7:1mL / g, 7.5:1mL / g, stirred for 1.5 hours to obtain leachate slurry. Red mud and leachate slurry are mixed at a mass ratio of 30:100, stirred evenly, and red mud leachate slurry is obtained. The red mud leachate slurry is dried and then roasted to obtain activated mud, wherein the roasting temperature is 700°C and the roasting time is 2.5 hours. The activated clay material is ground into powder, and water and the activated clay material powder are mixed at a liquid-solid ratio of 0.4:1 mL / g, and granulated to obtain activated clay material particles. The activated clay material particles are added to a reactor for hydrothermal reaction to obtain a catalyst, wherein the hydrothermal reaction temperature is 270° C. and the hydrothermal reaction time is 3 hours.

[0045] The photocatalytic removal test, COD concentration detection and COD removal rate calculation, total phosphorus concentration detection and total phosphorus removal rate calculation, ammonia nitrogen concentration detection and ammonia nitrogen removal rate calculation are all the same as in Example 1. The test results of this example are shown in Table 2.

[0046] Table 2 Effect of liquid-to-solid ratio of landfill leachate and roasted anode mud on the performance of the prepared catalyst

[0047]

[0048] It can be seen from Table 2 that when the liquid-to-solid ratio of leachate and roasted anode mud is less than 2:1 mL / g (such as in Table 2, the liquid-to-solid ratio of leachate and roasted anode mud = 1.75:1 mL / g, 1.5:1 mL / g, 1.25:1 mL / g and lower ratios not listed in Table 2), the amount of leachate added is small, and the reaction between leachate and roasted anode mud is insufficient, resulting in the removal rates of COD, total phosphorus and ammonia nitrogen by the prepared catalyst to be significantly reduced as the liquid-to-solid ratio of leachate and roasted anode mud decreases. When the liquid-solid ratio of landfill leachate and roasted anode mud is equal to 2-6:1 mL / g (as in Table 2, the liquid-solid ratio of landfill leachate and roasted anode mud = 2:1 mL / g, 4:1 mL / g, 6:1 mL / g), the landfill leachate and roasted anode mud are mixed, and the water-soluble metal sulfate in the roasted anode mud dissolves into the landfill leachate and reacts with organic pollutants, ammonia nitrogen, phosphate and other pollutants in the landfill leachate to form a mixed slurry containing metal organic complexes, metal ammonium sulfate salts, and metal phosphates (precipitates). Finally, the prepared catalysts have a COD removal rate of more than 91%, a total phosphorus removal rate of more than 84%, and an ammonia nitrogen removal rate of more than 90%. When the liquid-solid ratio of landfill leachate and roasted anode mud is greater than 6:1 mL / g (such as in Table 2, the liquid-solid ratio of landfill leachate and roasted anode mud = 6.5:1 mL / g, 7:1 mL / g, 7.5:1 mL / g and higher ratios not listed in Table 2), the landfill leachate is added excessively, and the liquid reaction of landfill leachate and roasted anode mud is unbalanced during the roasting process, resulting in the removal rate of COD, total phosphorus and ammonia nitrogen by the prepared catalyst to be significantly reduced as the liquid-solid ratio of landfill leachate and roasted anode mud further increases. In summary, combining benefits and costs, when the liquid-solid ratio of landfill leachate and roasted anode mud is equal to 2 to 6:1 mL / g, it is most conducive to improving the performance of the prepared catalyst.

[0049] Example 3 Effect of the mass ratio of red mud to leachate slurry on the performance of the prepared catalyst

[0050] Sulfuric acid solution and copper anode mud are mixed at a liquid-solid ratio of 0.45:1 mL / g, stirred evenly, and sulfuric acid-doped anode mud is obtained, wherein the concentration of the sulfuric acid solution is 16 M. Sulfuric acid-doped anode mud is roasted to obtain roasted anode mud, wherein the roasting time is 4.5 hours and the roasting temperature is 750°C. Leachate and roasted anode mud are mixed at a liquid-solid ratio of 6:1 mL / g, stirred for 2.75 hours, and leachate mud is obtained. Red mud and leachate mud are mixed at a mass ratio of 7.5:100, 10:100, 12.5:100, 15:100, 30:100, 45:100, 50:100, 55:100, and 60:100, stirred evenly, and red mud leachate slurry is obtained. The red mud leachate slurry is dried and then roasted to obtain activated mud, wherein the roasting temperature is 850°C and the roasting time is 4.5 hours. The activated clay material is ground into powder, and water and the activated clay material powder are mixed at a liquid-solid ratio of 0.55:1 mL / g, and granulated to obtain activated clay material particles. The activated clay material particles are added to a reactor for hydrothermal reaction to obtain a catalyst, wherein the hydrothermal reaction temperature is 360° C. and the hydrothermal reaction time is 5 hours.

[0051] The photocatalytic removal test, COD concentration detection and COD removal rate calculation, total phosphorus concentration detection and total phosphorus removal rate calculation, ammonia nitrogen concentration detection and ammonia nitrogen removal rate calculation are all the same as in Example 1. The test results of this example are shown in Table 3.

[0052] Table 3 Effect of red mud and leachate slurry mass ratio on the performance of the prepared catalyst

[0053]

[0054]

[0055] It can be seen from Table 3 that when the mass ratio of red mud to leachate slurry is less than 15:100 (such as in Table 3, the mass ratio of red mud to leachate slurry = 12.5:100, 10:100, 7.5:100 and lower ratios not listed in Table 3), less red mud is added, and the red mud and leachate slurry do not react fully during the subsequent roasting process, resulting in the removal rates of COD, total phosphorus and ammonia nitrogen by the prepared catalyst being significantly reduced as the mass ratio of red mud to leachate slurry decreases. When the mass ratio of red mud to leachate slurry is equal to 15-45:100 (as in Table 3, the liquid-solid ratio of landfill leachate and roasted anode mud is 15:100, 30:100, 45:100), the red mud and leachate slurry are mixed, and the alkaline substances and minerals containing aluminum, titanium, iron, silicon, and calcium in the red mud are adsorbed and reacted with metal organic complexes, metal ammonium sulfate salts, and metal phosphates (precipitates) to form a multi-component mixture. The red mud leachate slurry is dried and then roasted. During the roasting process, organic pollutants are pyrolyzed to form carbon-based materials, while ammonia nitrogen pollutants are oxidized. The inorganic salts introduced into the landfill leachate induce the multi-component mixture to further undergo oxidation reaction and phase transformation on the surface of the carbon-based material to form an activated mud containing a variety of catalytic materials such as gold, copper, silver, iron, tellurium, and titanium. Finally, the prepared catalysts have a COD removal rate of more than 95%, a total phosphorus removal rate of more than 89%, and an ammonia nitrogen removal rate of more than 93%. When the mass ratio of red mud to leachate slurry is greater than 45:100 (such as in Table 3, the mass ratio of red mud to leachate slurry = 50:100, 55:100, 60:100 and higher ratios not listed in Table 3), excessive red mud is added, and the reaction of red mud and leachate slurry is unbalanced during the subsequent roasting process, resulting in the removal rate of COD, total phosphorus and ammonia nitrogen by the prepared catalyst significantly decreasing as the mass ratio of red mud to leachate slurry further increases. In summary, combining benefits and costs, when the mass ratio of red mud to leachate slurry is equal to 15-45:100, it is most conducive to improving the performance of the prepared catalyst.

Claims

1. A method for preparing a catalyst using landfill leachate and copper anode mud, characterized in that: The following steps are involved: (1) mixing sulfuric acid solution and copper anode mud, stirring evenly, to obtain sulfuric acid mixed with anode mud; (2) roasting the sulfuric acid-mixed anode mud to obtain roasted anode mud; (3) mixing the landfill leachate and the roasted anode mud, stirring them evenly to obtain leachate slurry; (4) mixing the red mud and the leachate slurry and stirring them evenly to obtain a red mud leachate slurry; (5) drying the red mud percolation slurry and then roasting it to obtain activated mud; (6) grinding the activated clay into powder, mixing water and the activated clay powder, and granulating to obtain activated clay granules; (7) Adding the activated mud particles into a reactor for hydrothermal reaction to obtain a catalyst.

2. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The liquid-to-solid ratio of the sulfuric acid solution and the copper anode mud in step (1) is 0.15-0.45:1 mL / g, and the concentration of the sulfuric acid solution is 4-16 M.

3. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The calcination time in step (2) is 0.5 to 4.5 hours, and the calcination temperature is 550 to 750°C.

4. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The liquid-to-solid ratio of the landfill leachate and the roasted anode mud in step (3) is 2-6:1 mL / g, and the stirring time is 0.25-2.75 hours.

5. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The mass ratio of the red mud to the leachate slurry in step (4) is 15 to 45:

100.

6. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The calcination temperature in step (5) is 550-850° C., and the calcination time is 0.5-4.5 hours.

7. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The liquid-to-solid ratio of water to activated mud powder in step (6) is 0.25-0.55:1 mL / g.

8. The method for preparing a catalyst using landfill leachate and copper anode mud according to claim 1, characterized in that: The temperature of the hydrothermal reaction in step (7) is 180 to 360° C., and the hydrothermal reaction time is 1 to 5 hours.

9. Use of a catalyst prepared by the method according to any one of claims 1 to 8 in the treatment of landfill leachate.

10. The use according to claim 9, characterized in that: The application is to remove one or more of COD, total phosphorus and ammonia nitrogen in landfill leachate.

Citation Information

Cited By

  • Method for preparing heavy metal contaminated soil stabilizer from electrolytic manganese residues and landfill leachate and application of heavy metal contaminated soil stabilizer

    CN119799346A