Casting assembly
By designing the core and shell with hollow cavity in the casting assembly, and combining the ligament structure to match thermal performance and reduce internal stress, the irregularity of cooling hole diameter caused by thermal performance mismatch and internal stress in the casting assembly is solved. The problem is that the dimensional accuracy and finished product quality of the castings are improved.
Patent Information
- Application Number
- CN202410567950.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-22
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-22
AI Technical Summary
In casting components, especially in parts with large internal cavity, mismatch in thermal performance and internal stress lead to irregular cooling hole diameters and excessive shear force, resulting in geometric irregularities of finished parts and possible cracks or breaks. .
By designing casting components with hollow cavity cores and shells, the thickness and thermal properties of the body are printed and adjusted using additive manufacturing techniques, combined with ligament structures to match thermal properties, reduce internal stress and shear forces, and through multiple Sub-iteration design optimizes casting components to meet the needs of different castings.
The castings are improved in dimensional accuracy, internal stress and shear forces are reduced, the problem of irregular pore size of cooling holes is reduced, and the quality and reliability of finished parts are improved.
Smart Images

Figure CN118989246A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates generally to a casting assembly, and more particularly to a casting assembly having a shell / core arrangement. Background Art
[0002] Casting processes such as investment casting, metal casting, sand casting, etc. can be used to form various castings. The casting process generally includes a core at least partially surrounded by a shell to form an intermediate cavity. Molten material can be introduced into the cavity to form the casting, and at least one of the core or the shell is then generally removed. In some examples, the core can be formed of a sacrificial material, such as wax, which can be recovered after casting. In some examples, the core can include a brittle material so that the core can be crushed or broken for removal. In some examples, the core can remain in the casting after the casting process is completed. BRIEF DESCRIPTION OF THE DRAWINGS
[0003] A full and enabling disclosure of the present disclosure, including the best mode thereof, to one of ordinary skill in the art is set forth in the specification with reference to the accompanying drawings, in which:
[0004] Figure 1 is a schematic perspective view of a casting assembly according to various aspects described herein.
[0005] Figure 2 yes Figure 1 A cross-sectional view of a casting assembly taken along line II-II and showing a core, a shell, and a hollow cavity according to various aspects described herein.
[0006] Figure 3 yes Figure 2 A cross-sectional view of the cast assembly taken along line III-III.
[0007] Figure 4 yes Figure 2 A cross-sectional view of the cast assembly taken along line IV-IV.
[0008] Figure 5 yes Figure 2 A cross-sectional view of the cast assembly taken along line VV.
[0009] Figure 6 is similar to Figure 1 A cross-sectional view of another casting assembly of a casting assembly and showing a first core and a first hollow cavity according to various aspects described herein.
[0010] Figure 7 yes Figure 6 A cross-sectional view of a casting assembly showing a second core and a second hollow cavity according to various aspects described herein.
[0011] Figure 8 is similar to Figure 1 and Figure 6 A cross-sectional view of another casting assembly of a casting assembly is shown, and illustrates a body having a first hollow cavity according to various aspects described herein.
[0012] Fig. 9 yes Figure 8 0014] A cross-sectional view of a casting assembly of FIG. 1 and illustrating a body having a second hollow cavity according to various aspects described herein. DETAILED DESCRIPTION
[0013] Reference will now be made in detail to the present embodiments of the present disclosure, one or more examples of which are illustrated in the accompanying drawings. The detailed description uses numerical and letter references to refer to features in the drawings. Like or similar reference numbers in the drawings and description have been used to refer to like or similar parts of the present disclosure.
[0014] As may be used herein, the terms “first,” “second,” and “third” may be used interchangeably to distinguish one component from another, and are not intended to indicate the position or importance of the respective components.
[0015] The terms "upstream" and "downstream" refer to relative directions with respect to flow in a path. For example, with respect to fluid flow, "upstream" refers to the direction from which the fluid is flowing, and "downstream" refers to the direction toward which the fluid is flowing.
[0016] The term "fluid" refers to a gas or a liquid. The term "fluid communication" or "fluid coupling" refers to the ability of a fluid to establish a connection between designated areas.
[0017] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0018] As used herein, an "additive manufacturing" part will refer to a part formed by an additive manufacturing (AM) process, in which the part is built layer by layer by continuous deposition of material. AM is an appropriate name for describing the technology of building 3D objects by adding layer after layer of material, whether the material is plastic, ceramic or metal. AM technology can utilize computers, 3D modeling software (computer-aided design or CAD), machine equipment and layered materials. Once a CAD sketch is generated, the AM equipment can read the data from the CAD file and lay or add continuous layers of liquid, powder, sheet or other materials in a layer-by-layer manner to manufacture a 3D object. It is understood that the term "additive manufacturing" covers many technologies, including subsets such as 3D printing, rapid prototyping (RP), direct digital manufacturing (DDM), layered manufacturing and additive manufacturing. Non-limiting examples of additive manufacturing that can be used to form additive manufacturing parts include powder bed fusion, reduced photopolymerization, binder jetting, material extrusion, directed energy deposition, material jetting or sheet lamination. It is also expected that the method used may include printing a negative of a part by refractory metal, ceramic or printed plastic, and then using the negative to cast the part.
[0019] All directional references (e.g., radial, axial, proximal, distal, upper, lower, upward, downward, left, right, lateral, front, rear, top, bottom, above, below, vertical, horizontal, clockwise, counterclockwise, upstream, downstream, front, rear, etc.) are used only for identification purposes to help the reader understand the present disclosure and do not create limitations, particularly limitations on the position, orientation, or use of the various aspects of the present disclosure described herein. Connection references (e.g., attachment, connection, connection, and engagement) should be interpreted broadly and include intermediate structural elements between sets of elements and relative motion between elements, unless otherwise specified. Therefore, connection references do not necessarily infer that two elements are directly connected and have a fixed relationship to each other. The exemplary drawings are for illustrative purposes only, and the dimensions, positions, orders, and relative sizes reflected in the attached drawings may vary.
[0020] As used herein, the "body area" (denoted as "A") of a cast component core having a core outer surface is the area of the core. b ”) refers to the cross-sectional area defined by the outer surface of the core in a cross section through the cast component.
[0021] As used herein, the "hollow area" (denoted as "A") of a cast component core having a core interior surface defining a hollow cavity is h ”) refers to the cross-sectional area of the hollow cavity in a cross section through the cast component.
[0022] As used herein, the "minimum core thickness" (denoted as "CT") of the core min”) refers to the minimum material thickness between the core outer surface and the core inner surface in a cross section through the casting component. In an exemplary embodiment where the core body includes a plurality of hollow cavities defined by a corresponding plurality of core inner surfaces, each core inner surface defines a minimum core thickness CT in the cross section relative to the core outer surface. min .
[0023] As used herein, the "maximum core thickness" (denoted as "CT max ”) refers to the maximum material thickness between the core outer surface and the core inner surface in a cross section through the casting assembly. In an exemplary embodiment where the core body includes a plurality of hollow cavities defined by a corresponding plurality of core inner surfaces, each core inner surface defines a maximum core thickness CT in cross section relative to the outer surface. max .
[0024] As used herein, the "minimum shell thickness" (denoted as "ST") of a component shell having a first shell surface and a second shell surface defining a part cavity is min ”), wherein the first shell surface is fluidly isolated from the part cavity refers to the minimum material thickness between the first shell surface and the second shell surface in a cross section through the casting component.
[0025] As used herein, "hollow cavity parameter" (denoted as "HCP") refers to a parameter that describes the area of the body A. b , hollow area A h , minimum core thickness CT min , Maximum core thickness CT max and minimum shell thickness ST min The value of the relationship between .
[0026] Various aspects of the present disclosure relate to a casting assembly having at least a core and a shell. At least one of the first body or the second body can be printed in an additive manufacturing process. In some embodiments, the core defines a casting core and the shell defines a casting shell spaced from the casting core and at least partially surrounding the casting core. The core defines a pattern of portions of the casting. In some embodiments, the casting assembly forms a cooling airfoil having internal cooling channels and film cooling holes.
[0027] The core and shell are arranged relative to each other to form a part cavity. In some embodiments, one or more elongated ligaments extending between the core and the shell are provided. Such ligaments can be used to maintain a separation distance between the first body and the second body, or to form a hole through the casting. Typically, the ligament has a smaller thickness than the core or the shell.
[0028] Once assembled, the casting assembly is heat treated / fired and cooled to harden or strengthen the casting assembly to receive the molten material. The molten material is poured, injected or otherwise introduced into the part cavity to form a casting. The casting assembly and the casting are cooled, and at least one of the first body or the second body is subsequently removed from the casting to form a finished component.
[0029] When printing one or both bodies by additive manufacturing, one factor to consider is that during the printing process of the body, as additional layers are added to the body, internal stresses are generated in the thickness of the body, which may cause deformation, surface irregularities or other printing problems. It should be understood that such printing problems result in corresponding irregularities in the finished part.
[0030] Another factor to consider, whether or not the body is made by additive manufacturing, is that during firing of the cast component, thermal contraction of the first and second bodies results in geometric contraction. The thickness of the first or shell body corresponds to their thermal mass and the amount of contraction. If the thickness of the first and second bodies are significantly different, they will experience different amounts or rates of contraction, resulting in geometric irregularities in the cast component.
[0031] Another factor to consider during casting is that when the molten material is provided to the cast component, thermal and solidification shrinkage of the casting occurs during cooling and hardening. This effect causes the size of the casting to be reduced relative to the design size of the part cavity.
[0032] Another factor to consider is that castings experience internal stresses during cooling and hardening. For example, unequal shrinkage in the casting due to differences in part thickness can cause cracks, fractures or grain defects.
[0033] Another factor to consider is that during cooling and hardening, the casting exerts various forces on the casting component as each component cools at a different rate. Such forces can cause shearing, yielding, or breaking of the casting component. For example, thermal or solidification shrinkage of the casting constrained within the casting component can produce shearing forces on ligaments in the casting component, resulting in ligament breaking and corresponding geometric irregularities in the casting.
[0034] Another factor to consider is that the cast component also experiences thermal contraction and deformation around the casting during cooling and hardening. The material selection and geometry of the cast component results in a trade-off between the strength required to contain the molten material and the flexibility required to deform so that the cast component does not exert excessive forces on the casting during solidification.
[0035] Standard practices for solving the above problems have been used to design casting components with a first body and a second body of similar thickness, which provide more uniform thermal effects (such as shrinkage) within the casting component and more uniform thermal interactions between the casting component and the casting. However, this approach is difficult when casting parts with large internal cavities. For example, known casting processes are used to produce cooling airfoils with large internal cooling channels and multiple small-diameter cooling holes extending from the internal cooling channels through the outer wall. In this case, one or more large central cores are formed by or connected to multiple smaller and thinner ligaments. During the casting process, the central core and multiple smaller ligaments are placed in the casting shell to form a central cooling channel and multiple cooling holes in the casting, respectively. Different component thicknesses in the casting result in a mismatch in thermal properties or thermal characteristics between the central core and the casting shell. When the molten material is introduced and cooled, this thermal property mismatch produces excessive shear forces on the ligaments during casting, resulting in irregular cooling hole diameters in the finished part.
[0036] The inventor's practice proceeds as follows: a casting component is designed for a selected part design, the casting component is printed, and the casting component design is modified as needed based on the printing stress or irregularity in the printed first body or second body. The inventor's practice then proceeds in a firing and casting manner, checking whether the resulting part has undesirable properties, features or defects, and making additional modifications to the casting component design as needed based on thermal properties, internal stresses, component shear, or as described above. A part is made from the modified casting component and the process is repeated. This iterative trial and error process continues for a long period of time until a feasible casting component design is determined for a given casting. The above iterative process is then repeated for each casting component corresponding to each casting required for production. A description of an example of a novel casting component developed by the inventor is provided below.
[0037] Now referring to the accompanying drawings, Figure 1 A casting assembly 10 according to various aspects described herein is shown. The casting assembly 10 includes a core 20 and a shell 30. A mold base 12 for supporting the casting assembly 10 is schematically shown. In some exemplary embodiments, the mold base 12 may be integrally formed with the core 20 or the shell 30.
[0038] For reference purposes, Figure 1 A set of relative reference directions and a coordinate system are shown in FIG. The casting assembly 10 defines an axial direction A, which is shown extending vertically along the page. The first horizontal axis H1 and the second horizontal axis H2 each extend orthogonally to the axial direction A and are each shown extending partially into the page.
[0039] In the exemplary illustration shown, the core 20 is a rectangular prism and the shell 30 is a hollow rectangular prism. It should be understood that the core 20 or the shell 30 can have any geometric profile. In addition, either or both of the core 20 or the shell 30 are formed of a monolithic ceramic.
[0040] The core 20 includes a core inner surface 22 and a core outer surface 24. In the example shown, the core 20 is a single body having the core inner surface 22 and the core outer surface 24. In another non-limiting embodiment, the core 20 includes a central body having an outer layer, shell, skin, etc. defining the core outer surface 24, and a central body having an inner layer, shell, skin, etc. defining the core inner surface 22.
[0041] The shell 30 includes a first shell surface 31 and a second shell surface 32. As shown, the second shell surface 32 defines the part cavity 15. The core outer surface 24 is spaced apart from the second shell surface 32. The first shell surface 31 is fluidly isolated from the part cavity 15. In some embodiments, the first shell surface 31 defines the outer surface of the shell 30. In some embodiments, the shell 30 includes an additional cavity or hollow area defined by the first shell surface 31.
[0042] The core 20 extends between a first end 26 and a second end 28 along the axial direction A. The housing 30 also extends between a first end 36 and a second end 38 along the axial direction A. In the exemplary embodiment shown, the first ends 26, 36 and the second ends 28, 38 are aligned with each other such that the first body 20 and the second body 30 have the same axial length.
[0043] Additionally, the core inner surface 22 at least partially defines a hollow cavity 25 within the core body 20. The hollow cavity 25 is fluidly isolated or separated from the part cavity 15. Any number of hollow cavities 25 may be provided in the core body 20.
[0044] In the exemplary embodiment shown, the casting assembly 10 is in the form of an investment casting mold, wherein the core body 20 defines a casting core and the shell 30 defines a casting shell surrounding the casting core. During operation, molten material is introduced into the part cavity 15 and hardened to form a casting. The core outer surface 24 is exposed to the molten material and forms the inner part surface of the casting. The second shell surface 32 forms the outer part surface of the casting. It should be understood that the core inner surface 22 is fluidly isolated from the part cavity 15 and is not exposed to the molten material during casting.
[0045] It should also be understood that the described aspects of the casting assembly 10 can have other exemplary embodiments. In another example, the shell 30 partially surrounds the core 20 to form an outer edge or outer tip of the casting, such as by a closed end or cap at one end of the shell 30 facing the core 20.
[0046] Steering Figure 2 , a side cross-sectional view of the cast assembly 10 shows additional details of the part cavity 15 and the hollow cavity 25. The axial direction A and the first horizontal axis H1 are shown.
[0047] The part cavity width 19 is defined between the second shell surface 32 and the core outer surface 24. The hollow cavity width 29 is defined by the core inner surface 22. In the exemplary embodiment shown, the part cavity width 19 and the hollow cavity width 29 are variable along the axial direction A. The hollow cavity width 29 is narrowed at the first end 26 and the second end 28 of the core 20. The hollow cavity width 29 is also widened in the portion of the core 20 spaced apart from the first end 26 and the second end 28. In other words, as shown, the hollow cavity width 29 has a maximum value at a position spaced apart from the first end 26 and the second end 28. In addition, as shown, the part cavity width 19 is constant in one portion of the part cavity 15 and variable along the axial direction A in another portion of the part cavity 15. It should be understood that the part cavity 15 and the hollow cavity 25 can have a variety of geometric profiles along the axial direction A. In this manner, in some exemplary embodiments, either or both of the part cavity width 19 or the hollow cavity width 29 are constant or variable along the axial direction A.
[0048] In some embodiments, the casting assembly 10 may further include one or more ligaments. In the example shown, a first ligament 41 and a second ligament 42 are disposed in the casting assembly 10. The first ligament 41 and the second ligament 42 extend from the core 20 through the part cavity 15 to the shell 30. In the example shown, the first ligament 41 and the second ligament 42 also partially extend into the page, as shown in FIG. Figure 3 shown.
[0049] As shown, the first ligament 41 and the second ligament 42 are each separate components coupled to the first body 20 and the second body 30. In some embodiments, the first ligament 41 and the second ligament 42 are integrally formed or additively manufactured with at least one of the core 20 or the shell 30. In some embodiments, the core 20, the shell 30, the first ligament 41 and the second ligament 42 are formed as a single integral component by an additive manufacturing method. Such ligaments form hollow holes extending through the casting, such as cooling holes, slots, etc.
[0050] Figure 3-5 Shown along Figure 2 Referring now to FIG. 1 , various cross-sectional views of the casting assembly 10 are taken along common parallel planes indicated by lines III-III, IV-IV, and VV. Figure 3 , showing that along Figure 21 is an axial cross-sectional view of the casting assembly 10 along line III-III. A first cross-sectional view 101 (also referred to herein as "first plane 101") corresponding to line III-III is shown for reference. A first horizontal axis H1 and a second horizontal axis H2 are also shown for reference. It should be understood that the axial direction A ( Figure 2 ) is perpendicular to the first cross section 101.
[0051] The first plane 101 is located at the second ends 28, 38 of the first body 20 and the second body 30. Figure 3 In the axial view of FIG. 2 , the core inner surface 22 is shown forming a variable hollow cavity width 29 as described above.
[0052] In the first plane 101, the maximum core thickness CT max and minimum core thickness CT min is defined between the core inner surface 22 and the core outer surface 24. As shown, the core inner surface 22 defines a hollow area A h , and the core outer surface 24 defines a main body area A b In addition, in the first plane 101 , a minimum shell thickness ST is defined between the second shell surface 32 and the first shell surface 31 in the shell 30 . min .
[0053] Figure 4 Shown along Figure 2 1 is another axial cross-sectional view of the casting assembly 10 along line IV-IV. A second cross-sectional view 102 (also referred to herein as "second plane 102") corresponding to line IV-IV is shown for reference. The first horizontal axis H1 and the second horizontal axis H2 are also shown for reference. It should be understood that the second plane 102 is perpendicular to the axial direction A ( Figure 2 ).
[0054] In the second plane 102, the maximum core thickness CT in the core 20 is shown. max , minimum core thickness CT min , hollow area A h and the main body area A b The minimum shell thickness ST of the shell 30 is also shown. min It should be understood that the maximum core thickness CT max , minimum core thickness CT min , hollow area A h 、Main body area A b or minimum shell thickness ST min Can vary in different cross sections.
[0055] In addition, the first ligament 41 and the second ligament 42 each define a ligament thickness 43 as shown. In some embodiments, the minimum core thickness CTmin Between 0.9-40 times the ligament thickness 43.
[0056] Figure 5 Shown along Figure 2 1 is another cross-sectional view of the casting assembly 10 along line VV. A third cross-section 103 (also referred to herein as "third plane 103") corresponding to line VV is shown for reference. A first horizontal axis H1 and a second horizontal axis H2 are also shown for reference. It should be understood that the axial direction A ( Figure 2 ) is perpendicular to the third plane 103.
[0057] In the third plane 103, the maximum core thickness CT in the core 20 is shown. max , minimum core thickness CT min , hollow area A h and the main body area A b The minimum shell thickness ST of the shell 30 is also shown. min A second ligament 42 is also provided in the casting assembly 10. The second ligament 42 extends from the core 20 through the part cavity 15 to the shell 30. In the non-limiting embodiment shown, the second ligament 42 forms a support structure between the core 20 and the shell 30. It should be understood that the ligament can be provided in any portion of the part cavity 15.
[0058] General Reference Figure 1-5 , main body area A b , hollow area A h , minimum core thickness CT min , Maximum core thickness CT max or minimum shell thickness ST min At least one of the core thicknesses CT is non-constant along the axial direction. For example, the maximum core thickness CT in the third plane 103 is greater than that in the first plane 101. max As shown in the figure, the main body area A b Along the axial direction A is constant, while the hollow area A h , minimum core thickness CT min , Maximum core thickness CT max and minimum shell thickness ST min Each of is non-constant along the axial direction A.
[0059] When the core 20 is manufactured by additive manufacturing, the hollow cavity 25 reduces the core thickness, which results in a reduction in the printing force or internal stress in the portion of the core 20 during printing. In addition, during casting and firing, the hollow cavity 25 provides a reduction in core thickness, so that the thermal characteristics of the first body 20 and the second body 30 are more similar to those of the solid core 20. As described above, this matching of thermal characteristics between the casting assembly 10 and the casting reduces the internal stress in the casting and the shear force or other forces on the casting assembly 10. In addition, the size of the hollow cavity 25 in the core 20 can be set or customized to anticipate the shrinkage that occurs during the firing of the casting assembly 10, which can improve the accuracy of the dimensions of the casting. For example, in some exemplary embodiments, the casting assembly 10 is used to form a thin-walled casting with a part cavity 15 that is sensitive to shrinkage or other casting irregularities. In this case, the core 20 is provided with a corresponding large hollow cavity 25 to improve the thermal similarity with the thin-walled casting. The hollow cavity 25 being fluidly isolated from the part cavity 15 further provides for easier removal from the casting, as the core 20 may be crushed, segmented, etc. for removal from either the first end 36 or the second end 38 .
[0060] Steering Figure 6 , another casting assembly 110 according to various aspects described herein is shown. The casting assembly 110 is similar to the casting assembly 10; therefore, like parts will be described with like reference numerals plus 100, and it should be understood that the description of like parts of the casting assembly 10 applies to the casting assembly 110 unless otherwise specified.
[0061] The casting assembly 110 is formed to pass through a cross section similar to the first cross section 101 ( Figure 3 ) is shown in cross section 201. A first horizontal axis H1 and a second horizontal axis H2 are also shown for reference. It should be understood that the axial direction A ( Figure 2 ) is perpendicular to cross section 201.
[0062] A housing 130 is provided that includes a first housing surface 131 and a second housing surface 132. The second housing surface 132 defines a part cavity 115, as shown. In some embodiments, the first housing surface 131 defines an outer surface of the housing 130. In some embodiments, the housing 130 includes an additional cavity or hollow area defined by the first housing surface 131.
[0063] In the illustrated example, the shell 130 is a single body having a first shell surface 131 and a second shell surface 132. In another non-limiting embodiment, the shell 130 includes a central body having an outer layer, shell, skin, etc. defining the first shell surface 131, and a central body having an inner layer, shell, skin, etc. defining the second shell surface 132.
[0064] One difference compared to casting assembly 10 is that casting assembly 110 includes multiple cores within part cavity 115. As shown, a first core 120A, a second core 120B, and a third core 120C are positioned within part cavity 115. Any number of cores may be provided.
[0065] The first, second and third cores 120A, 120B, 120C are similar to the core 20 ( Figure 2 ). The first core 120A and the second core 120B include respective first and second inner surfaces 122A, 122B and respective first and second outer surfaces 124A, 124B. The first and second inner surfaces 122A, 122B define respective first and second hollow cavities 125A, 125B. The first and second hollow cavities 125A, 125B are both fluidically isolated from the part cavity 115.
[0066] The third core 120C includes a third outer surface 124C. Another difference compared to the casting assembly 10 is that the third core 120C is a solid body without a hollow cavity.
[0067] In the example shown, the first core 120A is a single body having a first inner surface 122A and a first outer surface 124A, and the third core 120C is a single body having a third outer surface 124C. Another difference compared to the casting assembly 10 is that the second core 120B includes a center body 150 coupled to a shell or outer layer 152. In the non-limiting embodiment shown, the center body 150 defines the second inner surface 122B, and the outer layer 152 defines the second outer surface 124B. In one non-limiting embodiment, at least one of the center body 150 or the outer layer 152 includes at least one of a ceramic material, a metallic material, alumina, silica, zircon, molybdenum, tungsten, aluminum, or a combination thereof. In yet another non-limiting embodiment, at least one of the first or third cores 120A, 120C includes a center body having an outer layer, shell, skin, etc. that defines the corresponding first outer surface 124A or third outer surface 124C. In another non-limiting embodiment, the first core 120A includes an inner layer, shell, skin, etc. that defines a first inner surface 122A.
[0068] In the cross section 201, the minimum first core thickness CT min,A and the maximum first core thickness CT max,A The first inner surface 122A defines a first hollow area A. h,A , and the first outer surface 124A defines a first body area A b,A, as shown in the figure. In addition, in the cross section 201, a minimum shell thickness ST is defined between the second shell surface 132 and the first shell surface 131 in the shell 130. min .
[0069] Figure 7 Additional details of the casting assembly 110 are shown. In cross section 201, the minimum second core thickness CT min,B and the maximum second core thickness CT max,B is defined between the second inner surface 122B and the second outer surface 124B. It should be understood that the minimum second core thickness CT min,B and the maximum second core thickness CT max,B The second inner surface 122B defines a second hollow area A. h,B , and the second outer surface 124B defines a second main body area A b,B , as shown in the figure.
[0070] Reference now Figure 8 , another casting assembly 210 according to various aspects described herein is shown. The casting assembly 210 is similar to the casting assemblies 10, 110; therefore, like parts will be described with like reference numerals further increased by 100, and it should be understood that the description of like parts of the casting assemblies 10, 110 applies to the casting assembly 210 unless otherwise specified.
[0071] The casting assembly 210 is formed to pass through a cross section similar to the first cross section 101 ( Figure 3 ) and cross section 201( Figure 6 ) is shown in cross section 301. The first horizontal axis H1 and the second horizontal axis H2 are also shown for reference. It should be understood that the axial direction A ( Figure 2 ) is perpendicular to cross section 301.
[0072] A core 220 is provided, which includes a core outer surface 224. One difference compared to the casting assembly 10, 110 is that multiple core inner surfaces are provided in the core 220. More specifically, the core 220 includes a first core inner surface 222A and a second core inner surface 222B. As shown, the first core inner surface 222A and the second core inner surface 222B define a respective first hollow cavity 225A and a second hollow cavity 225B.
[0073] Another difference compared to the casting assembly 10, 110 is that the core 220 includes a center body 250 coupled to an outer shell or outer layer 252 and an inner layer 254. In one non-limiting example, at least one of the center body 250, the outer layer 252, or the inner layer 254 includes at least one of a ceramic material, a metallic material, alumina, silica, zircon, molybdenum, tungsten, aluminum, or a combination thereof. In the non-limiting embodiment shown, the outer layer 252 defines a core outer surface 224, the inner layer 254 defines a second shell surface 222B, and the center body 250 defines a core inner surface 222A. In another non-limiting embodiment, the core 220 includes a single or unitary body portion that defines the core outer surface 224 and the inner surfaces 222A, 222B.
[0074] A housing 230 is also provided, which includes a first housing surface 231 and a second housing surface 232. The second housing surface 232 defines a part cavity 215, as shown. In some embodiments, the first housing surface 231 defines an outer surface of the housing 230. In some embodiments, the housing 230 includes an additional cavity or hollow area defined by the first housing surface 231.
[0075] In the illustrated example, the shell 230 is a single body having a first shell surface 231 and a second shell surface 232. In another non-limiting embodiment, the shell 230 includes a central body having an outer layer, shell, skin, etc. defining the first shell surface 231, and a central body having an inner layer, shell, skin, etc. defining the second shell surface 232.
[0076] In cross section 301, the minimum core thickness CT min,A and maximum core thickness CT max,A Each of the cores is defined between the inner surface 222A and the core outer surface 224. It should be understood that the minimum core thickness CT min,A and maximum core thickness CT max,A The inner surface 222A defines a hollow area A. h,A and the core outer surface 224 defines a main body area A b In addition, in the cross section 301 , a minimum shell thickness ST is defined between the second shell surface 232 and the first shell surface 231 in the shell 230 . min .
[0077] Fig. 9 Additional details of the casting assembly 210 are shown. In cross section 301, the minimum core thickness CT min,B and maximum core thickness CT max,B Each of the cores is defined between the inner surface 222B and the core outer surface 224. It should be understood that the minimum core thickness CT min,B and maximum core thickness CTmax,B The inner surface 222 defines a hollow area A. h,B , and the core outer surface 224 defines a main body area A b,B .
[0078] General Reference Figure 1-9 , when the core 20, 120A, 120B, 120C, 220 is manufactured by additive manufacturing, the hollow cavity 25, 125A, 125B, 225A, 225B reduces the maximum core thickness compared to a solid core, which reduces the printing force on the core, which may otherwise cause stress or deformation of the core as described above. Regardless of whether the core 20, 120A, 120B, 120C, 220 is made by additive manufacturing, the hollow cavity 25, 125A, 125B, 225A, 225B also provides a reduced thickness difference between the core and the casting, which improves the similarity of thermal characteristics of all bodies in the casting assembly 10, 110, 210 during casting and firing, thereby resulting in a reduction of internal stress, deformation, shrinkage, etc. in the casting assembly and the casting.
[0079] As mentioned previously, finding a feasible casting component design for a given casting involves finding a balance between casting design parameters, corresponding casting component dimensions, material property considerations, and thermal property considerations during printing, firing, and casting. These are labor-intensive and time-intensive processes.
[0080] Table 1 below shows some examples of casting components that produce possible solutions to the above problems. Each casting component example describes a casting component having one or more hollow cavities (e.g., hollow cavity 25 in core 20) as described above. Figure 2 )、Second core 120B( Figure 6 ) in the hollow cavity 125B, or the core 220 ( Figure 8 ) in the hollow cavity 225B) of the core body of the minimum core thickness CT min , Maximum core thickness CT max and hollow area A h It will also be appreciated that for each of the following cast component examples, the minimum core thickness CT min , Maximum core thickness CT max and hollow area A h The value of is for a single common cross section, such as the first plane 101 ( Figure 3 )、cross section 201( Figure 6 ) or cross section 301( Figure 8 ).
[0081] Table 1
[0082]
[0083] During the time-consuming process of designing the casting assembly described above, it was unexpectedly discovered that the main body area A b , hollow area A h , minimum core thickness CT min , Maximum core thickness CT max and minimum shell thickness ST min The inventors have discovered that an improved casting assembly and corresponding castings cannot be easily, consistently or reliably found based on performing different experiments, each using different casting assembly dimensions. Instead, better and more durable casting assemblies and castings are found when the casting assembly includes at least one core having a hollow cavity and the casting assembly has specific dimensions in a specific relationship to each other. This result is unexpected.
[0084] The desired relationship is expressed in terms of the hollow cavity parameter (denoted as "HCP"):
[0085]
[0086] Among them A b is the main body area, A h is the hollow cavity area, CT min is the minimum core thickness, CT max is the maximum core thickness, ST min is the minimum shell thickness in a single cross section through the cast component 10, 110, 210. More specifically, the hollow cavity parameter HCP relates to the ratio A of the hollow cavity area to the body area. h / A b , the ratio of the maximum core thickness to the minimum core thickness CT max / CT min and the ratio of the minimum shell thickness to the minimum core thickness ST min / CT min .
[0087] Expression (1) is valid for a single cross section through the casting component 10, 110, 210 perpendicular to the axial direction A, such as the first plane 101, the second plane 102, the third plane 103, the cross section 201, or the cross section 301 as described above. In some embodiments, expression (1) is also valid for each cross section through the casting component 10, 110, 210 that is orthogonal to the axial direction A. For each hollow cavity in the casting component 10, 110, 210, such as the hollow cavity 25 ( Figure 2 )、Hollow cavities 125A, 125B ( Figure 6 ) or hollow cavities 225A, 225B ( Figure 8 ), expression (1) is also valid.
[0088] By utilizing this relationship, the inventors have also discovered that the number of casting component designs that provide suitable or feasible solutions for a given casting design can be greatly reduced at the outset, thereby facilitating a more rapid down-selection of casting component designs to be considered for a given casting. The discovered relationship provides more insight into the requirements of a given casting component and also avoids or prevents late redesign of a desired casting.
[0089] Area Ratio A h / A b , thickness ratio CT max / CT min and ST min / CT min , and the values of the hollow cavity parameter HCP corresponding to the above examples 1-7 are provided in the following Table 2:
[0090] Table 2
[0091]
[0092] The range of values of the hollow cavity parameter HCP in Table 2 was found to be relevant for cast components with cores having hollow cavities adjacent to ligaments, thereby reducing the variability of thermal properties and stresses during firing and casting, while also providing a method for casting parts (e.g., airfoils) having large internal cavities directly adjacent to small holes formed by ligaments in the cast components.
[0093] Additionally, the minimum and maximum values for the cast component properties described in Table 2, where expression (1) is applicable and consistent with the teachings of the present disclosure, are provided in Table 3 below:
[0094] Table 3
[0095]
[0096] As shown above, it was found that the design range of the hollow cavity parameter HCP was 0.04-8.28, providing for the desired casting component, ligament stability, material effects during printing, thermal effects during firing and casting, and material quality of the finished casting. The inventors also found that the design range of the hollow cavity parameter HCP was narrowed, providing particularly desirable properties for the casting component to form a casting. In an exemplary embodiment, the hollow cavity parameter HCP is between 0.07-4.51. In another exemplary embodiment, the hollow cavity parameter HCP is between 0.09-3.34. This narrowed design range provides a more effective selection of casting component characteristics, as well as the associated savings in time and resources.
[0097] Additional benefits associated with the Hollow Cavity Parameters HCP described herein include rapid evaluation of design parameters in terms of relative cavity size, wall thickness, and thermal properties. Limiting these multiple factors to a specific range of possibilities can save time, money, and resources. Additional restriction of the Hollow Cavity Parameters HCP to a narrower design range allows for faster evaluation of design parameters and more efficient exploration of cast component characteristics within a suitable design space. Furthermore, the HCP described herein enables the development and production of high-performance and durable castings across multiple performance metrics within a given set of constraints.
[0098] To the extent that one or more of the structures provided herein are known in the art, it should be understood that the present disclosure may include combinations of previously unknown structures for reasons based at least in part on conflicts of interest and penalties, desired modes of operation, or other forms of reasons taught in the art.
[0099] This written description uses examples to disclose the present disclosure, including the best mode, and also to enable any person skilled in the art to practice the present disclosure, including making and using any devices or systems and performing any incorporated methods. The patentable scope of the present disclosure is defined by the claims, and may include other examples that occur to those skilled in the art. Such other examples are intended to fall within the scope of the claims if they include structural elements that do not differ from the literal language of the claims, or if they include equivalent structural elements that do not differ substantially from the literal language of the claims.
[0100] Further aspects of the disclosure are provided by the subject matter of the following clauses:
[0101] A casting assembly for forming a casting and defining an axial direction, comprising: a core extending along the axial direction between a first end and a second end, the core having a core inner surface and a core outer surface, wherein the core inner surface at least partially defines a hollow cavity, and wherein the core outer surface is fluidically isolated from the hollow cavity and shapes a part surface of the casting; and a shell extending along the axial direction and having a first shell surface and a second shell surface, wherein at least a portion of the second shell surface faces the core outer surface of the core; wherein the core comprises: a main body area A b , the main body area A b is defined as the area bounded by the outer surface of the core in a cross section through the casting assembly, wherein the axial direction is perpendicular to the cross section; the hollow area A h , the hollow area A h Defined as the area of the hollow cavity bounded by the core inner surface in the cross section; Minimum core thickness CT min , the minimum core thickness CT mindefined in the cross section between the core outer surface and the core inner surface; and a maximum core thickness CT max , the maximum core thickness CT max defined in the cross section between the core outer surface and the core inner surface; wherein the shell comprises a minimum shell thickness ST defined in the cross section between the first shell surface and the second shell surface min ; wherein the main body area A b , the hollow area A h , the minimum core thickness CT min , the maximum core thickness CT max and the minimum shell thickness ST min The hollow cavity parameter HCP is defined as:
[0102]
[0103] Wherein, the hollow cavity parameter HCP is between 0.04-8.28 (0.04≤HCP≤8.28).
[0104] The cast component according to any preceding clause, wherein in all cross sections perpendicular to the axial direction between the first end and the second end, the hollow cavity parameter HCP is between 0.04-8.28 (0.04≤HCP≤8.28).
[0105] The cast component according to any preceding clause, wherein the hollow cavity parameter HCP is between 0.07-4.51 (0.07≤HCP≤4.51).
[0106] The cast component according to any preceding clause, wherein in all cross sections perpendicular to the axial direction between the first end and the second end, the hollow cavity parameter HCP is between 0.07-4.51 (0.07≤HCP≤4.51).
[0107] The cast component according to any preceding clause, wherein the hollow cavity parameter HCP is between 0.09-3.34 (0.09≤HCP≤3.34).
[0108] The cast component according to any preceding clause, wherein in all cross sections perpendicular to the axial direction between the first end and the second end, the hollow cavity parameter HCP is between 0.09-3.34 (0.09≤HCP≤3.34).
[0109] A casting component according to any preceding clause, wherein the hollow area A h With the main body area A bThe ratio is between 0.02-0.99 (0.02≤A h / A b ≤0.99).
[0110] A cast component according to any preceding clause, wherein the maximum core thickness CT max With the minimum core thickness CT min The ratio is between 1.00-9.80 (1.00≤CT max / CT min ≤9.80).
[0111] A cast component according to any preceding clause, wherein the minimum shell thickness ST min With the minimum core thickness CT min The ratio is between 0.36-18.17 (0.36≤ST min / CT min ≤18.17).
[0112] A casting assembly according to any preceding clause, wherein the body area A b , the hollow area A h , the minimum core thickness CT min , the maximum core thickness CT max or the minimum shell thickness ST min At least one of is non-constant along the axial direction.
[0113] A casting assembly as described in any preceding clause, further comprising a second shell surface defining a second hollow cavity in the core.
[0114] A casting assembly as claimed in any preceding clause, wherein the hollow cavity defines a hollow cavity width that is variable along the axial direction.
[0115] A casting assembly as described in any preceding clause wherein the hollow cavity defines a constant hollow cavity width along the axial direction.
[0116] A casting assembly as claimed in any preceding clause, wherein the hollow cavity width has a maximum value at a location spaced from the first end and the second end.
[0117] A casting assembly as described in any preceding clause, wherein the core outer surface and the second shell surface at least partially define a part cavity, wherein the part cavity is fluidly isolated from the hollow cavity.
[0118] A cast assembly as claimed in any preceding clause, wherein the part cavity defines a part cavity width that is variable along the axial direction.
[0119] A cast assembly as claimed in any preceding clause, wherein the part cavity defines a part cavity width that is constant along the axial direction.
[0120] A casting assembly as described in any preceding clause, further comprising a ligament extending between the core and the shell.
[0121] A casting assembly as claimed in any preceding clause wherein the ligament forms a hollow bore extending through the casting.
[0122] A casting assembly as described in any preceding clause wherein the ligament forms a support structure between the core and the shell.
[0123] A casting assembly as in any preceding clause, wherein the core comprises a center body coupled to an outer layer, wherein the center body defines the core inner surface and the outer layer defines the core outer surface.
[0124] The casting assembly of any preceding clause, wherein the core further comprises an inner layer coupled to the center body and defining the core inner surface.
[0125] A cast component as described in any preceding clause, wherein at least one of the core or the shell comprises monolithic ceramic.
Claims
1. A casting assembly for forming a casting and defining an axial direction, characterized in that include: a core extending along the axial direction between a first end and a second end, the core having an inner core surface and an outer core surface, wherein the inner core surface at least partially defines a hollow cavity, and wherein the outer core surface is fluidly isolated from the hollow cavity and shapes a part surface of the casting; as well as a shell extending along the axial direction and having a first shell surface and a second shell surface, wherein at least a portion of the second shell surface faces the core outer surface of the core body; The core comprises: Main body area A b , the main body area A b is defined as the area bounded by the outer surface of the core in a cross section through the casting assembly, wherein the axial direction is perpendicular to the cross section; Hollow area A h , the hollow area A h defined as the area of said hollow cavity bounded by said core inner surface in said cross section; Minimum core thickness CT min , the minimum core thickness CT min defined in said cross section between said core outer surface and said core inner surface; and Maximum core thickness CT max , the maximum core thickness CT max defined in said cross section between said core outer surface and said core inner surface; wherein the shell comprises a minimum shell thickness ST defined between the first shell surface and the second shell surface in the cross section min ; The main body area A b , the hollow area A h , the minimum core thickness CT min , the maximum core thickness CT max and the minimum shell thickness ST min The hollow cavity parameter HCP is defined as: The hollow cavity parameter HCP is between 0.04 and 8.28 (0.04≤HCP≤8.28).
2. The casting assembly according to claim 1, characterized in that In all cross sections between the first end and the second end that are perpendicular to the axial direction, the hollow cavity parameter HCP is between 0.04 and 8.28 (0.04≤HCP≤8.28).
3. The casting assembly according to claim 1, characterized in that The hollow cavity parameter HCP is between 0.07 and 4.51 (0.07≤HCP≤4.51).
4. The casting assembly according to claim 3, characterized in that In all cross sections between the first end and the second end that are perpendicular to the axial direction, the hollow cavity parameter HCP is between 0.07 and 4.51 (0.07≤HCP≤4.51).
5. The casting assembly according to claim 1, characterized in that The hollow cavity parameter HCP is between 0.09 and 3.34 (0.09≤HCP≤3.34).
6. The casting assembly according to claim 5, characterized in that In all cross sections perpendicular to the axial direction between the first end and the second end, the hollow cavity parameter HCP is between 0.09 and 3.34 (0.09≤HCP≤3.34).
7. The casting assembly according to claim 1, characterized in that The hollow area A h With the main body area A b The ratio is between 0.02-0.99 (0.02≤A h / A b ≤0.99).
8. The casting assembly according to claim 1, characterized in that Where the maximum core thickness CT max With the minimum core thickness CT min The ratio is between 1.00-9.80 (1.00≤CT max / CT min ≤9.80).
9. The casting assembly according to claim 1, characterized in that The minimum shell thickness ST min With the minimum core thickness CT min The ratio is between 0.36-18.17 (0.36≤ST min / CT min ≤18.17).
10. The casting assembly according to claim 1, characterized in that The main body area A b , the hollow area A h , the minimum core thickness CT min , the maximum core thickness CT max or the minimum shell thickness ST min At least one of is non-constant along the axial direction.