Control method for increasing pulling speed in round billet continuous casting

By employing technologies such as crystallizer feeding strip, progressive cooling nozzles, electromagnetic stirring, and non-sinusoidal vibration devices during the continuous casting process of round billets, the problem of uneven cooling was solved, enabling the production of high-speed and high-quality billets.

CN118989272AInactive Publication Date: 2024-11-22WUHAN GAOZHIDA CONTINUOUS CASTING INTELLIGENT TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410962165.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the continuous casting process of round billets, uneven cooling affects the increase of billet casting speed, and existing technologies make it difficult to achieve higher casting speeds while ensuring billet quality.

Method used

The process employs crystallizer feeding strip technology, secondary cooling nozzles with alternating strong and weak intervals in a ring distribution, crystallizer electromagnetic stirring and end electromagnetic synchronous stirring, dynamic water control technology, and a non-sinusoidal vibration device, combined with a quadratic function model for full-process digital control, to optimize the uniformity of billet cooling.

Benefits of technology

This improved the cooling uniformity and quality of the billet under high casting speed, shortened maintenance time, and increased production efficiency and billet surface quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989272A_ABST
    Figure CN118989272A_ABST
Patent Text Reader

Abstract

The invention discloses a control method for increasing the pulling speed in round billet continuous casting. The control method comprises the steps that S1, the superheat degree of tundish molten steel is stably controlled to be 27 + / -5 DEG C; s2, feeding a steel belt into molten steel of the crystallizer; s3, the width of a crystallizer water tank is 6 mm, and the depth of the water tank is 8 mm. By means of the crystallizer steel belt feeding technology, the superheat degree of molten steel in a crystallizer can be reduced, the solidification process is improved, the length of a casting blank liquid core is shortened, secondary cooling spraying section nozzles are annularly distributed in a strong-weak progressive interval staggered mode, and a zero section and a first section are arranged to be high-pressure full water so that the cooling efficiency of a high-temperature section can be enhanced; other sections are subjected to aerial fog cooling so as to relieve the surface temperature returning overspeed of the casting blank, the maintenance time is shortened, a dynamic water control technology is adopted, and the whole-course digital control over the liquid core length, the center temperature, the surface temperature and the blank shell thickness of the casting blank is achieved through a quadratic function model water distribution curve; and better casting blank surface quality can be obtained in a high-pulling-speed state by adopting a non-sinusoidal vibration process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting, and in particular to a control method for increasing the casting speed of round billet continuous casting. Background Art

[0002] In the field of continuous casting technology, round billet and square billet continuous casting machines have strict requirements for cooling. However, the cooling of round billet continuous casting is different from that of square billet. Square billet is mainly cooled in the middle of each surface, while the corners are generally avoided from spraying to avoid overcooling and cracking. Whether round billet continuous casting is primary cooling or secondary cooling, it requires full-cycle cooling of the billet without dead corners, so its uniformity requirements are higher. Whether the billet is cooled evenly will directly affect the increase of the billet drawing speed.

[0003] There are two main uses for round billets for subsequent processes: one is to be used for direct pipe threading, which has very high requirements on the shape and surface quality of the round billet, as well as the level of inclusions and surface cracks; the other is to provide billets for bar rolling mills, which have very high requirements on the internal structure of the round billet, such as center segregation, center porosity, and internal cracks.

[0004] To increase the casting speed of round billet continuous casting, a higher casting speed should be achieved under the premise of ensuring stable and good billet quality. However, in the actual production process, with the increase of casting speed, in addition to ensuring uniform cooling as mentioned above, several important key nodes are the core points of the present invention:

[0005] 1) Use stable low superheat pouring; 2) Feed steel strip or wire into the crystallizer to obtain better primary grain structure and lower superheat; 3) Use water tank crystallizer to obtain uniform cooling characteristics of full-circle one-time cooling; Use large-taper double-taper crystallizer to obtain high-speed strong cooling state to meet the requirements of rapid cooling and shrinkage of the billet in the crystallizer; 4) The nozzles are arranged in an intermittent ring, with progressive distribution from top to bottom, and full arc arrangement, and the zero section and the first section are set to high-pressure full water, and the other sections are gas mist cooling; 5) Use crystallizer electromagnetic stirring and end electromagnetic stirring at the same time to obtain better internal crystal structure of the billet; 6) Use dynamic water control technology to achieve full digital control of the billet liquid core length, center temperature, surface temperature, and billet shell thickness; 7) Use excess metallurgical length to obtain sufficient shrinkage compensation space under high pulling speed conditions. 8) Use non-sinusoidal vibration device to control the surface quality of the billet to obtain better under high pulling speed conditions.

[0006] Therefore, whether the round billet continuous casting is cooled evenly and uniformly is an important factor affecting the billet drawing speed. How to improve the billet drawing speed of round billet continuous casting is an urgent problem that needs to be solved. Summary of the invention

[0007] In view of the problems in the related art, the present invention proposes a control method for increasing the casting speed of round billet continuous casting to overcome the above-mentioned technical problems existing in the existing related art.

[0008] To this end, the specific technical solution adopted by the present invention is as follows:

[0009] A control method for increasing the casting speed of round billet continuous casting, comprising:

[0010] Step S1, stably controlling the superheat of molten steel in the tundish at 27±5°C;

[0011] Step S2, feeding the steel strip into the molten steel in the crystallizer;

[0012] Step S3, the width of the crystallizer water tank is 6 mm, the depth is 8 mm, and the flow rate and water pressure of the cooling water at the water tank are greater than 12 m / min and greater than 1.2 MPa respectively;

[0013] Step S4, the nozzles of the secondary cooling spray section are arranged in a staggered annular pattern with progressively strong and weak nozzles;

[0014] Step S5, using electromagnetic stirring in the crystallizer and synchronous electromagnetic stirring at the end;

[0015] Step S6, by calculating and detecting the length of the liquid core of the ingot, the surface of the ingot, the cross-sectional temperature and the solidification thickness, adjusting the water volume and the heat exchange amount in real time, and making the data into a quadratic function model;

[0016] Step S7: the crystallizer vibration device adopts non-sinusoidal vibration.

[0017] Preferably, in step S1, the ladle and the tundish are covered, and argon sealing devices are added at the water inlets of the ladle and the tundish.

[0018] Preferably, in step S3, the length of the crystallizer copper tube is 900 mm.

[0019] Preferably, in step S3, the taper of the crystallizer is a double taper, with an upper taper of 2.8% / m and a lower taper of 0.7% / m.

[0020] Preferably, in step S4, the nozzle adopts an adjustment ratio nozzle, and the adjustment ratio is 1:15.

[0021] Preferably, in step S2, the thickness of the steel strip is 1.0-2.0 mm, and the width of the steel strip is 10-50 mm.

[0022] Preferably, in step S2, the speed at which the belt feeder feeds the steel belt is 2-15 m / min.

[0023] Preferably, in step S2, the amount of the steel strip fed is 0.3%-1.2% / ton of steel.

[0024] Beneficial effects of the present invention:

[0025] The present invention reduces the superheat of molten steel in the crystallizer, improves the solidification process, and shortens the liquid core length of the ingot by using the crystallizer steel strip feeding technology. The secondary cooling spray section nozzles are arranged in an annular manner with strong and weak progressive intervals. The zero section and the first section are set to high-pressure full water to enhance the cooling efficiency of the high-temperature section. The other sections are gas mist cooling to alleviate the excessive temperature recovery of the ingot surface and shorten the maintenance time. The dynamic water control technology is adopted, and the quadratic function model water distribution curve is used to realize full digital control of the liquid core length, center temperature, surface temperature, and shell thickness of the ingot. The non-sinusoidal vibration process is adopted to obtain better ingot surface quality under high pulling speed conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 is a flow chart of a control method for increasing the casting speed of round billet continuous casting according to an embodiment of the present invention;

[0028] Figure 2 is a graph showing the relationship between the water volume and the casting speed of a round billet Ø210 mm according to an embodiment of the present invention;

[0029] Figure 3 This is a temperature distribution diagram of the cross section of a round billet with a diameter of 210 mm when the liquid core length is 5 m according to an embodiment of the present invention;

[0030] Figure 4 This is a temperature distribution diagram of the cross section of a round billet with a diameter of 210 mm when the liquid core length is 18 m according to an embodiment of the present invention;

[0031] Figure 5 It is a surface and center temperature distribution diagram of a round billet Ø210 mm and a billet shell thickness variation diagram according to an embodiment of the present invention;

[0032] Figure 6 is a schematic diagram of a non-sinusoidal curve using an overall function method according to an embodiment of the present invention;

[0033] Figure 7 It is a schematic diagram of the structure of the crystallizer feeding steel strip according to an embodiment of the present invention.

[0034] In the figure:

[0035] 1. Steel strip coil; 2. Strip feeder; 3. Crystallizer. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] According to an embodiment of the present invention, a control method for increasing the casting speed of round billet continuous casting is provided.

[0038] Embodiment 1;

[0039] like Figure 1 As shown, a control method for increasing the casting speed of round billet continuous casting according to an embodiment of the present invention comprises:

[0040] Step S1, the superheat of the molten steel in the tundish is stably controlled at 22°C, the ladle and the tundish are covered, and an argon sealing device is added at the water inlet of the ladle and the tundish;

[0041] Step S2, feeding a steel strip into the molten steel of the crystallizer, the thickness of the steel strip is 1.0 mm, the width of the steel strip is 10 mm, the speed of the steel strip feeding machine is 5 m / min, and the amount of the steel strip fed is 0.3% / ton of steel;

[0042] Step S3, the width of the crystallizer water tank is 6 mm, the depth is 8 mm, the flow rate and water pressure of the cooling water at the water tank are greater than 12 m / min and greater than 1.2 MPa respectively, the length of the crystallizer copper tube is 900 mm, the crystallizer taper is double taper, the upper taper is 2.8% / m, and the lower taper is 0.7% / m;

[0043] Step S4, the secondary cooling spray section nozzles are arranged in a staggered annular pattern with progressively strong and weak nozzles, and the nozzles are adjustment ratio nozzles with an adjustment ratio of 1:15;

[0044] Step S5, using electromagnetic stirring in the crystallizer and synchronous electromagnetic stirring at the end;

[0045] Step S6, by calculating and detecting the length of the liquid core of the ingot, the surface of the ingot, the cross-sectional temperature and the solidification thickness, adjusting the water volume and the heat exchange amount in real time, and making the data into a quadratic function model;

[0046] Step S7: the crystallizer vibration device adopts non-sinusoidal vibration.

[0047] Embodiment 2:

[0048] like Figure 1 As shown, a control method for increasing the casting speed of round billet continuous casting according to an embodiment of the present invention comprises:

[0049] Step S1, the superheat of the molten steel in the tundish is stably controlled at 27°C, the ladle and the tundish are covered, and an argon sealing device is added at the water inlet of the ladle and the tundish;

[0050] Step S2, feeding a steel strip into the molten steel of the crystallizer, the thickness of the steel strip is 1.5 mm, the width of the steel strip is 30 mm, the speed of the steel strip feeding machine is 10 m / min, and the amount of the steel strip fed is 0.9% / ton of steel;

[0051] Step S3, the width of the crystallizer water tank is 6 mm, the depth is 8 mm, the flow rate and water pressure of the cooling water at the water tank are greater than 12 m / min and greater than 1.2 MPa respectively, the length of the crystallizer copper tube is 900 mm, the crystallizer taper is double taper, the upper taper is 2.8% / m, and the lower taper is 0.7% / m;

[0052] Step S4, the secondary cooling spray section nozzles are arranged in a staggered annular pattern with progressively strong and weak nozzles, and the nozzles are adjustment ratio nozzles with an adjustment ratio of 1:15;

[0053] Step S5, using electromagnetic stirring in the crystallizer and synchronous electromagnetic stirring at the end;

[0054] Step S6, by calculating and detecting the length of the liquid core of the ingot, the surface of the ingot, the cross-sectional temperature and the solidification thickness, adjusting the water volume and the heat exchange amount in real time, and making the data into a quadratic function model;

[0055] Step S7: the crystallizer vibration device adopts non-sinusoidal vibration.

[0056] Embodiment three;

[0057] like Figure 1 As shown, a control method for increasing the casting speed of round billet continuous casting according to an embodiment of the present invention comprises:

[0058] Step S1, the superheat of the molten steel in the tundish is stably controlled at 32°C, the ladle and the tundish are covered, and an argon sealing device is added at the water inlet of the ladle and the tundish;

[0059] Step S2, feeding a steel strip into the molten steel of the crystallizer, the thickness of the steel strip is 2.0 mm, the width of the steel strip is 50 mm, the speed of the steel strip feeding machine is 15 m / min, and the amount of the steel strip fed is 1.2% / ton of steel;

[0060] Step S3, the width of the crystallizer water tank is 6 mm, the depth is 8 mm, the flow rate and water pressure of the cooling water at the water tank are greater than 12 m / min and greater than 1.2 MPa respectively, the length of the crystallizer copper tube is 900 mm, the crystallizer taper is double taper, the upper taper is 2.8% / m, and the lower taper is 0.7% / m;

[0061] Step S4, the secondary cooling spray section nozzles are arranged in a staggered annular pattern with progressively strong and weak nozzles, and the nozzles are adjustment ratio nozzles with an adjustment ratio of 1:15;

[0062] Step S5, using electromagnetic stirring in the crystallizer and synchronous electromagnetic stirring at the end;

[0063] Step S6, by calculating and detecting the length of the liquid core of the ingot, the surface of the ingot, the cross-sectional temperature and the solidification thickness, adjusting the water volume and the heat exchange amount in real time, and making the data into a quadratic function model;

[0064] Step S7: the crystallizer vibration device adopts non-sinusoidal vibration.

[0065] In order to facilitate understanding of the above technical solution of the present invention, the above technical solution of the present invention is further explained below based on specific detailed steps.

[0066] Through further explanation on feeding steel strip into molten steel in crystallizer, staggered annular distribution of nozzles in secondary cooling spray section with progressive strong and weak intervals, quadratic function model and non-sinusoidal vibration of crystallizer vibration device, a more systematic scheme to improve the continuous casting speed of round billet is proposed.

[0067] 1. In the above step S2, if Figure 7 As shown, the crystallizer feeding steel belt technology can reduce the superheat of molten steel in the crystallizer, improve the solidification process, and shorten the length of the liquid core of the ingot; at the same time, the vibration of the steel belt will break up the formed dendrites, promote nucleation, and increase the nucleation rate, thereby increasing the equiaxed crystal area and improving the ingot quality and production efficiency.

[0068] 1. In the above step S2, if Figure 7 As shown, the crystallizer feeding steel belt technology can reduce the superheat of molten steel in the crystallizer, improve the solidification process, and shorten the length of the liquid core of the ingot; at the same time, the vibration of the steel belt will break up the formed dendrites, promote nucleation, and increase the nucleation rate, thereby increasing the equiaxed crystal area and improving the ingot quality and production efficiency.

[0069] The technical parameters of the crystallizer feeding steel strip are shown in the following table:

[0070] Steel belt size 1.0-2.0mm, width 10-50mm Feeding speed 0-15m / min Feeding steel belt quantity 0.3-1.2% / ton steel

[0071] 2. In the above step S4, the nozzles of the secondary cooling spray section are arranged in a staggered annular pattern with progressive intervals of strong and weak, and a large adjustment ratio nozzle (adjustment ratio is 1:15) is used. The zero section and the first section can be set to high-pressure full water to enhance the cooling efficiency of the high-temperature section, and the other sections are gas mist cooling to alleviate the over-speed temperature recovery of the surface of the casting. Due to the use of a large adjustment ratio nozzle, except for the zero section, the nozzles can take into account both the low casting speed water flow and the high casting speed water flow, which greatly reduces the types of nozzles and shortens the maintenance time to 80% of the original

[0072] 3. In the above step S5, the crystallizer electromagnetic stirring and the end electromagnetic stirring are used simultaneously to obtain a better internal crystal structure of the ingot: the main function of the crystallizer electromagnetic stirring is to increase the equiaxed crystal rate and reduce the developed columnar crystals; the main function of the end electromagnetic stirring is to reduce the end center segregation and improve the looseness of the ingot center.

[0073] 4. In the above step S6, dynamic water control technology is adopted, and the quadratic function model water distribution curve is used to realize full digital control of the liquid core length, center temperature, surface temperature and shell thickness of the ingot: by calculating and detecting the liquid core length, surface temperature and solidification thickness of the ingot, the water volume and heat exchange amount are adjusted in real time, so that the continuous casting machine can always maintain a high pulling speed limit state for a long time and stably, and ensure that the continuous casting machine does not have quality problems. The present invention emphasizes that the intelligent model calculates and monitors the movement state of the ingot, which can maximize the pulling speed. Taking the round billet Ф210 as an example, the relationship between the water volume and the pulling speed control obtained by the secondary cooling water volume control model is as follows Figure 2 As shown; the temperature distribution obtained by the temperature calculation model of the billet cross section is as follows Figure 3 and Figure 4 As shown; the thickness variation relationship obtained by the solidification model of the ingot is as follows Figure 5 shown.

[0074] 5. In the above step S6, excess metallurgical length is used to obtain sufficient shrinkage compensation space under higher casting speed conditions. The traditional calculation formula is:

[0075]

[0076] Where, L M is the metallurgical length, D is the round billet diameter, V is the pulling speed, and η is the solidification coefficient.

[0077] The liquid core length is positively correlated with the drawing speed and is also a limiting factor of the drawing speed. In the traditional design process, when the drawing speed is increased, the solidification coefficient is increased by increasing the cooling intensity, thereby balancing the increase in metallurgical length caused by the increase in the drawing speed. However, excessive increase in cooling intensity of many steel grades will affect the quality of the ingot, especially for crack-sensitive steel grades. Therefore, the present invention proposes that an excess metallurgical length should be used in the early stage of continuous casting machine design, which helps to achieve a higher drawing speed without affecting the quality of the ingot.

[0078] 6. In the above step S7, the non-sinusoidal vibration process can obtain better surface quality of the ingot under high casting speed. The double-unit hydraulic vibration adopted by the original casting machine, in addition to the partial modification of the guide mechanism, will re-compile the hydraulic non-sinusoidal vibration curve, adopt the double-unit non-sinusoidal software technology developed by Gaozhida, and can provide a variety of vibration control models according to different steel types. The technical features are as follows:

[0079] A. Non-sinusoidal curves use the overall function method; specifically, Figure 6 As shown, the acceleration curve of the non-sinusoidal vibration curve is continuous and smooth, avoiding the discontinuity of the traditional piecewise function acceleration curve and the sudden change caused by the change of the inertia force of the vibration mass, thereby affecting the stability of the vibration.

[0080] B. The control model takes the control of negative slip time as the core control target; the increase of negative slip time, that is, the increase of the time for the crystallizer to move downward relative to the billet, during which the billet shell is subjected to compression, is beneficial to the quality of the billet; but on the other hand, it will cause the amount of protection slag to penetrate between the billet shell and the crystallizer wall to decrease, which is not conducive to the improvement of the lubrication and heat transfer conditions of the billet. Therefore, the selection of negative slip time should not be too large or too small. Under the same vibration conditions, the negative slip time of non-sinusoidal waveforms is smaller than that of sinusoidal waveforms, and decreases with the increase of waveform deflection rate. When selecting the target negative slip time, it should be different for sinusoidal waveforms and non-sinusoidal waveforms. Combining the actual application of production and theoretical calculations, it is shown that for sinusoidal waveforms, the target negative slip time is usually between 0.15 and 0.25; for non-sinusoidal waveforms, due to the effect of deflection rate, the target negative slip time is further reduced, usually between 0.10 and 0.20.

[0081] C. Non-sinusoidal synchronization model adopts V--f, h synchronization control model; namely:

[0082] f=-BV C +C

[0083] h=MV C +N

[0084] Where f is the frequency, h is the amplitude, V C is the pulling speed; B, C, M, N are model setting constants.

[0085] The biggest advantage of this control model is that, within a certain range, as the pulling speed increases, the frequency gradually decreases, while the amplitude increases, and the negative sliding time remains relatively constant within the optimal range. In this way, when achieving high pulling speed, it not only takes into account the good lubrication of the protective slag, but also ensures the good vibration mark depth and surface quality of the ingot.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A control method for increasing the casting speed of round billet continuous casting, characterized in that: include: Step S1, stably controlling the superheat of molten steel in the tundish at 27±5°C; Step S2, feeding the steel strip into the molten steel in the crystallizer; Step S3, the width of the crystallizer water tank is 6 mm, the depth is 8 mm, and the flow rate and water pressure of the cooling water at the water tank are greater than 12 m / min and greater than 1.2 MPa respectively; Step S4, the nozzles of the secondary cooling spray section are arranged in a staggered annular pattern with progressively strong and weak nozzles; Step S5, using electromagnetic stirring in the crystallizer and synchronous electromagnetic stirring at the end; Step S6, by calculating and detecting the length of the liquid core of the ingot, the surface of the ingot, the cross-sectional temperature and the solidification thickness, adjusting the water volume and the heat exchange amount in real time, and making the data into a quadratic function model; Step S7: the crystallizer vibration device adopts non-sinusoidal vibration.

2. A control method for increasing the casting speed of round billet continuous casting according to claim 1, characterized in that: In the step S1, the ladle and the tundish are covered, and argon sealing devices are added at the water inlets of the ladle and the tundish.

3. The method for controlling round billet continuous casting to increase casting speed according to claim 1, characterized in that: In step S3, the length of the crystallizer copper tube is 900 mm.

4. A control method for increasing casting speed of round billet continuous casting according to claim 1, characterized in that: In step S3, the taper of the crystallizer is a double taper, with an upper taper of 2.8% / m and a lower taper of 0.7% / m.

5. The method for controlling round billet continuous casting to increase casting speed according to claim 1, characterized in that: In step S4, the nozzle adopts an adjustment ratio nozzle, and the adjustment ratio is 1:

15.

6. A control method for increasing casting speed of round billet continuous casting according to claim 1, characterized in that: In step S2, the thickness of the steel strip is 1.0-2.0 mm, and the width of the steel strip is 10-50 mm.

7. A control method for increasing casting speed of round billet continuous casting according to claim 1, characterized in that: In step S2, the speed of the steel strip fed by the strip feeder is 2-15 m / min.

8. The method for controlling round billet continuous casting to increase casting speed according to claim 1, characterized in that: In the step S2, the amount of the steel strip fed is 0.3%-1.2% / ton of steel.

Citation Information

Patent Citations

  • Continuous casting secondary cooling dynamic control method based on online temperature measuring and heat transferring model

    CN102814481A

  • Method for improving blank casting temperature by using blank shell thickness control system

    CN104759599A

  • System method for intelligent control over continuous-casting process

    CN106180619A

  • Method for controlling drawing speed of billet

    CN111618266A

  • Method for direct intervening of internal quality of casting blank

    CN1876274A