Method for repairing surface damage of undercarriage suspended beam connecting lug
By preparing wire materials through wire cutting and controlling the welding temperature with a water-cooling device, and using a cold welding machine and electric spark welding technology for progressive heat input repair, the problems of heat-affected zone and hydrogen embrittlement risk in the existing technology are solved, and efficient repair and performance improvement of landing gear lug parts are achieved.
Patent Information
- Application Number
- CN202410999439.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing technologies for repairing surface damage to landing gear lugs in aviation equipment pose risks of thermal impact leading to performance degradation and hydrogen embrittlement, thus affecting the service performance of the equipment.
Rectangular wires and cylindrical rods were prepared using wire cutting technology. After hydrogen removal treatment, the welding temperature was controlled by a water cooling device. Gradual heat input repair was performed using a cold welding machine and electric spark welding technology. Subsequently, laser shock peening was carried out to ensure low hydrogen content and reduce heat impact. Finally, fine repair and experimental verification were performed.
Hydrogen was effectively removed, the thermal impact was reduced, and the hardness and mechanical properties of the repaired area were improved, ensuring that the repaired landing gear lug parts met or exceeded their original performance.
Smart Images

Figure CN118989857A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of remanufacturing, and in particular to a method for repairing surface damage of a landing gear pylon lug. Background Art
[0002] After long-term service, especially in marine environments, stress corrosion of the landing gear lugs of aviation equipment can cause surface cracks, affecting the service safety of the aviation equipment.
[0003] Conventional welding repair methods may cause problems such as thermal effects leading to reduced performance, which in turn affects the service performance of the equipment. Patent CN115026460A discloses a method for preparing welding wire and a method for online repairing surface cracks of 1Cr15Ni4Mo3N substrate using the welding wire, which can be used to repair surface damage of landing gear pylon lugs and achieve equal strength welding, but this method does not completely eliminate the risk of hydrogen embrittlement. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a method for repairing the surface damage of the landing gear pylon lug.
[0005] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0006] A method for repairing the surface damage of a landing gear pylon lug comprises the following steps:
[0007] Step 1: Perform flaw detection and polishing on the landing gear ear parts to eliminate the damaged areas:
[0008] Use magnetic particle or dye flaw detection on the landing gear ear parts to determine the damaged area. First, grind the damaged area to reduce the thickness to 0.6-0.8mm. Then inspect again to check whether there is a damaged area. If there is, continue grinding, removing 0.2-0.4mm each time, until no damaged area is found in the flaw detection, and use acetone to clean the damaged area.
[0009] Step 2: Cutting rectangular wires and cylindrical rods from raw material bars or plates of corresponding grades of landing gear lug parts using a wire cutting process;
[0010] Step 3: Dehydrogenate the rectangular wire and the cylindrical rod at a temperature of 500-550° C. for 8-15 hours;
[0011] Step 4: sandblast the rectangular wire and the cylindrical rod to remove the oxide layer on the surface of the rectangular wire and the cylindrical rod, then use acetone to remove the oil stains on the rectangular wire and the cylindrical rod, and use a hair dryer to heat and air dry;
[0012] Step 5: Design a water cooling device and install it on the landing gear lug parts:
[0013] A cylindrical boss is provided at the front side of the water cooling device. Thermal conductive silicone grease is applied on the cylindrical surface of the cylindrical boss and inserted into the cylindrical hole on the landing gear ear part. After the thermal conductive silicone grease solidifies, the water cooling device is fixed on the landing gear ear part.
[0014] Step 6: Use a cold welding machine to remelt the damaged part. The process parameters of the remelting process are current 1 to 8A and welding time 1 to 5ms.
[0015] Step 7: Use the electric spark welding repair machine to perform the first surface welding on the damaged part after the base remelting:
[0016] The cylindrical rod prepared in steps 2 to 4 is selected as the electrode rod, and the surface surfacing process parameters are power 900-1500W, frequency 280-500HZ, voltage 60-80V, and argon gas flow rate 5-8L / min. The electrode rod rotates and contacts the surface of the part to emit electric sparks to form a surfacing layer. The thickness of the part before and after surfacing is measured using an external groove digital display vernier caliper to obtain the thickness of the surfacing layer;
[0017] Step 8: Use a cold welding machine to remelt the cladding layer formed in step 7. The remelting process parameters of the cladding layer are current 9-15A and welding time 6-15ms;
[0018] Step 9, repeat steps 7 to 8 for four times, so that the total thickness of the cladding layer is greater than 0.4 mm;
[0019] Step 10: Use a cold welding machine to perform wire feeding welding repair, the thickness of a single repair welding is 0.5-0.7mm:
[0020] Use a cold welding machine to weld the rectangular wire prepared in step 2 to step 4 to the damaged part, the wire feeding welding repair process parameters are current 15-40A, welding time 15-40ms, and during the repair welding process, argon and nitrogen mixed gas is used for protection, and the nitrogen volume mixing ratio is 0.5-2%;
[0021] Step 11: Use block dry ice to close to the welding repair position for cold treatment for 2-4 hours;
[0022] Step 12: Perform laser shock strengthening on the repair welding area of the landing gear ear parts, with the process parameters of laser energy 4-8J, spot size 2-4mm, and overlap rate 30-70%;
[0023] Step 13: Use an electric grinder to grind the laser shock peening surface to make the surface smooth, and then use acetone to clean the damaged area;
[0024] Step 14, repeating Step 10 to Step 13 until the thickness of the landing gear ear part after repair is greater than the required thickness by more than 0.1mm. If the thickness of the last welding repair is less than 0.5mm, the thickness of the landing gear ear part after repair can be greater than the required thickness by more than 0.1mm. In this case, the thickness of the last welding repair can be less than 0.5mm. If the thickness after one wire feeding welding repair is greater than the required thickness by more than 0.1mm, there is no need to repeat Step 10 to Step 13. Drain the water in the water cooling device, use a hair dryer to blow hot air at the joint between the cylindrical boss on the water cooling device and the landing gear ear part, so that the thermal conductive silicone grease can restore a certain fluidity, and remove the water cooling device.
[0025] Step 15: Grind and fine-tune the repaired landing gear lug parts to make the dimensions of the landing gear lug parts meet the use requirements;
[0026] Step 16: Prepare test pieces to verify the repair effect:
[0027] The test piece material is the material of the corresponding grade of the landing gear lug parts. The test pieces include repaired parts and reference parts. The repaired parts are test pieces with artificial defects and repaired. The reference parts are treated with the heat treatment process during the manufacturing of the landing gear lugs. The performance of the repaired parts and the reference parts are compared to judge the effect after the repair.
[0028] Step 17. Artificially process the surface of the repaired part to a depth equivalent to the defect removed in step 1, use the rectangular wire and cylindrical rod processed in steps 2 to 4 for welding repair, repeat steps 5 to 15 in the repair process, and process the repaired part and the reference part into strength test specimens and fatigue test specimens. Compare the tensile strength of the repaired part with that of the reference part, and the fatigue performance of the repaired part with that of the reference part. The fatigue test load is 800 MPa and the stress ratio is 0.1. If it is not broken after 10,000 times, it is considered to have passed. If the tensile strength of the repaired part reaches more than 95% of the performance of the reference part and the fatigue performance passes the fatigue test, it is determined that the landing gear ear part has been repaired successfully.
[0029] Preferably, in step 2, the rectangular wire has a width dimension of 0.5-0.7 mm, a height dimension of 0.5-0.7 mm, and a length dimension of ≥150 mm, and the cylindrical rod has a diameter dimension of 2-6 mm and a length of 80-100 mm.
[0030] Preferably, the sandblasting process parameters in step 4 include: using corundum sand or quartz sand, with a particle size of 180 mesh or more, and a pressure of 0.3 to 0.6 MPa.
[0031] Preferably, a water inlet is provided at the bottom of the water cooling device and a water outlet is provided at the top. The water cooling device is made of copper material and uses flowing water at room temperature.
[0032] Preferably, the diameter of the cylindrical boss on the water cooling device is 0.5 mm smaller than the diameter of the cylindrical hole on the landing gear ear part.
[0033] Preferably, the thickness of the first cladding layer in step seven is controlled to be 80-100 μm.
[0034] The beneficial effects of the present invention are:
[0035] The invention adopts a high-temperature dehydrogenation process of 500-550°C to ensure thorough dehydrogenation and ensure that the hydrogen content after dehydrogenation is less than 0.0008%, thereby reducing the hydrogen content of rectangular wires and cylindrical rods. Compared with the prior art, the invention can more completely remove hydrogen from the material; adopts a progressively increasing heat input method to increase the heat input in an area far away from the substrate, thereby greatly reducing the thermal impact on the substrate area and ensuring the mechanical properties of the welding repair; adjusts the welding temperature to room temperature, and there is no condensed water on the surface of the parts, thereby avoiding the risk of hydrogen embrittlement induced by condensed water during the welding process; during the repair welding process, argon and nitrogen mixed gas is used for protection, so that the nitrogen element in the repair welding area is supplemented during the repair welding process; cold treatment is performed on the welding repair area by using dry ice, so that the material in the repair welding area undergoes a transformation from metastable austenite to martensite, thereby improving the hardness of the repair area; after remelting by using a cold welding machine, defects can be greatly reduced, and the surfacing layer can be changed into a dense remelting layer; and laser shock strengthening can be carried out to ensure that both the repair welding area and the heat affected zone are in a compressive stress state. In addition, the shock wave of the laser strengthening process will cause micro-area deformation of the material in the repair welding area, thereby inducing phase transformation, causing metastable austenite to transform into martensite, and increasing the dislocation density, further improving the hardness of the repair welding area, making the repair welding area exceed the hardness of the matrix, and improving the comprehensive mechanical properties of the repaired sample. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present invention is further described below in conjunction with the accompanying drawings and embodiments:
[0037] Figure 1 The figure is a schematic diagram of the structure of the damaged landing gear lug parts;
[0038] Figure 2 It is a schematic diagram of the structure of the water cooling device in the present invention.
[0039] In the figure: 1. Landing gear ear parts; 2. Damaged area; 3. Cylindrical hole; 4. Water cooling device; 5. Water inlet; 6. Water outlet; 7. Cylindrical boss. DETAILED DESCRIPTION
[0040] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to the accompanying drawings and embodiments.
[0041] A method for repairing the surface damage of a landing gear pylon lug comprises the following steps:
[0042] Step 1: Perform flaw detection and polishing on the landing gear ear part 1 to eliminate the damaged area. Figure 1 , which is a schematic structural diagram of the landing gear ear part 1.
[0043] Use magnetic powder or dye flaw detection on landing gear ear part 1 to determine damaged area 2. Use an electric grinder to grind the damaged area, and use an external groove digital display vernier caliper to measure the thickness of the grinded area. For the first time, grind the damaged area 2 to reduce the thickness to 0.6-0.8mm, and then perform flaw detection again to check whether there is damaged area 2. If there is, continue grinding, removing 0.2-0.4mm of thickness each time, until no damaged area 2 is found in the flaw detection, and use acetone to clean the damaged area.
[0044] Landing gear lug parts 1 Surface cracks caused by stress corrosion are usually caused by stress corrosion. The depth is usually about 1mm. Step grinding + flaw detection is used. The first grinding depth is 0.6-0.8mm, and then each grinding is 0.2-0.4mm. This avoids excessive welding areas caused by excessive grinding depth, and also avoids waste of resources caused by excessive grinding and flaw detection. Usually 1-3 times can remove defects.
[0045] In this embodiment, the specific thickness reduction by the first grinding is 0.7 mm, the specific thickness reduction by the subsequent grinding is 0.3 mm, and the total thickness reduction is 1 mm.
[0046] Step 2: Cut rectangular parallelepiped wires and cylindrical rods from the raw material bar or plate of the landing gear ear part 1 corresponding to the grade 1Cr15Ni4Mo3N by wire cutting technology. The rectangular parallelepiped wire has a width dimension of 0.5-0.7 mm, a height dimension of 0.5-0.7 mm, and a length dimension of ≥150 mm. The cylindrical rod has a diameter dimension of 2-6 mm and a length of 80-100 mm.
[0047] In this embodiment, the width dimension of the rectangular wire is specifically 0.6 mm, the height dimension is specifically 0.6 mm, and the length dimension is specifically 180 mm, and the diameter dimension of the cylindrical rod is specifically 4 mm and the length is 100 mm.
[0048] Step 3: Dehydrogenate the rectangular wire and the cylindrical rod at a temperature of 500-550°C for 8-15 hours. Ensure that the dehydrogenation is thorough and the hydrogen content after dehydrogenation is less than 0.0008%, thereby reducing the hydrogen content of the rectangular wire and the cylindrical rod.
[0049] In this embodiment, the rectangular wire and the cylindrical rod are subjected to dehydrogenation treatment at a temperature of 520° C. for a holding time of 10 hours to ensure thorough dehydrogenation.
[0050] The hydrogen binding energy of weak hydrogen traps such as dislocations and grain boundaries in steel is lower than 55 kJ / mol, and the peak temperature of hydrogen escape during material heating is generally between 100 and 200 ° C. For hydrogen traps such as carbide precipitation phase, the binding energy is as high as 140 kJ / mol, and the peak temperature of hydrogen escape is about 400 ° C. Obviously, the dehydrogenation treatment temperature specified in the prior art (such as patent CN115026460A) is 200 ° C, which is difficult to remove hydrogen in the carbide precipitation phase hydrogen traps, while the dehydrogenation temperature in the present invention is 520 ° C, which can more completely remove hydrogen from the material.
[0051] Step 4: sandblast the rectangular wire and the cylindrical rod using corundum sand or quartz sand with a particle size of 180 mesh or more and a pressure of 0.3-0.6 MPa to remove the surface oxide layer of the rectangular wire and the cylindrical rod, then use acetone to remove oil stains on the rectangular wire and the cylindrical rod, and use a hair dryer to heat and air dry.
[0052] In this embodiment, the sandblasting pressure is specifically 0.5 MPa.
[0053] Step 5: Design a water cooling device 4 and install the water cooling device 4 on the landing gear ear part 1. Figure 2 , which is a schematic structural diagram of the water cooling device 4.
[0054] The water cooling device 4 is provided with a water inlet 5 at the bottom and a water outlet 6 at the top. A cylindrical boss 7 is provided at the front side of the water cooling device 4. The diameter of the cylindrical boss 7 is 0.5 mm smaller than the diameter of the cylindrical hole 3 on the landing gear lug part 1. Thermal conductive silicone grease is applied on the cylindrical surface of the cylindrical boss 7 and inserted into the cylindrical hole 3 on the landing gear lug part 1. After the thermal conductive silicone grease solidifies, the water cooling device 4 is fixed to the landing gear lug part 1.
[0055] The material of the water cooling device 4 is copper, and the water cooling device uses running water, the water temperature is room temperature, and the welding temperature is room temperature. In the prior art (such as patent CN115026460A), the 1Cr15Ni4Mo3N matrix is cooled to make its pre-welding temperature in the range of 0 to 5°C. If the temperature of the part is too low, water in the air will continue to condense onto the surface of the part. The presence of water during the welding process will cause the risk of hydrogen embrittlement. In the present invention, the welding temperature is room temperature, there is no condensed water on the surface of the part, and the risk of hydrogen embrittlement induced by condensed water during the welding process is avoided.
[0056] In this embodiment, the water temperature is controlled at 25° C. Water flows in from the water inlet 5 at the bottom of the water cooling device 4 and flows out from the water outlet 6 at the top.
[0057] Use a thermometer to constantly monitor the surface temperature of the landing gear lug part 1 during the welding process. When the temperature measured by the thermometer reaches above 50°C, wait for the temperature to cool down before continuing the repair welding.
[0058] Step 6: Use a cold welding machine to remelt the damaged part. The process parameters of the remelting process are current 1 to 8A and welding time 1 to 5ms.
[0059] In this embodiment, a cold welding machine is used to remelt the damaged part of the substrate. The substrate remelting process is 5A current and the welding time is 5ms.
[0060] Step 7: Use the electric spark welding repair machine to perform the first surface welding on the damaged part after the base remelting:
[0061] The cylindrical rod prepared in steps 2 to 4 is selected as the electrode rod. The surface surfacing process parameters are power 900-1500W, frequency 280-500HZ, voltage 60-80V, and argon gas flow rate 5-8L / min. The electrode rod rotates and contacts the surface of the part to emit electric sparks to form a surfacing layer. The thickness of the part before and after surfacing is measured using an external groove digital display vernier caliper to obtain the thickness of the surfacing layer. The thickness of the first surfacing layer is controlled at 80-100μm.
[0062] In this embodiment, an electric spark surfacing repair machine is used to perform the first surface surfacing on the damaged part that has been remelted by the substrate. The cylindrical rod prepared in steps 2 to 4 is selected as the electrode rod. The surface surfacing process is 1400W power, 400HZ frequency, 60V voltage, and 6L / min argon gas flow. The electrode rod rotates, contacts the surface of the part to emit electric sparks, and forms a surfacing layer. The thickness of the part before and after surfacing is measured with an external groove digital display vernier caliper to obtain the thickness of the surfacing layer. The thickness of the first surfacing layer is 90μm.
[0063] Step eight, using a cold welding machine to remelt the cladding layer formed in step seven, the cladding layer remelting process parameters are current 9-15A, welding time 6-15ms.
[0064] In this embodiment, a cold welding machine is used to remelt the cladding layer formed in step 7. The remelting process parameters of the cladding layer are current 10A and welding time 8ms.
[0065] Step 9: Repeat steps 7 to 8 four times to make the total thickness of the cladding layer greater than 0.4 mm.
[0066] In this embodiment, steps 7 to 8 are repeated four times, and the total thickness of the surfacing layer is 0.45 mm.
[0067] Step 10: Use a cold welding machine to perform wire feeding welding repair, the thickness of a single repair welding is 0.5-0.7mm:
[0068] Use a cold welding machine to weld the rectangular wire prepared in steps two to four to the damaged part. The wire feeding welding repair process parameters are current 15-40A and welding time 15-40ms. During the repair welding process, argon and nitrogen mixed gas is used for protection. The nitrogen volume mixing ratio is 0.5-2%, so that the nitrogen element in the repair welding area is obtained during the repair welding process.
[0069] In this embodiment, a cold welding machine is used for wire feeding welding repair, and the repair welding thickness is 0.7mm. The rectangular wire prepared in steps 2 to 4 is welded to the damaged part using a cold welding machine. The wire feeding welding repair process has a current of 20A and a welding time of 20ms. During the repair welding process, argon and nitrogen mixed gas is used for protection, and the nitrogen volume mixing ratio is 1%.
[0070] The weakened welding performance area is caused by the coarsening of fine precipitation phases of the base material caused by heat input. The greater the heat input, the more serious the performance weakening.
[0071] The present invention adopts a progressive heat input method, and the heat input is increased only in the area far away from the substrate. Specifically, the substrate is remelted, five times of electric spark surfacing + low energy surfacing layer remelting, and cold welding wire feeding welding repair method greatly reduces the thermal impact on the substrate area. Due to the small heat input, the thermally affected weakened zone is small, only about 0.05mm, and the reduction in tensile strength after welding repair does not exceed 3%, ensuring the mechanical properties of the welding repair.
[0072] Step 11: Use block dry ice to cold treat the welding repair position for 2-4 hours.
[0073] Use dry ice to cold treat the welding repair area, so that the material in the repair area undergoes a transformation from metastable austenite to martensite, thereby increasing the hardness of the repair area.
[0074] In this embodiment, block dry ice is used to perform cold treatment close to the welding repair position for 4 hours.
[0075] Step 12: laser shock strengthening is performed on the repair welding area of the landing gear ear part 1, and the process parameters are laser energy 4-8J, spot size 2-4mm, and overlap rate 30-70%.
[0076] In this embodiment, the repair welding area of the part is subjected to laser shock strengthening, and the specific process parameters are laser energy 5J, spot size 2.5mm, and overlap rate 40%.
[0077] Compared with traditional strengthening processes, the compressive stress area of laser shock strengthening can reach more than 1.5mm, which can ensure that the repair welding area and the heat-affected zone are in a compressive stress state. In addition, the shock wave of the laser strengthening process will cause micro-area deformation of the material in the repair welding area, thereby inducing phase transformation, causing metastable austenite to transform into martensite, and increase dislocation density, improve the hardness of the repair welding area, make the repair welding area exceed the matrix hardness, and improve the comprehensive mechanical properties of the repaired sample.
[0078] Step 13: Use an electric grinder to grind the laser shock intensive surface to make the surface smooth, and then use acetone to clean the damaged area.
[0079] Step 14, repeat steps 10 to 13 until the thickness of the landing gear ear part 1 after repair is greater than the required thickness by more than 0.1mm. If the thickness of the last welding repair is less than 0.5mm, the thickness of the landing gear ear part 1 after repair can be greater than the required thickness by more than 0.1mm. In this case, the thickness of the last welding repair can be less than 0.5mm. If the thickness after one wire feeding welding repair is greater than the required thickness by more than 0.1mm, there is no need to repeat steps 10 to 13. Drain the water in the water cooling device 4, use a hair dryer to blow hot air on the joint between the cylindrical boss 7 on the water cooling device 4 and the landing gear ear part 1, so that the thermal conductive silicone grease can restore a certain fluidity, and remove the water cooling device 4.
[0080] In this embodiment, the total thickness of the wire feeding welding repair is 1.15mm, and the removed thickness is only 1mm, that is, the thickness after the wire feeding welding repair is more than 0.1mm greater than the required thickness. There is no need to repeat steps 10 to 13. The water in the water cooling device 4 is released, and a hair dryer is used to blow hot air at the joint between the cylindrical boss 7 on the water cooling device 4 and the landing gear ear part 1 to restore a certain fluidity of the thermal conductive silicone grease, and the water cooling device 4 is removed.
[0081] Step 15: Grind and fine-tune the repaired landing gear lug part 1 so that the size of the landing gear lug part (1) meets the use requirements.
[0082] Step 16: Prepare test pieces to verify the repair effect:
[0083] The material of the test piece is 1Cr15Ni4Mo3N material corresponding to the landing gear part 1. The test piece includes a repaired piece and a reference piece. The repaired piece is a test piece with artificial defects and repaired, which is used to characterize the performance of the landing gear lug part 1 repaired by steps one to fifteen; the reference part is treated with the heat treatment process during the manufacturing of the landing gear lug, which is used to characterize the initial comprehensive performance of the landing gear lug part 1; comparing the performance of the repaired piece and the reference piece is used to judge the effect after the repair.
[0084] In this embodiment, the reference part is treated by the heat treatment process used in the manufacturing of the landing gear lug, specifically 1050°C×60min, oil cooling; -70°C×2h, air cooling; 350°C×3h, air cooling.
[0085] Step 17. Artificially process the surface of the repaired part to a depth equivalent to the defect removed in step 1, use the rectangular wire and cylindrical rod processed in steps 2 to 4 for welding repair, repeat steps 5 to 15 in the repair process, and process the repaired part and the reference part into strength test specimens and fatigue test specimens. Compare the tensile strength of the repaired part with that of the reference part, and the fatigue performance of the repaired part with that of the reference part. The fatigue test load is 800 MPa, and the stress ratio is 0.1. If it is not broken after 10,000 times, it is considered to have passed. If the tensile strength of the repaired part reaches more than 95% of the performance of the reference part, and the fatigue performance passes the fatigue test, it is determined that the landing gear ear part 1 has been repaired successfully.
[0086] In this embodiment, a 1mm deep defect is artificially processed on the surface of the repaired part, and the repair process follows the ear part repair process. The tensile strength of the reference part was measured to be 1440MPa, 1450MPa, and 1451MPa. The tensile strength of the repaired part was measured to be 1416MPa, 1425MPa, and 1423Mpa. The average tensile strength of the control part was 1447MPa, and the average tensile strength of the repaired part was 1421MPa. The tensile strength of the repaired part reached 98.3% of the reference part. The fatigue test load was 800MPa, the stress ratio was 0.1, and it was considered passed if it did not break after 10,000 times. Three reference parts and three repaired parts did not break after 10,000 fatigue tests. The tensile strength of the repaired part reached more than 95% of the performance of the reference part, and the fatigue performance passed the fatigue test, and it was determined that the landing gear ear part 1 was successfully repaired.
[0087] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for repairing the surface damage of a landing gear pylon lug, characterized in that: The following steps are involved: Step 1: Perform flaw detection and polishing on the landing gear lug parts (1) to eliminate the damaged areas: Use magnetic particle or dye flaw detection on the landing gear ear part (1) to determine the damaged area (2), first grind the damaged area (2) to reduce the thickness to 0.6-0.8 mm, perform flaw detection again to detect whether there is a damaged area (2), if there is, continue grinding, each time removing 0.2-0.4 mm of thickness, until no damaged area (2) is found by flaw detection, and use acetone to clean the damaged area; Step 2: Cutting rectangular wires and cylindrical rods from the raw material rods or plates of the corresponding grades of the landing gear lug parts (1) using a wire cutting process; Step 3: Dehydrogenate the rectangular wire and the cylindrical rod at a temperature of 500-550° C. for 8-15 hours; Step 4: sandblast the rectangular wire and the cylindrical rod to remove the oxide layer on the surface of the rectangular wire and the cylindrical rod, then use acetone to remove the oil stains on the rectangular wire and the cylindrical rod, and use a hair dryer to heat and air dry; Step 5: Design a water cooling device (4) and install the water cooling device (4) on the landing gear ear part (1): A cylindrical boss (7) is provided on the front side of the water cooling device (4); thermal conductive silicone grease is applied on the cylindrical surface of the cylindrical boss (7) and inserted into the cylindrical hole (3) on the landing gear ear part (1); after the thermal conductive silicone grease solidifies, the water cooling device (4) is fixed on the landing gear ear part (1); Step 6: Use a cold welding machine to remelt the damaged part. The process parameters of the remelting process are current 1 to 8A and welding time 1 to 5ms. Step 7: Use the electric spark welding repair machine to perform the first surface welding on the damaged part after the base remelting: The cylindrical rod prepared in steps 2 to 4 is selected as the electrode rod, and the surface surfacing process parameters are power 900-1500W, frequency 280-500HZ, voltage 60-80V, and argon gas flow rate 5-8L / min. The electrode rod rotates and contacts the surface of the part to emit electric sparks to form a surfacing layer. The thickness of the part before and after surfacing is measured using an external groove digital display vernier caliper to obtain the thickness of the surfacing layer; Step 8: Use a cold welding machine to remelt the cladding layer formed in step 7. The remelting process parameters of the cladding layer are current 9-15A and welding time 6-15ms; Step 9, repeat steps 7 to 8 for four times, so that the total thickness of the cladding layer is greater than 0.4 mm; Step 10: Use a cold welding machine to perform wire feeding welding repair, the thickness of a single repair welding is 0.5-0.7mm: Use a cold welding machine to weld the rectangular wire prepared in step 2 to step 4 to the damaged part, the wire feeding welding repair process parameters are current 15-40A, welding time 15-40ms, and during the repair welding process, argon and nitrogen mixed gas is used for protection, and the nitrogen volume mixing ratio is 0.5-2%; Step 11: Use block dry ice to close to the welding repair position for cold treatment for 2-4 hours; Step 12: laser shock peening is performed on the repair welding area of the landing gear ear part (1), and the process parameters are laser energy 4-8J, spot size 2-4mm, and overlap rate 30-70%; Step 13: Use an electric grinder to grind the laser shock intensive surface to make the surface smooth, and then use acetone to clean the damaged area; Step 14, repeating Step 10 to Step 13 until the thickness of the landing gear ear part (1) after repair is greater than the required thickness by more than 0.1 mm. If the thickness of the last welding repair is less than 0.5 mm, the thickness of the landing gear ear part (1) after repair can be greater than the required thickness by more than 0.1 mm. In this case, the thickness of the last welding repair can be less than 0.5 mm. If the thickness after one wire feeding welding repair is greater than the required thickness by more than 0.1 mm, it is not necessary to repeat Step 10 to Step 13. Drain the water in the water cooling device (4), use a hair dryer to blow hot air at the joint between the cylindrical boss (7) on the water cooling device (4) and the landing gear ear part (1), so that the thermal conductive silicone grease can restore a certain fluidity, and remove the water cooling device (4); Step 15: polish and fine-tune the repaired landing gear lug part (1) so that the size of the landing gear lug part (1) meets the use requirements; Step 16: Prepare test pieces to verify the repair effect: The material of the test piece is the material of the corresponding grade of the landing gear lug part (1). The test piece includes a repaired piece and a reference piece. The repaired piece is a test piece with artificial defects and repaired. The reference piece is treated with the heat treatment process during the manufacturing of the landing gear lug. The performance of the repaired piece and the reference piece is compared to judge the effect after the repair. Step 17: artificially process the surface of the repaired part to a depth equivalent to the thickness of the defect removed in step 1, and use the rectangular wire and cylindrical rod processed in steps 2 to 4 for welding repair. The repair process repeats steps 5 to 15. The repaired part and the reference part are processed into strength test specimens and fatigue test specimens. The tensile strength of the repaired part is compared with that of the reference part, and the fatigue performance of the repaired part is compared with that of the reference part. The fatigue test load is 800 MPa and the stress ratio is 0.
1. If it is not broken after 10,000 times, it is considered to have passed. If the tensile strength of the repaired part reaches more than 95% of the performance of the reference part and the fatigue performance passes the fatigue test, it is determined that the landing gear ear part (1) has been repaired successfully.
2. A method for repairing surface damage of a landing gear pylon lug according to claim 1, characterized in that: In step 2, the rectangular wire has a width dimension of 0.5-0.7 mm, a height dimension of 0.5-0.7 mm, and a length dimension of ≥150 mm. The diameter dimension of the cylindrical rod is 2-6 mm and the length is 80-100 mm.
3. A method for repairing the surface damage of a landing gear pylon lug according to claim 1, characterized in that: The sandblasting process parameters in step 4 include: using corundum sand or quartz sand, with a particle size of 180 mesh or more, and a pressure of 0.3 to 0.6 MPa.
4. A method for repairing the surface damage of a landing gear pylon lug according to claim 1, characterized in that: The water cooling device (4) is provided with a water inlet (5) at the bottom and a water outlet (6) at the top. The water cooling device (4) is made of copper material and uses flowing water at room temperature.
5. The method for repairing the surface damage of the landing gear pylon lug according to claim 1, characterized in that: The diameter of the cylindrical boss (7) on the water cooling device (4) is 0.5 mm smaller than the diameter of the cylindrical hole (3) on the landing gear ear part (1).
6. A method for repairing the surface damage of a landing gear pylon lug according to claim 1, characterized in that: In step seven, the thickness of the first cladding layer is controlled at 80-100 μm.
Citation Information
Patent Citations
Processing method for repairing chromium coating of undercarriage piston rod with unqualified air tightness
CN102031543A
A laser welding repair method for aircraft landing gear piston rods
CN113068434B
Laser additive repairing method for 300M steel aircraft undercarriage
CN113245551A
Repair material and method for corrosion defects of aluminum alloy component and application
CN113463084A
Method for repairing core rods for rolling seamless steel pipes