3DP sand mold printing cast iron coating and preparation method thereof
By using 3DP sand-type printing cast iron coatings in resin sand casting, combined with crosslinked polyimide and calcium oxide and other components, the problem of vein defects in resin sand casting is solved, and the finish and high-temperature performance of the casting surface is improved, significantly Improved casting quality.
Patent Information
- Application Number
- CN202411228867.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
Common vein defects in resin sand casting limit the quality of castings, especially on cast iron parts, resulting in increased workload of castings or even scrapped, affecting the development of resin sand casting.
3DP sand-printed cast iron coating is used, which contains crosslinked polyimide and calcium oxide, which has high permeability, chilling and sintering properties, forming a good solid-state protective surface and reducing the appearance of veins.
It effectively eliminates the vein defects on the surface of the casting, improves the metal permeability and low gas emission of the paint, enhances high temperature strength, prevents sand cracks, and significantly improves the quality of the casting.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the field of casting coatings, and in particular to a 3DP sand mold printing cast iron coating and a preparation method thereof. Background Art
[0002] Sand casting plays an important role in the foundry industry. According to statistics, 80% to 90% of the total global casting output is produced by sand casting. Compared with other casting methods, sand casting has the advantage of not being restricted by the shape, size, complexity and alloy type of the casting. According to the binder used for core making, sand casting can be divided into three categories, namely clay sand casting, water glass sand casting and resin sand casting. Among them, resin sand casting has occupied a very important position in casting production due to its advantages in various aspects.
[0003] Resin sand casting is a casting method that uses organic resins such as phenolic resin and furan resin as a binder to prepare sand molds (cores). In the past 70 years, with the increasing requirements for the output and quality of castings in the automotive industry, the types of resin sand have continued to increase, the core making methods have been continuously improved, and the supporting related process equipment has become more and more complete. Resin sand is gradually replacing clay sand and water glass sand and becoming the most mainstream casting modeling material.
[0004] The defects of castings in resin sand casting production have restricted its development. Vein defects are the most common problem. Vein defects frequently occur in the cylinder head of the engine block, which increases the workload of casting cleaning and even leads to the scrapping of castings in severe cases, limiting the development of resin sand casting.
[0005] Veining is a defect on the surface of a casting. It is irregular in shape, protruding from the surface of the casting, and distributed in strips or nets. It often occurs at the inner fillet and hot spots of the casting. Studies have shown that gray cast iron with high lead, carbon, silicon, and phosphorus content has a significant tendency to veining. The formation of veining requires two conditions. The first condition is that the sand core of the sand mold cracks due to the force generated by the expansion and contraction of the sand core of the sand mold or external mechanical treatment, and cracks appear on the surface of the sand core of the sand mold. The second condition is that the high-temperature liquid metal in the pouring state has sufficient fluidity and pressure to flow into the cracked sand core of the sand mold, thereby cooling to form veining.
[0006] It can be seen that in order to solve the vein defects of cast iron parts, it is necessary to improve the high temperature performance of resin sand molds, reduce the cracking tendency of sand molds, promote rapid solidification of liquid metal, and weaken the fluidity of liquid metal. This can be done from several aspects such as sand mold additives and casting coatings.
[0007] Compared with other veining prevention and control directions, anti-veining coating is the most economical and easiest to complete. The method of improving the binder to prevent and control veining requires the binder to have high high temperature strength, and organic resin binders are difficult to meet this requirement. Inorganic binders have high high temperature strength, but they have disadvantages in core making process and sand cleaning. For improved binders, it is also necessary to develop a core making process to match them. This process is far less convenient and economical than casting coatings. The biggest disadvantage of replacing low-expansion raw sand is that it greatly increases the cost. In addition, the low recycling rate of old sand in China has greatly limited the implementation of this method. Improving the casting process can avoid the generation of veining, but it may also cause other casting defects and should be used with caution. Sand mold additives are an effective method for preventing and controlling veining and are currently the most mainstream anti-veining method, but their cost is still higher than casting coatings. Summary of the invention
[0008] The invention provides a 3DP sand mold printing cast iron coating, which has high permeability, chilling and sintering properties, can form a good solid protective surface on the surface of the cast iron part, and the formed cast iron part surface has almost no veining.
[0009] A 3DP sand mold printing cast iron coating comprises the following raw materials, measured in percentage by mass: 45-75% of a refractory filler, 2-6% of a suspending agent, 1-5% of a modifying additive, 0.5-2% of a binder, 0.05-0.5% of a surfactant, 0.05-0.5% of a wetting agent, and 26-41% of deionized water; wherein the refractory filler comprises calcium oxide, and the modifying additive is a cross-linked polyimide.
[0010] In some embodiments of the present invention, the refractory filler further comprises at least two of graphite powder, mullite powder and phenolic resin coated sand. Specifically, the graphite powder can be flaky graphite or earthy graphite, or a mixture of the two in any proportion; the phenolic resin coated sand can be purchased from Pengxian Mineral Products Processing Factory, Lingshou County, Shijiazhuang, Hebei.
[0011] In some embodiments of the present invention, the particle size of the mullite powder is 300-325 mesh.
[0012] In some embodiments of the present invention, the method for preparing the cross-linked polyimide comprises the following steps: S1: Dissolve 4,4'-diaminodiphenyl ether in an organic solvent at room temperature, place it in an ice water bath, pass an inert gas, add pyromellitic anhydride, and stir overnight; S2: Add melamine to the solution obtained in S1 and stir at room temperature until it is completely dissolved, then heat the system to 180-200°C and maintain for 24 hours; S3: After cooling to room temperature, the precipitate is filtered, washed and dried to obtain the cross-linked polyimide.
[0013] Furthermore, the molar ratio of 4,4'-diaminodiphenyl ether to pyromellitic anhydride in S1 is 1:2-2.2.
[0014] Furthermore, the organic solvent in S1 can be dimethyl sulfoxide, tetrahydrofuran, propylene carbonate, cyclopentyl methyl ether, etc.
[0015] Furthermore, the molar amount of melamine added in S2 is 1-1.5 times the molar amount of pyromellitic anhydride.
[0016] In some embodiments of the present invention, the suspending agent is attapulgite.
[0017] In some embodiments of the present invention, the binder is at least one of xanthodextrin, xanthan gum and modified starch.
[0018] In the present invention, polyimide is prepared into a porous cross-linked structure as a modified additive, which can be used in combination with attapulgite as a preferred suspending agent. By utilizing the structural advantages, the other components of the coating are bound, the viscosity is increased, and a good suspension effect is achieved. More importantly, when the temperature of the coating begins to rise, the heat can be quickly transferred to the mold, reducing the possibility of the molten metal flowing into the cracks of the sand mold. At moderately high temperatures, the low thermal expansion rate of the cross-linked porous polyimide is conducive to improving the metal permeability resistance of the coating; after ultra-high temperature carbonization, the high residual carbon formed can improve the high temperature strength and yield of the coating, prevent the tendency of thermal cracking in the sand mold, and thus eliminate the veining defects of the casting.
[0019] The addition of calcium oxide can react with silicon dioxide produced by heat, as well as carbon monoxide and carbon dioxide produced by carbonization of organic matter in the system, preventing the occurrence of sand sticking, reducing gas generation, and thus reducing the appearance of veining.
[0020] The preparation method of the 3DP sand mold printing cast iron coating described above comprises the following steps: adding a binder and a modifying additive to deionized water, and stirring at a speed of 500-600r / min for 30-45min, adding a suspending agent while stirring, and continuously stirring for 5-10min, adding a refractory filler, increasing the speed to 800-900r / min and stirring for 10-15min, and then sequentially adding a surfactant and a wetting agent, and stirring evenly to obtain the 3DP sand mold printing cast iron coating.
[0021] In some embodiments of the present invention, when preparing 3DP sand mold printing cast iron coating, when adding surfactant and wetting agent, the stirring speed is reduced to 400-500 r / min.
[0022] Beneficial effects: Compared with the prior art, the present invention creatively adds cross-linked polyimide as a modifying additive for the coating, and uses it in conjunction with calcium oxide as a refractory filler to improve the metal permeability resistance and low gas evolution of the 3DP sand mold printed cast iron coating, ultimately achieving the anti-veining effect of the coating. DETAILED DESCRIPTION
[0023] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0024] The following is an exemplary description of the preparation process of the cross-linked polyimide used in the embodiment: Cross-linked polyimide-1 S1: Dissolve 20.0 g (100 mmol) of 4,4'-diaminodiphenyl ether in 200 ml of dimethyl sulfoxide at room temperature, place it in an ice-water bath, introduce nitrogen, add 43.6 g (200 mmol) of pyromellitic anhydride, and stir overnight; S2: Add 12.6 g (100 mmol) of melamine to the solution obtained in S1 and stir at room temperature until it is completely dissolved, then heat the system to 180 °C and maintain for 24 h; S3: After cooling to room temperature, the precipitate is filtered, washed and dried to obtain the cross-linked polyimide-1.
[0025] Cross-linked polyimide-2 S1: Dissolve 20.0 g (100 mmol) of 4,4'-diaminodiphenyl ether in 200 ml of tetrahydrofuran at room temperature, place the mixture in an ice-water bath, introduce nitrogen, add 45.78 g (210 mmol) of pyromellitic anhydride, and stir overnight; S2: Add 15.12 g (120 mmol) of melamine to the solution obtained in S1 and stir at room temperature until it is completely dissolved, then heat the system to 190 °C and maintain for 24 h; S3: After cooling to room temperature, the precipitate is filtered, washed and dried to obtain the cross-linked polyimide-2.
[0026] Cross-linked polyimide-3 S1: Dissolve 20.0 g (100 mmol) of 4,4'-diaminodiphenyl ether in 200 ml of cyclopentyl methyl ether at room temperature, place the mixture in an ice-water bath, introduce nitrogen, add 47.96 g (220 mmol) of pyromellitic anhydride, and stir overnight; S2: Add 18.9 g (150 mmol) of melamine to the solution obtained in S1 and stir at room temperature until it is completely dissolved, then heat the system to 200 °C and maintain for 24 h; S3: After cooling to room temperature, the precipitate is filtered, washed and dried to obtain the cross-linked polyimide-3.
[0027] Example 1 0.5% modified starch and 1% cross-linked polyimide-1 were added to 26% deionized water, and stirred at 500 r / min for 30 minutes, then 2% attapulgite was added while stirring, and stirring was continued for 5 minutes. Then, 75% refractory filler (20% graphite powder, 20% mullite powder, 20% phenolic resin coated sand, 15% calcium oxide) was added, and the speed was increased to 800 r / min and stirred for 10 minutes. Then, 0.35% fatty alcohol polyoxyethylene ether and 0.15% Triton X-102 were added in sequence, and the speed was reduced to 400 r / min and stirred evenly to obtain the 3DP sand mold printing cast iron coating.
[0028] Example 2 1% yellow dextrin and 3% cross-linked polyimide-2 were added to 32.5% deionized water, and stirred at 550 r / min for 40 minutes, then 4% attapulgite was added while stirring, and stirring was continued for 8 minutes. Then, 60% refractory filler (20% graphite powder, 20% phenolic resin coated sand, 20% calcium oxide) was added, and the speed was increased to 850 r / min and stirred for 12 minutes. Then, 0.2% fatty alcohol polyoxyethylene ether and 0.3% Triton X-102 were added in sequence, and the speed was reduced to 450 r / min and stirred evenly to obtain the 3DP sand mold printing cast iron coating.
[0029] Example 3 2% xanthan gum and 5% cross-linked polyimide-3 were added to 41% deionized water, and stirred at 600 r / min for 45 minutes, then 6% attapulgite was added while stirring, and stirring was continued for 10 minutes. Then, 45% refractory filler (10% mullite powder, 10% phenolic resin coated sand, 25% calcium oxide) was added, and the speed was increased to 900 r / min and stirred for 15 minutes. Then, 0.5% fatty alcohol polyoxyethylene ether and 0.5% Triton X-102 were added in sequence, and the speed was reduced to 500 r / min and stirred evenly to obtain the 3DP sand mold printing cast iron coating.
[0030] Comparative Example 1 Same as Example 3, except that the added amount of the cross-linked polyimide is 6%.
[0031] Comparative Example 2 Same as Example 3, except that the cross-linked polyimide is not added.
[0032] Comparative Example 3 Same as Example 3, except that calcium oxide is not added.
[0033] Comparative Example 4 Same as Example 3, except that the cross-linked polyimide and calcium oxide are not added at the same time.
[0034] Performance Testing Suspension: According to the measuring cylinder method, the uniformly stirred coating is introduced into the stoppered measuring cylinder along the glass rod to make it reach the 100ml mark, plug the stopper, let it stand for 24 hours, measure the volume of the upper clear liquid, and calculate the suspension rate; Surface finish: The coatings obtained in Examples 1-3 and Comparative Examples 1-4 were applied to the surface of the casting mold by brushing, dipping, spraying or flow coating, and then dried to form a coating. According to naked eye observation, the coating surface had obvious large particles, the coating appeared very rough and there were obvious flow marks, which was rated as Grade 1; the coating surface had fewer particles and was relatively rough, which was rated as Grade 2; the coating surface was relatively fine and smooth, which was rated as Grade 3; Gas emission: Dry the coating sample to be tested in an electric oven at (130±5)℃, cool it to room temperature in a desiccator, and grind it into powder for use; heat the gas emission tester to (850±5)℃, then weigh (1±0.01)g of the sample and evenly place it in a porcelain boat [the porcelain boat has been pre-burned at (850±5)℃ for 10 min and then placed in a desiccator to cool to room temperature for use]; send the porcelain boat into the red-hot part in the center of the quartz tube and quickly seal the tube mouth with a special rubber stopper; the recorder starts to record the gas emission of the sample, and read the maximum data recorded by the recorder within 3 minutes as the gas emission value of the sample; Determination of linear expansion coefficient: Take the material to be tested and use a mold to form a 10 mm×50 mm specimen. Avoid cracks in the specimen during the preparation process; place the test in an electric oven to dry at (110±5)℃, and cool to room temperature in a desiccator for use; calibrate the thermal expansion instrument and determine the calibration temperature A0; measure and record the length L0 of the specimen at room temperature, accurate to 0.023mm; place the specimen in the loading area of the sample tube, with the hot end of the thermocouple located at the center of the specimen length, and adjust the measuring device to ensure good contact between the specimen, the ejector rod, and the displacement sensor; heat at a heating rate of 10℃ / min until 1200℃, and record the reading of the displacement sensor within the temperature range, recorded as L1; calculate the linear expansion coefficient according to the following formula:
[0035] The test results are detailed in Table 1:
[0036] According to the results in Table 1, the amount of the cross-linked polyimide added has an appropriate range, i.e., 1-5%. If it exceeds this range (Comparative Example 1), the linear expansion coefficient of the obtained coating will not continue to rise, but will increase. This may be because the increase of the cross-linked polyimide makes the contact between it and other components closer and the mutual force is enhanced. Moreover, the lack of either the cross-linked polyimide or the calcium oxide will lead to the deterioration of the surface finish, gas emission and linear expansion coefficient of the obtained coating. It can be seen that the two are important for improving the anti-veining performance of the coating.
[0037] In summary, the 3DP sand mold printing cast iron coating provided by the present invention has excellent suspension properties. Due to its low thermal linear expansion coefficient, it can effectively enhance the coating's resistance to metal penetration, and the resulting coating has a smooth surface, thereby eliminating the veining defects of the casting.
Claims
1. A 3DP sand mold printing cast iron coating, characterized in that: The invention comprises the following raw materials in percentage by mass: 45-75% of refractory filler, 2-6% of suspending agent, 1-5% of modifying additive, 0.5-2% of binder, 0.05-0.5% of surfactant, 0.05-0.5% of wetting agent and 26-41% of deionized water; wherein the refractory filler comprises calcium oxide, and the modifying additive is cross-linked polyimide.
2. The 3DP sand mold printing cast iron coating according to claim 1, characterized in that: The refractory filler further comprises at least two of graphite powder, mullite powder and phenolic resin coated sand.
3. The 3DP sand mold printing cast iron coating according to claim 2, characterized in that: The particle size of the mullite powder is 300-325 meshes.
4. The 3DP sand mold printing cast iron coating according to claim 1, characterized in that: The preparation method of the cross-linked polyimide comprises the following steps: S1: Dissolve 4,4'-diaminodiphenyl ether in an organic solvent at room temperature, place it in an ice water bath, pass an inert gas, add pyromellitic anhydride, and stir overnight; S2: Add melamine to the solution obtained in S1 and stir at room temperature until it is completely dissolved, then heat the system to 180-200°C and maintain for 24 hours; S3: After cooling to room temperature, the precipitate is filtered, washed and dried to obtain the cross-linked polyimide.
5. The 3DP sand mold printing cast iron coating according to claim 4, characterized in that: The molar ratio of 4,4'-diaminodiphenyl ether to pyromellitic anhydride in S1 is 1:2-2.
2.
6. The 3DP sand mold printing cast iron coating according to claim 4, characterized in that: The molar amount of melamine added in S2 is 1-1.5 times the molar amount of 4,4'-diaminodiphenyl ether.
7. The 3DP sand mold printing cast iron coating according to claim 1, characterized in that: The suspending agent is attapulgite.
8. The 3DP sand mold printing cast iron coating according to claim 1, characterized in that: The binder is at least one of yellow dextrin, xanthan gum and modified starch.
9. The method for preparing the 3DP sand mold printing cast iron coating according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding a binder and a modifying additive to deionized water, stirring at a speed of 500-600 r / min for 30-45 minutes, adding a suspending agent while stirring, continuing stirring for 5-10 minutes, adding a refractory filler, increasing the speed to 800-900 r / min and stirring for 10-15 minutes, adding a surfactant and a wetting agent in sequence, and stirring evenly to obtain the 3DP sand mold printing cast iron coating.
10. The method for preparing 3DP sand mold printing cast iron coating according to claim 9, characterized in that: When adding surfactant and wetting agent, the stirring speed is reduced to 400-500r / min.