Method for impregnating wood surface layer with wax emulsion

Through wax emulsion impregnation and intermittent unloading technology, combined with steam and microwave pretreatment, the problems of high cost and easy damage in wood modification treatment are solved, the durability and service life of wood are improved, and environmentally friendly and efficient wood is achieved. Modification effect.

CN118990716AActive Publication Date: 2024-11-22NANJING FORESTRY UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411190268.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-22
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing wood modification treatment methods have problems such as not being able to maintain quality for a long time, being easily polluted by the environment, being easily cracked and deformed, and requiring frequent maintenance. The high-melting point polyethylene wax impregnation process is costly and complex.

Method used

The wax emulsion method is used to increase the permeability of wood by pretreatment such as steam and microwave treatment, combined with intermittent unloading technology to reduce the difficulty of impregnation of wood surfaces, improve the penetration efficiency of wax emulsion, and increase the contact area of ​​wax through side holes to increase the Immersion effect.

Benefits of technology

It effectively reduces the difficulty of wood impregnation, improves the durability, wear resistance and service life of wood, simplifies the process flow, avoids the use of high-temperature vacuum pressure devices, and realizes environmentally friendly and efficient wood modification treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990716A_ABST
    Figure CN118990716A_ABST
Patent Text Reader

Abstract

The invention discloses a method for impregnating a wood surface layer with wax emulsion. The method comprises the following steps that 1, wood is pretreated; 2, the pretreated wood is soaked in a wax emulsion; 3, the wood soaked in the wax emulsion is pressurized, and pressure relief is conducted after pressurization is completed; and 4, the wood is fished out of the wax emulsion, the wax emulsion on the surface of the wood is wiped dry, and the wood is dried. According to the method for impregnating the wood surface layer with the wax emulsion, the wood surface layer is impregnated and permeated with the wax emulsion, the wood impregnation difficulty is reduced, the wood permeation efficiency is improved, the wood color is effectively protected, the wood durability and wear resistance are improved, and the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of impregnated wood, in particular to a method for impregnating a wood surface layer with a wax emulsion. Background Art

[0002] As a natural carbon-fixing and renewable engineering material, wood has a history of thousands of years of construction use in my country. Although ancient wooden buildings with mortise and tenon joints as the main connection method have gone through thousands of years, a large number of ancient wooden buildings have been handed down, such as the Yingxian Wooden Pagoda built in 1056 AD, which is the tallest existing wooden tower building in the world; the Dule Temple in Jixian County, built in 987 AD during the Liao Dynasty, is one of the most famous existing wooden temples in China. Modern wooden buildings retain the characteristics of traditional wooden buildings such as environmental friendliness and beautiful shapes, while also having the characteristics of flexible design, short construction cycle, and high living comfort. As a natural biomass material, wood is easily affected by the environment and deteriorates such as cracking, deformation, decay, and insect pests when it serves in buildings for a long time. In order to make wood better adapt to the application requirements of buildings, physical or chemical methods are often used to modify wood or wood surfaces. However, traditional modified materials generally have the disadvantages of not being able to maintain quality for a long time, being easy to pollute the environment, being easy to crack and deform, and requiring frequent maintenance. Exploring a new, safe, and green modification method to improve the durability of wood is of great significance to broadening the application areas of wood and promoting the sustainable development of modern wooden structures.

[0003] The modern wax injection process is to inject melted wax into the wood without damaging the wood itself, so that excess moisture inside the wood can be discharged and the cell cavities and gaps between cells of the wood can be filled. When the wax successfully penetrates into the wood, it can eventually form a uniform wax film with a thickness of 0.03mm-1mm on the surface of the wood, relying on the hydrophobicity of the wax to improve the aging resistance of the wood.

[0004] High melting point polyethylene wax (PEW) is non-toxic and pollution-free, stable in nature, durable and hydrophobic. PEW can effectively protect the color of wood and improve the durability of wood. However, the high melting point PEW impregnation and modification of wood process has the disadvantages of long wax melting cycle, high requirements for high temperature impregnation equipment and high process cost. If the high melting point PEW is emulsified, it will be converted into a uniform and stable wax emulsion, such as PEW emulsion. PEW emulsion has good chemical stability, wear resistance and scratch resistance. If it is used to treat wood, it can improve the stability of wood, increase the wear resistance of wood, increase the service life of wood and ultimately achieve the purpose of improving economic benefits.

[0005] In summary, it is necessary to provide a method for impregnating the surface of wood with a wax emulsion without environmental pollution to protect the color of the wood, improve the durability of the wood, increase the wear resistance and service life of the wood, etc. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for impregnating the surface layer of wood with a wax emulsion in view of the deficiencies of the above-mentioned prior art. The method for impregnating the surface layer of wood with a wax emulsion impregnates the surface layer of wood with the wax emulsion, thereby reducing the difficulty of wood impregnation, improving the wood penetration efficiency and the penetration thickness of the wood, effectively protecting the color of the wood, and improving the durability, wear resistance and service life of the wood.

[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0008] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0009] Step 1: Pre-treat the wood;

[0010] Step 2: Immersing the pretreated wood in wax emulsion;

[0011] Step 3: Pressurizing the wood immersed in the wax emulsion, and releasing the pressure after the pressurization is completed;

[0012] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0013] As a further improved technical solution of the present invention, the step 1 is specifically as follows:

[0014] Step 1.1, measure the moisture content of the wood, and the obtained moisture content is A0;

[0015] Step 1.2, steaming the wood, and placing the steamed wood in a microwave oven for microwave treatment;

[0016] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0017] As a further improved technical solution of the present invention, before step 1.1, holes are punched on the side of the wood, and the holes are through holes in the wood.

[0018] As a further improved technical solution of the present invention, the step 1.2 is specifically: using an electrically heated constant temperature water tank to heat the wood to generate water vapor to steam the wood, the heating temperature is 95°C, after the water temperature rises to 95°C, putting the wood in, starting the timing, and completing the steaming after the steaming time is reached; putting the steamed wood in a microwave oven for microwave treatment, the firepower of the microwave oven is set to high, and completing the microwave treatment after the microwave treatment time is reached.

[0019] As a further improved technical solution of the present invention, the steaming treatment time is 30min-120min, and the microwave treatment time is 3min-9min.

[0020] As a further improved technical solution of the present invention, the wax emulsion adopts LW-109 PEW emulsion.

[0021] As a further improved technical solution of the present invention, the step 3 is specifically: using a mechanical testing machine to pressurize the wood immersed in the wax emulsion, the pressurization method is short-cycle intermittent loading and unloading or long-cycle intermittent loading and unloading, and the pressure is released after the pressurization is completed.

[0022] As a further improved technical solution of the present invention, when the pressurization mode is short-cycle intermittent loading and unloading, the pressurization speed is 10 mm / min, the wood compression ratio is set to 50%, the pressure relief speed is 40 mm / min, the impregnation time after each pressure relief is 3 minutes, and the cycle frequency of intermittent loading and unloading is 3-9 times;

[0023] When the pressurization method is long-cycle intermittent loading and unloading, the pressurization speed is 10mm / min, the wood compression ratio is set to 50%, the pressure relief speed is 40mm / min, the immersion time after each pressure relief is 14h, and the cycle frequency of intermittent loading and unloading is 1-3 times.

[0024] As a further improved technical solution of the present invention, the wood includes okoume wood or Larix gmelinii wood, the pressure bearing direction of intermittent loading and unloading of okoume wood is tangential pressure, and the pressure bearing direction of intermittent loading and unloading of Larix gmelinii wood is radial pressure.

[0025] As a further improved technical solution of the present invention, step 4 is: taking the wood out of the wax emulsion and wiping the wax emulsion on the surface of the wood; then, placing the wood in an electric constant temperature blast drying oven for drying, the drying temperature is 50°C, and the moisture content of the wood is measured every 0.5 hours during the drying process until the moisture content of the wood is reduced to A0, and then the drying is stopped.

[0026] The beneficial effects of the present invention are:

[0027] The present invention is based on the compression and rebound characteristics of wood. It utilizes the air pressure difference inside and outside the wood during intermittent loading and unloading to impregnate the wood with PEW emulsion, which is an effective method to reduce the difficulty of impregnation of the wood surface under normal pressure. The use of this technology facilitates the use of the hydrophobic advantages of PEW materials and the porosity advantages of wood components. Compared with the immersion method, the PEW intermittent loading and unloading impregnation of wood has high efficiency and good protection effect. Compared with the high-pressure impregnation method, the process is simple, the impregnation does not require a vacuum pressure tank, and the application advantages are obvious.

[0028] The wood of the present invention adopts a steaming + microwave pretreatment method, which is helpful to improve the permeability of the wood. While improving the air permeability of the wood, the compression rebound thereof is significantly improved. The rebound rate of the untreated wood is lower than that of the pretreated wood, and the rebound rate of the wood increases with the extension of the pretreatment time.

[0029] The intermittent loading and unloading frequency of the present invention is conducive to promoting the multiple absorption of PEW emulsion by the wood surface, and significantly improves its impregnation amount. The weight gain of wax-impregnated wood increases rapidly at first, then gradually slows down and finally begins to decline. In the process of intermittent loading and unloading of wood for impregnation modification, the frequency has a greater impact on the short-cycle wood impregnation than the long-cycle. Among the short-cycle frequencies, 9 times of impregnation is the most ideal; and among the long-cycle frequencies, 1 time of impregnation has the most reasonable weight gain rate.

[0030] In order to further increase the impregnation weight gain rate of the wood surface, the wood can be punched on the side to increase the area of ​​the wood side absorbing PEW emulsion. The wood can be punched in two forms: single hole and four holes. The side punching treatment does not affect the impregnation effect of PEW on the end face, but increases the contact area between the wood side and the wax. The presence of through holes allows the wax emulsion to enter the wood more freely and deeply, greatly enhancing the impregnation effect of PEW. Drilling holes in the wood can significantly increase the impregnation weight gain rate of the wood, and the weight gain rate increases positively with the number of holes. Due to the increase in the number of holes, the specific surface area of ​​the wood is greatly increased. At the same time, punching holes on the side solves the problem that the pressure-bearing wood only has good absorption effect at the end.

[0031] The PEW emulsion impregnated wood of the present invention has good stability, and the water absorption expansion rate and dimensional stability of the treated wood are greatly improved compared with the untreated test piece. The PEW emulsion is non-toxic and pollution-free, has stable properties, good durability and hydrophobicity. The PEW emulsion is used to impregnate wood through the method of the present invention, which reduces the difficulty of wood impregnation, improves the wood penetration efficiency, can penetrate to a thickness of 5mm below the wood surface, effectively protects the wood color, improves the stability of the wood, and improves the durability, wear resistance and service life of the wood. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of a single cycle of intermittent loading and unloading of wood PEW emulsion impregnation.

[0033] Figure 2 This is a graph showing the effect of short cycle frequency on the weight gain rate of the surface impregnation of Okoume wood.

[0034] Figure 3 This is a graph showing the effect of short cycle frequency on the weight gain rate of surface impregnation of Larix gmelinii wood.

[0035] Figure 4 This is a graph showing the effect of long-cycle frequency on the weight gain rate of the surface impregnation of Okoume wood.

[0036] Figure 5 This is a graph showing the effect of long-cycle frequency on the weight gain rate of surface impregnation of Larix gmelinii wood.

[0037] Figure 6 Graph showing the effect of pretreatment conditions on the impregnation permeability of the surface layer of Okoume wood.

[0038] Figure 7 This is a diagram showing the influence of pretreatment conditions on the surface impregnation permeability of Pinus sylvestris var. mongolica wood.

[0039] Figure 8 The effects of different compression rates and PEW emulsion types on the impregnation permeability of the wood surface of Okoume species.

[0040] Fig. 9 The influence of different compression rates and PEW emulsion types on the impregnation permeability of the wood surface of Pinus sylvestris var. mongolica species was studied.

[0041] Fig.10 The influence of different tree species on the impregnation permeability of wood surface.

[0042] Fig.11 The effect of drilling on the weight gain rate of impregnation pine wood.

[0043] Fig.12 Schematic diagram of environmental scanning electron microscope sample.

[0044] Fig.12 (a) is a schematic diagram of sampling the inner layer of wax-impregnated wood.

[0045] Fig.12 (b) is a real picture of wax impregnated wood sampling.

[0046] Fig.13 SEM images of the surface of wood impregnated with okoume and Pinus sylvestris wax.

[0047] Fig.14 SEM images of the inner layer of wood impregnated with okoume and scotch pine wax.

[0048] Fig.15 This is a graph showing the change in radial expansion rate of wood due to impregnation.

[0049] Fig.15 (a) is the change of radial immersion expansion rate of Okoume.

[0050] Fig.15 Middle (b) is the change diagram of radial immersion expansion rate of Pinus sylvestris var. mongolica.

[0051] Fig.16 This is a graph showing the change in the tangential expansion rate of wood.

[0052] Fig.16 (a) is the change of the tangential immersion expansion rate of Okoume.

[0053] Fig.16 (b) is the change of the tangential immersion expansion rate of Pinus sylvestris.

[0054] Fig.17 This is a typical freeze-thaw cycle resistance specimen diagram.

[0055] Fig.17 (a) is a specimen image after one freeze-thaw cycle.

[0056] Fig.17 (b) is a typical specimen after 10 freeze-thaw cycles.

[0057] Fig.17 (c) is a typical specimen after 15 freeze-thaw cycles.

[0058] Fig.18 Hardness diagram of intermittent loading and unloading impregnated wood resistance to freeze-thaw cycles.

[0059] Fig.19 SEM image of PEW-impregnated wood subjected to UV-accelerated aging. DETAILED DESCRIPTION

[0060] The specific embodiments of the present invention are further described below according to the accompanying drawings:

[0061] Embodiment 1:

[0062] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0063] Step 1: Pre-treat the wood.

[0064] Step 1.1: Punch a hole on the side of the wood, select a single hole, select a self-tapping screw with a screw radius of 1.5 mm, and drill a hole through the wood. Measure the moisture content of the wood, and the moisture content obtained is A0.

[0065] Step 1.2, steam the wood by heating the water vapor generated by the electric heating constant temperature water tank, the heating temperature is 95°C, after the water temperature rises to 95°C, put the wood in, start timing, and complete steaming after reaching the steaming treatment time, the steaming treatment time is 30 minutes. Put the steamed wood in a microwave oven for microwave, the firepower of the microwave oven is set to high, and the microwave treatment time is completed after reaching the microwave treatment time, the microwave treatment time is 3 minutes.

[0066] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0067] Step 2: Immerse the pretreated wood in wax emulsion, wherein the wax emulsion is PEW emulsion of LW-109.

[0068] Step 3: Pressurize the wood immersed in the wax emulsion, and release the pressure after the pressurization is completed.

[0069] Specifically, the wood impregnated in wax emulsion was pressurized using a mechanical testing machine, with short-cycle intermittent loading and unloading, and pressure relief after the pressurization was completed. The pressurization speed was 10 mm / min, the wood compression ratio was set to 50%, the pressure relief speed was 40 mm / min, and the impregnation rebound time after each pressure relief was 3 minutes. The frequency of intermittent loading and unloading cycles was 3 times.

[0070] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0071] Specifically: take the wood out of the wax emulsion and wipe off the wax emulsion on the surface of the wood; then, put the wood into an electric constant temperature air drying oven for drying at a temperature of 50°C. During the drying process, measure the moisture content of the wood every 0.5 hours until the moisture content of the wood drops to A0, then stop drying.

[0072] Embodiment 2:

[0073] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0074] Step 1: Pre-treat the wood.

[0075] Step 1.1: Punch holes on the side of the wood, select four holes, select self-tapping screws with a screw radius of 1.5 mm for drilling, and punch holes through the wood. Measure the moisture content of the wood, and the moisture content obtained is A0.

[0076] Step 1.2, steam the wood by heating the water vapor generated by the electric heating constant temperature water tank, the heating temperature is 95°C, after the water temperature rises to 95°C, put the wood in, start timing, and complete steaming after reaching the steaming treatment time, the steaming treatment time is 60 minutes. Put the steamed wood in a microwave oven, set the firepower of the microwave oven to high, and complete the microwave after reaching the microwave treatment time, the microwave treatment time is 6 minutes.

[0077] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0078] Step 2: Immerse the pretreated wood in wax emulsion, wherein the wax emulsion is PEW emulsion of LW-109.

[0079] Step 3: Pressurize the wood immersed in the wax emulsion, and release the pressure after the pressurization is completed.

[0080] Specifically, the wood impregnated in wax emulsion was pressurized using a mechanical testing machine. The pressurization method was intermittent loading and unloading in a short period of time, and the pressure was released after the pressurization was completed. The pressurization speed was 10mm / min, the wood compression ratio was set to 50%, the pressure release speed was 40mm / min, and the impregnation rebound time after each pressure release was 3min. The frequency of the intermittent loading and unloading cycle was 9 times.

[0081] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0082] Specifically: take the wood out of the wax emulsion and wipe off the wax emulsion on the surface of the wood; then, put the wood into an electric constant temperature air drying oven for drying at a temperature of 50°C. During the drying process, measure the moisture content of the wood every 0.5 hours until the moisture content of the wood drops to A0, then stop drying.

[0083] Embodiment 3:

[0084] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0085] Step 1: Pre-treat the wood.

[0086] Step 1.1: Punch a hole on the side of the wood, select a single hole, select a self-tapping screw with a screw radius of 1.5 mm, and drill a hole through the wood. Measure the moisture content of the wood, and the moisture content obtained is A0.

[0087] Step 1.2, steam the wood by heating the water vapor generated by the electric heating constant temperature water tank, the heating temperature is 95°C, after the water temperature rises to 95°C, put the wood in, start timing, and complete steaming after reaching the steaming treatment time, the steaming treatment time is 120 minutes. Put the steamed wood in a microwave oven, set the microwave oven to high power, and complete microwave after reaching the microwave treatment time, the microwave treatment time is 9 minutes.

[0088] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0089] Step 2: Immerse the pretreated wood in wax emulsion, wherein the wax emulsion is PEW emulsion of LW-109.

[0090] Step 3: Pressurize the wood immersed in the wax emulsion, and release the pressure after the pressurization is completed.

[0091] Specifically, the wood impregnated in wax emulsion was pressurized using a mechanical testing machine. The pressurization method was intermittent loading and unloading in a short period of time, and the pressure was released after the pressurization was completed. The pressurization speed was 10mm / min, the wood compression ratio was set to 50%, the pressure release speed was 40mm / min, and the impregnation rebound time after each pressure release was 3min. The frequency of the intermittent loading and unloading cycle was 6 times.

[0092] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0093] Specifically: take the wood out of the wax emulsion and wipe off the wax emulsion on the surface of the wood; then, put the wood into an electric constant temperature air drying oven for drying at a temperature of 50°C. During the drying process, measure the moisture content of the wood every 0.5 hours until the moisture content of the wood drops to A0, then stop drying.

[0094] Embodiment 4:

[0095] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0096] Step 1: Pre-treat the wood.

[0097] Step 1.1: Punch holes on the side of the wood, select four holes, select self-tapping screws with a screw radius of 1.5 mm for drilling, and punch holes through the wood. Measure the moisture content of the wood, and the moisture content obtained is A0.

[0098] Step 1.2, steam the wood by heating the water vapor generated by the electric heating constant temperature water tank, the heating temperature is 95°C, after the water temperature rises to 95°C, put the wood in, start timing, and complete steaming after reaching the steaming treatment time, the steaming treatment time is 60 minutes. Put the steamed wood in a microwave oven, set the firepower of the microwave oven to high, and complete the microwave after reaching the microwave treatment time, the microwave treatment time is 6 minutes.

[0099] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0100] Step 2: Immerse the pretreated wood in wax emulsion, wherein the wax emulsion is PEW emulsion of LW-109.

[0101] Step 3: Pressurize the wood immersed in the wax emulsion, and release the pressure after the pressurization is completed.

[0102] Specifically, the wood impregnated in wax emulsion was pressurized using a mechanical testing machine. The pressurization method was intermittent loading and unloading with a long period of frequency. After the pressurization was completed, the pressure was released. The pressurization speed was 10mm / min, the wood compression ratio was set to 50%, the pressure release speed was 40mm / min, and the impregnation rebound time after each pressure release was 14h. The frequency of the intermittent loading and unloading cycle was 3 times.

[0103] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0104] Specifically: take the wood out of the wax emulsion and wipe off the wax emulsion on the surface of the wood; then, put the wood into an electric constant temperature air drying oven for drying at a temperature of 50°C. During the drying process, measure the moisture content of the wood every 0.5 hours until the moisture content of the wood drops to A0, then stop drying.

[0105] Embodiment 5:

[0106] A method for impregnating a wood surface layer with a wax emulsion comprises the following steps:

[0107] Step 1: Pre-treat the wood.

[0108] Step 1.1: Measure the moisture content of the wood and obtain the moisture content A0.

[0109] Step 1.2, steam the wood by heating the water vapor generated by the electric heating constant temperature water tank, the heating temperature is 95°C, after the water temperature rises to 95°C, put the wood in, start timing, and complete steaming after reaching the steaming treatment time, the steaming treatment time is 60 minutes. Put the steamed wood in a microwave oven, set the firepower of the microwave oven to high, and complete the microwave after reaching the microwave treatment time, the microwave treatment time is 6 minutes.

[0110] Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.1.

[0111] Step 2: Immerse the pretreated wood in wax emulsion, wherein the wax emulsion is PEW emulsion of LW-109.

[0112] Step 3: Pressurize the wood immersed in the wax emulsion, and release the pressure after the pressurization is completed.

[0113] Specifically, the wood impregnated in wax emulsion was pressurized using a mechanical testing machine. The pressurization method was intermittent loading and unloading with a long period of frequency, and the pressure was released after the pressurization was completed. The pressurization speed was 10mm / min, the wood compression ratio was set to 50%, the pressure relief speed was 40mm / min, and the impregnation rebound time after each pressure relief was 14h. The frequency of the intermittent loading and unloading cycle was 1 time.

[0114] Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

[0115] Specifically: take the wood out of the wax emulsion and wipe off the wax emulsion on the surface of the wood; then, put the wood into an electric constant temperature air drying oven for drying at a temperature of 50°C. During the drying process, measure the moisture content of the wood every 0.5 hours until the moisture content of the wood drops to A0, then stop drying.

[0116] The results of the above examples 1-5 are analyzed and discussed below:

[0117] In the above-mentioned embodiments 1-5, the wood is selected from Okoume wood or Scotch pine wood. After the wood is pretreated by steaming + microwave, the instantaneous rebound rate of the wood can be improved to a certain extent. By intermittently loading and unloading, the wood is pressurized, and the compression and rebound characteristics of the wood are utilized to allow the wood to actively absorb external fluid substances, thereby increasing the impregnation effect of the wood and achieving the purpose of impregnation of the wood surface.

[0118] In the above examples 1-5, the PEW emulsion is a cationic emulsion, numbered LW-109, which is a uniform oil-in-water (O / W) fluid. It is a milky white opaque emulsion at room temperature, odorless, with good fluidity and good uniformity when observed by naked eyes. The melting point of LW-109 is around 100°C and the density is 0.93±2g / cm 3 . PEW emulsion is made by using the emulsifier maleic acid (MAH, C4H2O3) at 95°C to uniformly disperse the high melting point PEW (PEW, R-(CH2–CH2)n–CH3) in the water phase by directional adsorption. The carboxyl group of the MAH emulsifier can esterify with the hydroxyl group of the wood fiber to form a strong chemical bond. After the esterification reaction, the dimensional stability and hydrophobicity of the wood can be improved to a certain extent. At the same time, the PEW attached to the surface can provide deeper and lasting protection for the wood.

[0119] In the above embodiments 1-5, when the bearing direction of the wood is perpendicular to the tangent direction of the wood ring, the wood is radially bearing; when the angle between the bearing direction of the wood and the annual ring is 45°, the wood is obliquely bearing; when the bearing direction of the wood is parallel to the tangent direction of the annual ring, the wood is tangentially bearing. The bearing direction of intermittent loading and unloading of Okoume is tangential bearing, and the bearing direction of intermittent loading and unloading of Pinus sylvestris is radial bearing.

[0120] In the above embodiments 1-5, the formula for the weight gain rate of wood is:

[0121]

[0122] Where: α max Indicates the weight gain rate of wax impregnated wood, %; Mmax It indicates the mass of wood just after impregnation or impregnation drying during the impregnation process, g; M1 indicates the mass of wood before impregnation, g.

[0123] In the above-mentioned embodiments 1-4, in order to further improve the impregnation weight gain rate of the wood surface, the wood can be punched on the side to increase the area of ​​the wood side absorbing the PEW emulsion. The wood can be punched in two forms: single hole and four holes. The side punching process does not affect the impregnation effect of PEW on the end face, but increases the contact area between the side of the wood and the wax. The presence of the through holes allows the wax emulsion to enter the interior of the wood more freely and deeply, greatly enhancing the impregnation effect of PEW. Drilling holes in the wood can significantly increase the impregnation weight gain rate of the wood, and the weight gain rate increases in a positive direction with the number of holes. Due to the increase in the number of holes, the specific surface area of ​​the wood is greatly increased. At the same time, punching holes on the side solves the problem that the compressed wood only has a good absorption effect at the end.

[0124] like Figure 1 As shown, Figure 1 Schematic diagram of a single cycle of intermittent loading and unloading of wood PEW emulsion impregnation in Examples 1-5.

[0125] Compared with intermittent loading and unloading with long cycle frequency, the difference between the two is the impregnation time. The impregnation time of intermittent loading and unloading with long cycle frequency is 14h, and the frequency is set to 1, 2 or 3 times. Leaking wax emulsion in the air for a long time will cause viscous precipitation of PEW emulsion, increasing the difficulty of impregnation. Therefore, when PEW emulsion is impregnated with wood for a long period of time, it is sealed with plastic wrap.

[0126] Effect of short cycle frequency on the weight gain rate of wood surface impregnation:

[0127] Effect of short cycle frequency on the weight gain rate of Okoume wood surface impregnation Figure 2 As shown, Figure 2 A is 3 intermittent loading and unloading cycles, B is 6 intermittent loading and unloading cycles, and C is 9 intermittent loading and unloading cycles. The frequency has a great influence on the weight gain rate of wood wax impregnation, and the weight gain rate of wood will increase positively with the increase of intermittent loading and unloading frequency. When the frequency is 3 times, there is almost no PEW emulsion impregnation adsorption on the side of Okoume wood, and PEW emulsion is adsorbed only on the end face of the wood; when the frequency is 6 times, a small amount of wax begins to be adsorbed on the side of the wood, and the amount of wax adsorption on the end face increases significantly; when the wood undergoes 9 cycles, there is a large amount of PEW adsorption on the end face of the wood. Therefore, during the rebound process, the wood mainly absorbs air or wax emulsion through the end face.

[0128] In the process of intermittent loading and unloading to impregnate the surface of the wood, not only will PEW enter, but also the moisture content of the wood will increase, resulting in an increase in the quality of the wood. Therefore, it is necessary to dry the wood. The wet weight gain rate of Okoume wood after three intermittent loading and unloading cycles is 6.6%, and the weight gain rate of the wood after drying is 1.4%; the wet weight gain rate of Okoume wood after six intermittent loading and unloading cycles is 8.1%, and the weight gain rate of the wood after drying is 2.3%; the wet weight gain rate of Okoume wood after nine intermittent loading and unloading cycles is 9.1%, and the weight gain rate of the wood after drying is 3.2%. Compared with three intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 18% in six intermittent loading and unloading cycles. Compared with three intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 27% in nine intermittent loading and unloading cycles. Compared with six intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 11% in nine intermittent loading and unloading cycles. Compared with three intermittent loading and unloading cycles, the dry weight gain rate of wood increased by 43.4% in six intermittent loading and unloading cycles. The dry weight gain rate of wood increased by 59.3% after 9 intermittent loading and unloading cycles compared with 3 intermittent loading and unloading cycles. The dry weight gain rate of wood increased by 28.1% after 9 intermittent loading and unloading cycles compared with 6 intermittent loading and unloading cycles. Whether it is the wet weight gain rate or the dry weight gain rate, the wax impregnation amount of wood is the highest when the intermittent loading and unloading is repeated for a short period of time.

[0129] Effect of short cycle frequency on weight gain rate of surface impregnation of Pinus sylvestris var. mongolica wood Figure 3 As shown. The effect of short cycle frequency on the weight gain rate of Scotch pine wood is roughly the same as that of frequency on the weight gain rate of Okoume wood, but the overall weight gain rate of Scotch pine wood is greater than that of Okoume wood. During the three intermittent loading and unloading, there will be a small amount of wax emulsion adsorbed on the side of Scotch pine wood, and the end surface of the wood can achieve relatively uniform and complete adsorption.

[0130] The wet weight gain rate of Larix gmelinii wood after three intermittent loading and unloading cycles is 11.5%, and the weight gain rate of wood after drying is 4.4%; the wet weight gain rate of Larix gmelinii wood after six intermittent loading and unloading cycles is 12.7%, and the dry weight gain rate of wood is 5.1%; the wet weight gain rate of Larix gmelinii wood after nine intermittent loading and unloading cycles is 16.6%, and the dry weight gain rate is 8%. Compared with three intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 9.4% after six intermittent loading and unloading cycles. Compared with three intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 29% after nine intermittent loading and unloading cycles. Compared with six intermittent loading and unloading cycles, the wet weight gain rate of wood increased by 23.4% after nine intermittent loading and unloading cycles. Compared with three intermittent loading and unloading cycles, the dry weight gain rate of wood increased by 13.7% after six intermittent loading and unloading cycles. Compared with three intermittent loading and unloading cycles, the dry weight gain rate of wood increased by 45% after nine intermittent loading and unloading cycles. The dry weight gain rate of wood after 9 intermittent loading and unloading cycles increased by 36.2% compared with 6 intermittent loading and unloading cycles.

[0131] Therefore, whether it is Okoume or Pinus sylvestris, the frequency of intermittent loading and unloading of PEW emulsion impregnation is the best among the three established frequencies. The wood weight gain rate of Okoume wood is about 3% when dry weight, and the wood weight gain rate of Pinus sylvestris wood is about 8% when dry weight. This is because the rebound rate of Pinus sylvestris wood itself is greater than that of Okoume wood, and its adsorption capacity for PEW is also stronger. Therefore, for the short cycle frequency, the best frequency of Okoume and Pinus sylvestris is 9 times, and the adsorption capacity of Okoume wood for PEW emulsion is less than that of Pinus sylvestris wood.

[0132] Effect of long-term frequency on the weight gain rate of wood surface impregnation:

[0133] Effect of long cycle frequency on the weight gain rate of Okoume wood surface impregnation Figure 4 As shown in Figure 2, the effect of long cycle frequency on the weight gain rate of the surface impregnation of Pinus sylvestris var. mongolica wood is as follows: Figure 5 shown.

[0134] The long-cycle frequency of Okoume wood has a wet weight gain rate of about 28%, and a dry weight gain rate of about 14%. The long-cycle frequency of Larix gmelinii has a wet weight gain rate of about 50%, and a dry weight gain rate of about 29%. As can be seen from the figure, the weight gain rate of the wood is the highest when the wet weight of the wood is measured in the second cycle. This is because during the three long-cycle impregnation processes, even if plastic wrap is used to protect the wax emulsion, it is still difficult to avoid water loss during the 42-hour impregnation process, making the wax emulsion viscous, with partial precipitation and reduced fluidity. Therefore, the wet weight gain rate of the three cycles will be less than the wet weight gain rate of the two cycles.

[0135] Comparison of intermittent loading and unloading with long and short cycle frequencies shows that the wood weight gain rate of short cycle frequency has not reached the limit state of wood being able to absorb PEW. However, the advantage of short cycle frequency process compared to long cycle frequency process is that it takes less time and can make the wood surface and interior absorb a large amount of PEW, achieving the purpose of making PEW wood. The long cycle frequency has the advantages of simpler process and ideal wax impregnation effect.

[0136] Effect of pretreatment conditions on the impregnation permeability of wood surface:

[0137] Effect of pretreatment conditions on the impregnation permeability of the surface layer of Okoume wood Figure 6As shown. The adsorption effect of the end surface of the pretreated Okoume wood is better than that of the unpretreated specimen, but the adsorption effect of the wax on the side of the Okoume wood is not much improved. The pretreatment time has an important influence on the wax impregnation amount of the wood, and the wax impregnation amount will increase significantly with the extension of the pretreatment time. When steaming for 120 minutes + microwave for 9 minutes, the wax impregnation amount of the wood is the best, which reflects the enhancement of the permeability of the wood. When Okoume is treated with steaming for 30 minutes + microwave for 3 minutes, its dry weight gain rate compared with no pretreatment is 4.2%; when steaming for 60 minutes + microwave for 6 minutes, its dry weight gain rate compared with no pretreatment is 6.8%; when steaming for 120 minutes + microwave for 9 minutes, its dry weight gain rate compared with no pretreatment is 7.8%. The increase rate of pretreatment with steaming for 60 minutes + microwave for 6 minutes compared with pretreatment with steaming for 30 minutes + microwave for 3 minutes was 38.2%; the increase rate of pretreatment with steaming for 120 minutes + microwave for 9 minutes compared with pretreatment with steaming for 60 minutes + microwave for 6 minutes was 12.8%; the increase rate of pretreatment with steaming for 120 minutes + microwave for 9 minutes compared with pretreatment with steaming for 30 minutes + microwave for 3 minutes was 46.1%. Therefore, although the wood weight gain rate is the largest when the pretreatment is steaming for 120 minutes + microwave for 9 minutes, considering the processing efficiency and time cost comprehensively, the best pretreatment time for Okoume wood is steaming for 60 minutes + microwave for 6 minutes.

[0138] Effects of pretreatment conditions on the impregnation permeability of the surface of Pinus sylvestris var. mongolica wood Figure 7As shown. The wax adsorption characteristics of the surface of Larix gmelinii wood are similar to those of Okoume wood, but the degree of improvement of the impregnation effect is less than that of Okoume wood. When the pretreatment is steaming for 120 minutes + microwave for 9 minutes, the permeability improvement effect of Larix gmelinii wood is the best. When the Larix gmelinii wood is pretreated with steaming for 30 minutes + microwave for 3 minutes, its dry weight gain rate compared with no pretreatment is 9.3%; when the pretreatment is steaming for 60 minutes + microwave for 6 minutes, its dry weight gain rate compared with no pretreatment is 10.6%; when the pretreatment is steaming for 120 minutes + microwave for 9 minutes, its dry weight gain rate compared with no pretreatment is 12.5%. The dry weight gain rate of wood with pretreatment of steaming for 60 minutes + microwave for 6 minutes increased by 12.2% compared with that with pretreatment of steaming for 30 minutes + microwave for 3 minutes; the dry weight gain rate of wood with pretreatment of steaming for 120 minutes + microwave for 9 minutes increased by 15.2% compared with that with pretreatment of steaming for 60 minutes + microwave for 6 minutes; the dry weight gain rate of wood with pretreatment of steaming for 120 minutes + microwave for 9 minutes increased by 25.6% compared with that with pretreatment of steaming for 30 minutes + microwave for 3 minutes. Therefore, although the weight gain rate of wood is high when the pretreatment method is steaming for 120 minutes + microwave for 9 minutes, considering the processing efficiency and time cost comprehensively, the best pretreatment method for wax impregnation of Pinus sylvestris var. mongolica wood is steaming for 60 minutes + microwave for 6 minutes.

[0139] The influence trend of pretreatment time on okoume and larch wood is roughly the same. The weight gain rate of wood will increase with the increase of pretreatment time, and the increase of okoume is more obvious. This is because okoume itself contains a large number of inclusions. Steaming + microwave pretreatment can vaporize the water in the wood cell cavity and increase the pressure in the wood cell cavity. When the water vapor pressure inside the wood cell cavity increases to a certain extent, the weak parts of the wood (such as the pit membrane) or the thin-walled tissue (such as the thin-walled ray cells) will rupture, thereby forming a fluid channel, which greatly reduces the content of inclusions. Larch itself has excellent wood rebound and adsorption capabilities. A simple pretreatment procedure can achieve a good impregnation effect. If the pretreatment time is too long, it will cause a waste of resources.

[0140] Effect of wax emulsion type on wood surface impregnation penetration:

[0141] Figure 8The effect of different compression rates and PEW emulsion types of Okoume tree species on the impregnation permeability of the wood surface. The molecular weight of the wax emulsion directly affects the density of the emulsion. The larger the molecular weight, the greater the density of the wax emulsion. The molecular weight of LW-111PEW emulsion is large, which increases the difficulty of wood impregnation. At the end of Okoume, LW-111PEW will also be adsorbed, which can achieve the purpose of wax protecting wood. As can be seen from the figure, the 50% compression rate has a more obvious improvement in the impregnation effect of LW-109 on Okoume. At the same time, it can be seen that for Okoume tree species, when LW-111 is dried from wet weight to dry weight, the weight gain rate of wood decreases less than that of LW-109. This may be because LW-111PEW emulsion falls off less during the drying process. But the overall effect of LW-109's impregnation weight gain is better than that of LW-111. The dry weight gain rate of LW-109 with 50% compression rate of Okoume is 13.4%, and the weight gain rate of direct impregnation without pressure is 3.3%; the weight gain rate of LW-111 with 50% compression rate is 12.9%, and the weight gain rate of direct impregnation without pressure is 7.6%. When the compression rate is 50%, the wood weight gain rate of LW-109 is greater than that of LW-111; when the compression rate is 0%, the wood weight gain rate of LW-111 is greater than that of LW-109. The intermittent loading and unloading impregnation method can increase the impregnation effect of the two wax emulsions, and the improvement effect on LW-109 is more obvious.

[0142] Effects of different compression rates of Pinus sylvestris var. mongolica and PEW emulsion types on the impregnation permeability of wood surface Fig. 9 As shown. Whether it is LW-109; or LW-111, intermittent loading and unloading can significantly improve the effect of PEW emulsion impregnation on the wood surface. At the same time, for larch wood, when LW-111 is dried from wet weight to dry weight, the decrease in wood weight gain rate is less than that of LW-109. The wax emulsion has a larger density and less water loss during the drying process. The dry weight gain rate of LW-109 with a compression rate of 50% larch is 28.8%, and the weight gain rate of direct impregnation without pressure is 7.5%; the weight gain rate of LW-111 with a compression rate of 50% is 14.5%, and the weight gain rate of direct impregnation without pressure is 6.6%. Therefore, the impregnation effect of LW-109 wax emulsion with a compression rate of 50% is improved by 73.9%; the impregnation effect of LW-111 wax emulsion is improved by 48.2%. No matter when the compression rate is 50% or 0%, the impregnation effect of LW-109 is better than that of LW-111. When the compression rate is 50%, the impregnation effect of LW-109 on Larix gmelinii is significantly improved, which is far better than the other three impregnation conditions.

[0143] The compression rate greatly improves the impregnation effect of both tree species, and LW-109 wax emulsion has the best weight gain rate at 50% compression rate. However, the degree of influence of pretreatment conditions and cycle frequency is different. Under the effect of compression rate and different wax emulsions, the improvement effect of the weight gain rate of Pinus sylvestris exceeds that of Okoume. For both tree species, the weight gain rate of LW-111 decreases less during the drying process. This is because the density of LW-111 itself is large. When the wood absorbs the same volume of PEW emulsion, the remaining mass is larger after drying. The impregnation effect of the wood surface with 50% compression rate is significantly better than that of the wood with 0% compression rate, which is the same as the test results of wood rebound in Chapter 2. Among the two wax emulsions, the best impregnation wax emulsion for Okoume and Pinus sylvestris is LW-109PEW wax emulsion.

[0144] Effects of different tree species on the impregnation permeability of wood surface:

[0145] Effects of different tree species on the impregnation permeability of wood surface Fig.10 As shown, the black line segment is okoume (A), corresponding to the left vertical axis; the red dotted line is Pinus sylvestris (Z), corresponding to the right vertical axis. The wood weight gain rate of okoume during the drying process decreased more than that of Pinus sylvestris. This is because okoume itself has a large density and fine pores, and the wood can absorb less wax emulsion. Most of the wax emulsion is adsorbed on the surface of the wood and falls off more during the drying process; while there are a large number of resin ducts visible to the naked eye in Pinus sylvestris, which provide a natural place for the retention of PEW emulsion. Therefore, during the drying process, compared with okoume, Pinus sylvestris loses less wax emulsion.

[0146] In the case of dry weight, the weight gain rate of okoume with a short cycle frequency of 9 times is 3.2%, the weight gain rate with a long cycle frequency of 1 time is 13.4%, and the weight gain rate with a pretreatment time of 60 minutes is 6.8%; the weight gain rate of Pinus sylvestris var. mongolica with a short cycle frequency of 9 times is 8.0%, the weight gain rate with a long cycle frequency of 1 time is 28.8%, and the weight gain rate with a pretreatment time of 60 minutes is 10.6%. Numerically, the various impregnation methods have a greater improvement on the impregnation effect of Pinus sylvestris var. mongolica than that of okoume, but the improvement degree of pretreatment time on okoume is due to Pinus sylvestris var. mongolica. This is because okoume contains a large amount of calcium oxalate, calcium carbonate, silica and other inclusions. After steaming + microwave pretreatment, the wood inclusions will be greatly reduced, and the blockage inside the wood will be cleared. However, Pinus sylvestris var. mongolica wood has good wood permeability, and long-term impregnation itself can achieve good impregnation effect. Before impregnation, it is pressurized to make use of its strong wood rebound ability to achieve a more ideal impregnation effect.

[0147] Impact of surface impregnation weight gain rate of Pinus sylvestris var. mongolica borer wood:

[0148] Effect of drilling on weight gain of Scotch pine wood after impregnation Fig.11 As shown. In order to explore the most convenient and best impregnation process of PEW emulsion impregnation wood, the wood is drilled when the size and strength of the wood allow. The drilling process does not affect the impregnation effect of PEW that is not on the end surface, but increases the contact area between the side of the wood and the wax. The presence of through holes allows the wax emulsion to enter the wood more freely and deeply, greatly enhancing the impregnation effect of PEW. Drilling holes in Pinus sylvestris wood can significantly increase the impregnation weight gain rate of the wood, and the weight gain rate increases positively with the number of holes. Due to the increase in the number of holes, the specific surface area of ​​the wood is greatly increased. At the same time, drilling holes on the side solves the problem that the compressed wood only has good absorption effect at the end. Under the condition of dry weight with 1 hole, the weight gain rate of the wood is 43.8%, and the weight gain rate of the wood with 4 holes is 61.8%. The weight gain rate of the wood increased by 34.2% for a single hole, and the weight gain rate of the wood increased by 53.3% for 4 holes.

[0149] Summarize:

[0150] (1) The frequency of intermittent loading and unloading can promote the multiple absorption of PEW emulsion by the wood surface. The increase in the wax content of the wood surface shows a trend of first increasing and then decreasing with the increase in frequency. The impregnation cycle is an important factor affecting the wax impregnation of the wood surface. In the short-cycle impregnation process, the comprehensive impregnation effect is best when the frequency is 9; in the long-cycle impregnation process, the comprehensive impregnation effect is better when the frequency is 1.

[0151] (2) Microwave and steam pretreatment can effectively improve the air permeability of wood and promote the impregnation and penetration of wax emulsion. Pretreatment time is an important process factor to improve the impregnation efficiency of wood wax emulsion. The wax impregnation weight gain rate of wood increases with the increase of pretreatment time. The change trend of the impregnation weight gain rate of okoume wood and larch wood with the pretreatment time is consistent, and the impregnation efficiency of larch wood is slightly lower than that of okoume. When the pretreatment time of okoume wood is 30min steaming + 3min microwave, 60min steaming + 6min microwave and 120min steaming + 9min microwave, its weight gain rate in dry state is increased by 4.2%, 6.8% and 7.8% compared with the untreated wood, respectively. After the larch wood is treated in the same way, its weight gain rate is increased by 9.3%, 10.6% and 12.5% ​​compared with the untreated wood, respectively. Considering the processing efficiency and time cost, the best pretreatment time for okoume and larch wax impregnation wood is steaming for 60min + microwave for 6min.

[0152] (3) The molecular weight of the wax in the wax emulsion has a direct impact on the density of the emulsion. The larger the molecular weight, the greater the density of the emulsion. Emulsions with large molecular weight are not conducive to impregnation and penetration of wood. The impregnation effect of LW-109, a wax emulsion with a smaller density, is better than that of LW-111. Compared with Okoume, Larix gmelinii wood showed better impregnation effect in both wax emulsions. Among various impregnation methods, Larix gmelinii wood was impregnated with LW-109 wax emulsion for a long period of time and multiple times, and the impregnation weight gain rate reached 29%.

[0153] (4) Compared with the immersion method, the PEW intermittent loading and unloading impregnation of wood has high efficiency and good protection effect. Compared with the high-pressure impregnation method, the process is simple, the impregnation does not require a vacuum pressure tank, and the application advantages are obvious.

[0154] The following is an evaluation of the performance of PEW emulsion intermittent loading and unloading impregnated wood:

[0155] Any wood product needs to be used in a specific environment. Durable wood products are difficult to avoid rain, extreme environments, and ultraviolet radiation during service. The resulting dimensional changes, cracking, aging, discoloration, and other damages seriously reduce their service life. Wood dimensional stability, freeze-thaw resistance, and aging resistance are basic indicators for evaluating the use of durable wood, and are important parameters for understanding wax-impregnated wood.

[0156] To this end, in response to the problems that the above-mentioned durable wood may face, the following focuses on the technical requirements of PEW emulsion-impregnated wood construction applications, explores the impregnation degree of PEW emulsion-impregnated wood, and uses methods such as wood water absorption and expansion, freeze-thaw cycles, and ultraviolet accelerated aging to simulate the use environment of durable wood, and comprehensively evaluates the performance and use performance of PEW emulsion-impregnated wood in outdoor environments.

[0157] a. Test materials and methods:

[0158] a.1. Materials and equipment:

[0159] Test materials: Okoume and Scots pine wood. PEW impregnated wood was collected and its properties were studied.

[0160] The test equipment mainly includes: (1) Electric heating constant temperature water bath DK-600B. The temperature adjustment range is RT+5℃~99℃, the temperature fluctuation range is ±0.5℃, and the maximum power is 1000W. (2) Environmental scanning electron microscope FEIQuanta250. (3) Freezer ZH-20W50, with a volume of 50L and a minimum control temperature of -25℃. (4) UV ultraviolet aging instrument, with a frequency of 50HZ and a power of 2500W.

[0161] a.2. Test method:

[0162] (1) Observation method of inner wax layer on wood surface:

[0163] Small pieces with a cross section of 5 mm x 5 mm were peeled from the surface cross section and radial section of wax emulsion impregnated wood of Okoume and Pinus sylvestris after short-term 9 times, long-term 1 time, steaming + microwave pretreatment, respectively. There was no requirement for the height. The surface peeling position was 5 mm away from the end and side faces, and the inner layer peeling position was 5 mm away from the surface of the impregnated wood. The samples were as follows: Fig.12 As shown in (a) and (b) in the figure, the specimens were sprayed with gold and then observed under a scanning electron microscope. In order to observe the wood and PEW as finely as possible, low-power microscope and high-power microscope were used for observation. The distribution of wax emulsion impregnation on the wood surface was observed with a low-power microscope, and the vertical impregnation depth of the wood was observed with a high-power microscope. The specimen design is shown in Table 1. The impregnation wax emulsions are LW-109 and LW-111, which are replaced by Ⅰ and Ⅱ in the grouping table.

[0164] (2) Measurement method of wood swelling:

[0165] The test was conducted with reference to the national standard GB / T 1934.1-2009 "Determination of water absorption of wood". Before impregnation, the wood was dried and the moisture content of the wood was controlled to be absolutely dry. The tangential and radial dimensions were measured and recorded as L0. The constant temperature and humidity chamber was set at 20±2℃. The specimen was measured repeatedly with a measurement interval of 48h. At this time, the wood size measured each time was L1. Until there was no obvious change in the measured wood size (the moisture content reached saturation), the specimen design is shown in Table 1. Since wax emulsion will precipitate during the impregnation process, the wood was replaced with water after each measurement. The water absorption expansion rate of the specimen was calculated according to the following formula.

[0166]

[0167] Where: α is the water absorption expansion rate of wax impregnated wood, %; L1 is the radial or tangential dimension of the sample during water absorption, mm; L0 is the radial or tangential dimension of the sample before moisture absorption, mm.

[0168] (3) Treatment method for wood resistance to freeze-thaw cycles:

[0169] The test was conducted in accordance with the "Determination of Freeze-Thaw Cycle Resistance of Building Coatings" (GB9154-1988). The specimens were placed in a constant temperature and humidity chamber, the water temperature was controlled at 23±1℃, and the immersion time was 18h. After taking it out, wipe off the surface moisture, put it in a refrigerator at -10±1℃ and freeze it for 3h, and then put it in a 50±1℃ oven for constant temperature heat treatment for 3h. Each water immersion for 18h, freezing for 3h, and hot baking for 3h is a cycle. A total of 4 groups of specimens were set up, and 3 groups of specimens were cycled 5, 10, and 15 times respectively. In addition, it was always set as a control group, and 3 repeated samples were set up in each group. After the cycle was completed, the moisture content of the wood was measured, and the surface state and surface hardness of the specimens were observed and the test was set up. The specimen design is shown in Table 1.

[0170] The wood hardness test refers to the "Wood Hardness Test Method" (GB / T1941-2009), and the hardness test is carried out on the center of the specimen using a pressure head size of 5.64mm, and the loading speed is set to 2mm / min. The wood hardness of the specimen at this moisture content is calculated according to the following formula.

[0171] H W =KP×100%;

[0172] Where: H W —The hardness of the wood when the moisture content of the wood specimen is W, N; K—The coefficient when the depth of the specimen is 5.64 mm, generally 1; P—The load that the wood bears when the hemispherical indenter is completely pressed into the wood, N.

[0173] (4) Wood UV accelerated aging treatment method:

[0174] The test was conducted in accordance with the aging test method for rubber materials (GB / T14522-2008), with the lighting temperature set to (50±3)℃, continuous lighting for 8 hours, followed by a 4-hour stop, 12 hours as one cycle, and 12 cycles in total. After the continuous lighting was completed, the changes on the wood surface were observed, and then the wood slices were scanned by an environmental electron microscope to observe the changes in the wood at the microscopic level. The specimen design is shown in Table 1.

[0175] a.3. Experimental design:

[0176] The specific design scheme is shown in Table 1, which is the specimen grouping table.

[0177]

[0178]

[0179]

[0180] b. Results analysis and discussion:

[0181] b.1. Analysis of PEW distribution in the inner layer of wood surface:

[0182] (1) Analysis of PEW distribution on wood surface:

[0183] Scanning electron microscopy can truly reflect the bonding between wood and PEW emulsion at a microscopic level. Typical PEW emulsion impregnation wood surface SEM images of 9 intermittent loading and unloading in a short cycle Fig.13 As shown. Most of the wood end surface has been covered with wax, especially the side of the wood end surface, where the wax impregnation effect is relatively uniform, but the impregnation effect in the center of the wood is not ideal. The early wood area has obvious characteristics, the cell cavity is small, and the wax adheres to the cell wall surface and occupies part of the cell cavity space. In the radial section, the wood cell wall is almost completely covered with wax. After the PEW emulsion dries, the distribution of wax is strip-shaped, and it is concentrated in the early wood area. This is because Pinus sylvestris var. mongolica is a species that changes rapidly from early to late wood. The early wood grows faster, the cambium cells are active, the wood cells formed are larger, the cell walls are thinner, the wood fiber components are less, and the material appears loose. Therefore, the permeability of the wood in the early wood is better. The late wood is the secondary xylem formed by the wood in the late growing season. During this period, the climate generally becomes dry and cold, and the cambium activity weakens. At this time, the cells formed are smaller, the cell walls are thick and flat, and the material appears tight and solid. Therefore, the permeability of the wood in the late wood is lower than that of the early wood. The cell cavity in the early wood is large and the wood permeability is good, which gives the wax emulsion enough space to enter the wood cells. The distribution of wax in the figure is strip-shaped. At the same time, the volume of PEW emulsion shrinks after solidification, which will cause some cells to be exposed outside on the cross section.

[0184] (2) Analysis of PEW distribution in the inner layer of wood:

[0185] SEM of the inner layer of wood impregnated with PEW emulsion Fig.14 As shown. For the long-term intermittent loading and unloading impregnation of the wood surface, the amount of wax emulsion attached to the wood cell surface after solidification is small, the cell characteristics of the cross section and radial section are relatively clear, and the impregnation of the inner layer of the wood is still difficult. The wax emulsion inside the wood condenses less wax after drying, and Oguman is only distributed in a small amount on the edge. The color of Oguman wood itself is darker, and the color difference with the solid wax is large and easy to observe. The wax inside Oguman is tightly combined with the wood and presents block shape. However, the solid wax inside the Larix gmelinii wood is relatively loose and not well combined with the wood. Only a small amount of solid wax is condensed in the pits, and it is difficult to clearly distinguish the wax and wood. Overall, the wax is in the form of smaller blocks and is partially uneven. Even if a relatively complete wax film has been formed on the surface of the wood, it still takes a certain amount of time, that is, the impregnation cycle, for the wax emulsion to be impregnated into the interior of the wood. In addition, the PEW molecule itself is a macromolecular impregnating agent, which makes impregnation difficult. Therefore, if you want to ensure a good impregnation effect, you need to extend the impregnation cycle and frequency while ensuring that the surface of the wood is completely impregnated to ensure that there is enough wax inside the wood to protect the wood from erosion.

[0186] b.2. Analysis of swelling properties of impregnated wood during intermittent loading and unloading:

[0187] The radial and chordal water absorption expansion rates of Okoume and Pinus sylvestris PEW emulsion samples in distilled water at room temperature are as follows: Fig.15 , 16 As shown in (a)-(b). Overall, regardless of the tree species, treatment cycle length, pretreatment, and wax emulsion type, the water absorption expansion rate of PEW emulsion-impregnated wood specimens is lower than that of untreated specimens, indicating that PEW intermittent loading and unloading impregnation treatment can effectively improve the dimensional stability of wood. The radial and tangential impregnation expansion rates of Okoume are both greater than those of Pinus sylvestris; in the case of the same tree species, the radial impregnation expansion rates of Okoume and Pinus sylvestris are both lower than those of Pinus sylvestris. The impregnation expansion rate of wood treated for a long period is lower than that of wood treated for a short period, which also indirectly reflects that the wax weight gain rate of wax-impregnated wood treated for a long period is higher than that of wood treated for a short period. For pretreated wood, the swelling of wood will increase to a large extent regardless of whether it is treated with PEW emulsion intermittent loading and unloading impregnation. For the type of wax emulsion, only the tangential impregnation expansion rate of Okoume treated with LW-111 is lower, and the impregnation expansion rate of the rest of the wood treated with LW-109 is lower than that of LW-111.

[0188] Depend on Fig.15It can be seen that the impregnation expansion rate of the untreated wood is less than that of the pretreated wood, but greater than that of the pretreated and PEW emulsion treated wood. At the same time, when DY was impregnated for 6-8 days, the wood showed a large impregnation expansion. This shows that while pretreatment increases the permeability of wood and reduces the difficulty of wood wax impregnation, it also increases the swelling of wood and reduces the dimensional stability of wood; at the same time, wax will gradually disappear during the impregnation of wood, and the loss of wood in the pretreatment group is more obvious. The radial PEW wax-treated wood impregnation expansion rate is about 3%, and the tangential one is about 5%. The best Okoume wax treatment is ACI-1, which is about 2.6%; the best wax treatment of Pinus sylvestris is ZC-Ⅰ-1, which is about 2.2%. The impregnation expansion rate of wood treated with a long cycle is lower than that of wood treated with a short cycle. The short-cycle impregnation expansion in the tangential direction of Okoume (8.1%) is 30.1% higher than that of the long-cycle impregnation expansion (5.6%); the short-cycle impregnation expansion in the tangential direction of Larix gmelinii (6.1%) is 32.7% higher than that of the long-cycle impregnation expansion (4.1%). Compared with the conventional impregnation treatment, the radial dimensional stability of Okoume and Larix gmelinii treated with intermittent loading and unloading has increased by 34.8% and 27% respectively, and the tangential dimensional stability has increased by 23.7% and 12.5% ​​respectively. Therefore, whether it is from the weight gain of wax or the impregnation expansion rate of wood, the intermittent loading and unloading long-cycle frequency is more reasonable. For the type of wax emulsion, whether it is Okoume for hardwood or Larix gmelinii for coniferous wood, or the long-cycle frequency or the short-cycle frequency, the impregnation expansion rate of wood impregnated with PEW emulsion LW-109 is lower, that is, it is more suitable for impregnating wood.

[0189] b.3. Analysis of freeze-thaw cycle resistance of intermittent loading and unloading impregnated wood:

[0190] (1) Surface condition:

[0191] During the cycle, wood not only has to endure the dimensional changes caused by moisture absorption and expansion, but also has to withstand the aging test caused by temperature difference. Typical wood freeze-thaw cycle test pieces are as follows: Fig.17As shown in (a)-(c) in the figure. The degree of damage of the wax-impregnated wood specimens will gradually increase with the increase of freeze-thaw cycles. Most of the wood on the end surface of the wood is still covered by PEW, but PEW will gradually fall off and lose with the increase of freeze-thaw cycles. During the loss process, the wood gradually produces shrinkage cracks, and the cracks mostly occur at the wood rays. This is because in the cyclic treatment test at a temperature of -10℃~50℃, most of the water in the wood exists in the form of free water, and the water transfer rate is relatively fast; at the same time, the cell arrangement at the wood rays is different from the arrangement of wood fiber cells, which is also an important reason for the cracking of the wood here. After 10 cycles, small cracks began to appear in the wood, that is, the PEW emulsion wax impregnated wood can protect the wood from 10 freeze-thaw cycles under the intermittent loading and unloading production process. When the wood is subjected to high temperature, the wood loses water and shrinks, causing the wax on the surface of the wood to change and the wax on the wood to gradually fall off, which is also an important reason for the reduction of the aging resistance of the PEW wax-impregnated wood.

[0192] (2) Surface hardness:

[0193] Hardness analysis of wood freeze-thaw cycle test specimens Fig.18 As shown, Fig.18 In the figure: W means untreated; L1 means treated with LW-109 wax emulsion; L2 means treated with LW-111 wax emulsion; C means long-term wax impregnation treatment; D means short-term wax impregnation treatment; Y means pretreatment. The hardness of wood is positively correlated with the surface wax content and the wax impregnation effect. The long-term impregnation PEW emulsion LW-109 has the best protection effect on wood. After the cycle, there is still a small amount of wax residue on the surface of the wood. When the moisture content is 12%, the hardness of Okoume without freeze-thaw cycle treatment can reach 2658N, and the hardness of Pinus sylvestris is 2184N. After the microwave pre-treated wax impregnated wood undergoes freeze-thaw cycles, the hardness of Okoume wood is only 1726.7N, and the hardness of Pinus sylvestris is 1102.8N. At this time, the hardness of the wood decreases by 35% and 49.5%, respectively. Long-term impregnation has the best protective effect on wood hardness, with Okoume and Scots pine decreasing by 6.8% and 25.7% respectively. Therefore, the degree of damage to Scots pine in terms of hardness caused by freeze-thaw cycles is much greater than that of Okoume. There is also a significant difference in the protective ability of the two wax emulsions for wood hardness. The protective ability of PEW emulsion LW-109 is better than that of LW-111. Under short-term PEW emulsion LW-109, the hardness of Okoume is 11.1% higher than that of LW-111, and the hardness of Scots pine is 19.9% ​​higher than that of LW-111.

[0194] b.4. SEM image analysis of the surface interface of wood impregnated with accelerated aging wax:

[0195] Fig.19 This is a SEM image of PEW impregnated wood after UV-accelerated aging. PEW has a certain protective effect on wood during the accelerated aging process, but the protective capacity is limited. After a 96-hour UV irradiation cycle, the surface of the wax-impregnated wood became uneven and the surface layer was partially degraded. The wood surface of Okoume wood is severely degraded, and the color difference of Larix gmelinii wood is smaller than that of Okoume, which directly reflects that the PEW emulsion impregnation effect of Larix gmelinii is better than that of Okoume. During the UV-accelerated aging process of wax-impregnated wood, not only the surface of the wood is uneven, but also the surface of the wood is accompanied by small fine lines. This is because ultraviolet rays destroy the cell structure of short-period wax-impregnated wood, reduce the lignin content inside the wood cells, thin the wood cell walls, and cracking occurs. It also directly reflects that the effect of intermittent loading and unloading PEW emulsion is better for long-period impregnation of wood than for short-period impregnation of wood.

[0196] c. Conclusion:

[0197] (1) Scanning electron microscopy can truly reflect the bonding between wood and PEW emulsion under microscopic conditions. For the surface of wood impregnated for a long period and low frequency, the wax emulsion is completely attached to the surface of wood cells after solidification, and the bonding is good. In the cross section, the characteristics of the early wood area are more obvious, the cell cavity is smaller, and the wax is attached to the cell wall surface and occupies part of the cell cavity space. In the radial section, the wood cell wall is almost completely covered with wax. For the surface of wood impregnated for a short period and high frequency, the amount of wax emulsion attached to the surface of wood cells after solidification is small, and the cell characteristics of the cross section and radial section are relatively clear.

[0198] (2) Wax emulsion impregnation treatment of the wood surface can not only save the amount of wax emulsion, but also improve the hydrophobicity of the wood, effectively protect the wood, and improve the dimensional stability of the wood. The dimensional stability of the wood impregnated with wax emulsion has been greatly improved, and the degree of improvement is directly related to the impregnation treatment method. Compared with the conventional impregnation treatment, the radial dimensional stability of Okoume and Larix gmelinii impregnated materials increased by 34.8% and 27% respectively, and the tangential dimensional stability increased by 23.7% and 12.5% ​​respectively.

[0199] (3) Wax emulsion impregnation treatment on the wood surface can not only improve the wood's resistance to freezing and thawing, but also improve the wood's resistance to ultraviolet aging. Under extreme high and low temperature cycles, the wood did not crack before 10 cycles; when the number of cycles reached 15, the wood began to produce shrinkage cracks, mostly at the wood rays. After 96 hours of ultraviolet irradiation, the wax-impregnated wood partially degraded on the surface and the lightness of the wood decreased; the ability of the wood impregnated with okoume wax to resist ultraviolet aging was lower than that of the wood impregnated with larch wax.

[0200] This paper focuses on the technical needs of PEW emulsion impregnated wood construction applications, takes Okoume and Pinus sylvestris as research objects, and systematically studies the basic performance of compression and rebound of wood after intermittent loading and unloading, the surface permeability of PEW emulsion impregnated wood, and the performance of impregnated wood through intermittent loading and unloading. The main research results are as follows:

[0201] (1) Based on the compression and rebound characteristics of wood, the PEW emulsion is impregnated into the wood by utilizing the air pressure difference inside and outside the wood during intermittent loading and unloading, which is an effective method to reduce the difficulty of impregnation of the wood surface under normal pressure. The use of this technology facilitates the use of the hydrophobic advantages of PEW materials and the porosity advantages of wood components. Compared with the immersion method, the PEW intermittent loading and unloading impregnation of wood has high efficiency and good protection effect. Compared with the high-pressure impregnation method, the process is simple, the impregnation does not require a vacuum pressure tank, and the application advantages are obvious.

[0202] (2) The performance of okoume and larch wood in the intermittent loading and unloading process is different from that in monotonous loading and unloading, mainly in terms of the instantaneous rebound rate of wood and the peak load at the same compression ratio. The cross-grain compression process of okoume and larch wood can be divided into three stages. The first stage is the elastic stage of early wood compression, and the load increases linearly with displacement; the second stage is the early wood compression loss process stage, and the load increases with displacement in a curve shape; the third stage is the late wood compression stage, during which the early wood appears to be crushed. When the intermittent loading and unloading process is selected in the first two stages of compression, okoume and larch wood can obtain a large compression ratio while maintaining good elastic properties, and the shape memory characteristics are obvious. The instantaneous rebound rate and the peak load when compressed to the same compression ratio during the intermittent loading and unloading process will gradually decrease with the increase of the frequency of intermittent loading and unloading. After 6 intermittent loading and unloading cycles, the instantaneous rebound rate of okoume decreased by 13.7% and the peak load decreased by 15.2%; the instantaneous rebound rate of larch decreased by 14.8% and the peak load decreased by 13%.

[0203] (3) Okoume and Scots pine were treated with steaming + microwave, which not only improved the air permeability of the wood, but also significantly improved its compression rebound. The rebound rate of the untreated wood was lower than that of the pretreated wood, and the wood rebound rate increased with the extension of the pretreatment time. The most reasonable pretreatment time for Okoume and Scots pine was steaming for 60 minutes + microwave for 6 minutes, which was about 9% higher than the pretreatment of steaming for 30 minutes + microwave for 3 minutes, but the degree of improvement in rebound rate was 2% lower than the pretreatment of steaming for 120 minutes + microwave for 9 minutes.

[0204] (4) The frequency of intermittent loading and unloading is conducive to promoting the multiple absorption of PEW emulsion by the wood surface, and its impregnation amount is significantly improved. The weight gain of wax-impregnated wood increases rapidly at first, then gradually slows down and finally begins to decline. In the process of intermittent loading and unloading of wood for wood impregnation modification, the frequency has a greater impact on short-cycle wood impregnation than long-cycle. Among the short-cycle frequencies, 9 times of impregnation has the most ideal effect. The dry weight gain rate of Okoume wood is 59% higher than that of the specimens treated with 3 times of intermittent loading and unloading, and that of Pinus sylvestris is 45% higher. Among the long-cycle frequencies, the weight gain rate of wood impregnated once is the most reasonable.

[0205] (5) Pretreatment helps improve the permeability of wood. The weight gain rate of wood PEW emulsion impregnation increases with the increase of pretreatment time. The influence of pretreatment time on okoume and Pinus sylvestris is roughly the same, and the improvement of the weight gain rate of Pinus sylvestris is less than that of okoume.

[0206] (6) The molecular weight of the wax in the wax emulsion has a direct impact on the density of the emulsion. The larger the molecular weight, the greater the density of the emulsion. A large molecular weight is not conducive to the penetration and impregnation modification of wood. The impregnation effect of LW-109, which has a smaller wax emulsion density, is better than that of LW-111. The impregnation effect of PEW emulsion on larch, which has good elastic recovery of the wood itself, is better than that on okoume. The best impregnation effect is larch with LW-109 wax emulsion impregnated for a long period of time. The impregnation weight gain rate after the wood is dried is 29%.

[0207] (7) Scanning electron microscopy can truly reflect the combination of wood and PEW emulsion in a microscopic state. During the intermittent loading and unloading impregnation process, after the wood surface is occupied by the wax emulsion, the emulsion dehydrates to form solid wax, and the wood end area is evenly covered with wax, but the impregnation effect in the wood side area is not ideal. The overall wax adsorption of Okoume is less than that of Pinus sylvestris. The distribution of PEW in the SEM image of the wood end surface appears in strips, and is mostly concentrated in the early wood area.

[0208] (8) PEW emulsion impregnated wood has good stability. The water absorption expansion rate and dimensional stability of the treated wood are greatly improved compared with the untreated specimens. The radial PEW emulsion impregnation modified wood expansion rate is about 3%, and the tangential direction is about 5%. Compared with the untreated specimens, the tangential water absorption expansion rate of Okoume decreased by 62.5% and the radial direction decreased by 50%; the tangential water absorption expansion rate of Pinus sylvestris var. mongolica decreased by 68.9% and the radial direction decreased by 42.8%.

[0209] (9) Freeze-thaw cycles can reflect the performance of wax-impregnated wood in extreme environments. Intermittent loading and unloading of PEW emulsion impregnated wood in a short period of time can achieve better performance. During the freeze-thaw cycle, the wood was not significantly damaged before the temperature and humidity acted synergistically for 10 times; but when the number of cycles reached 15 times, shrinkage cracks gradually appeared in the wood, and the cracks mostly occurred at the wood rays.

[0210] (10) After the wax-impregnated wood was exposed to ultraviolet light for a cycle, the lightness of the wood decreased, the color deepened, and the wood surface became uneven in the SEM image, indicating partial degradation. The color difference of Pinus sylvestris was smaller than that of Okoume, which directly reflects that the PEW emulsion impregnation effect of Pinus sylvestris was better than that of Okoume.

[0211] The protection scope of the present invention includes but is not limited to the above embodiments. The protection scope of the present invention shall be based on the claims. Any replacement, deformation, and improvement of the technology that can be easily thought of by technicians in this field shall fall within the protection scope of the present invention.

Claims

1. A method for impregnating a wood surface layer with a wax emulsion, characterized in that: The following steps are involved: Step 1: Pre-treat the wood; Step 2: Immersing the pretreated wood in wax emulsion; Step 3: Pressurizing the wood immersed in the wax emulsion, and releasing the pressure after the pressurization is completed; Step 4: Remove the wood from the wax emulsion, wipe off the wax emulsion on the surface of the wood, and dry the wood.

2. The method for impregnating a wood surface layer with a wax emulsion according to claim 1, characterized in that: The step 1 is specifically as follows: Step 1.1, measure the moisture content of the wood, and the obtained moisture content is A0; Step 1.2, steaming the wood, and placing the steamed wood in a microwave oven for microwave treatment; Step 1.3: After the microwave is finished, measure the moisture content of the wood to ensure that the current moisture content of the wood is consistent with the moisture content measured in step 1.

1.

3. The method for impregnating a wood surface layer with a wax emulsion according to claim 2, characterized in that: Before step 1.1, the wood is also perforated on the side, and the perforations are holes penetrating the wood.

4. The method for impregnating a wood surface layer with a wax emulsion according to claim 2, characterized in that: The step 1.2 is specifically as follows: steaming the wood by using water vapor generated by heating in an electrically heated constant temperature water tank, the heating temperature being 95° C. After the water temperature rises to 95° C., putting the wood in, starting the timing, and completing the steaming after the steaming treatment time is reached; putting the steamed wood in a microwave oven for microwave treatment, setting the firepower of the microwave oven to high, and completing the microwave treatment after the microwave treatment time is reached.

5. The method for impregnating a wood surface layer with a wax emulsion according to claim 4, characterized in that: The steaming treatment time is 30min-120min, and the microwave treatment time is 3min-9min.

6. The method for impregnating a wood surface layer with a wax emulsion according to claim 1, characterized in that: The wax emulsion adopts LW-109 PEW emulsion.

7. The method for impregnating a wood surface layer with a wax emulsion according to claim 1, characterized in that: The step 3 is specifically as follows: using a mechanical testing machine to pressurize the wood immersed in the wax emulsion, the pressurization method is short-cycle intermittent loading and unloading or long-cycle intermittent loading and unloading, and the pressure is released after the pressurization is completed.

8. The method for impregnating a wood surface layer with a wax emulsion according to claim 7, characterized in that: When the pressurization mode is short-cycle intermittent loading and unloading, the pressurization speed is 10mm / min, the wood compression ratio is set to 50%, the pressure relief speed is 40mm / min, the impregnation time after each pressure relief is 3min, and the cycle frequency of intermittent loading and unloading is 3-9 times; When the pressurization method is long-cycle intermittent loading and unloading, the pressurization speed is 10mm / min, the wood compression ratio is set to 50%, the pressure relief speed is 40mm / min, the immersion time after each pressure relief is 14h, and the cycle frequency of intermittent loading and unloading is 1-3 times.

9. The method for impregnating a wood surface layer with a wax emulsion according to claim 1, characterized in that: The wood includes okoume wood or larch wood. The pressure bearing direction of intermittent loading and unloading of okoume wood is tangential pressure, while the pressure bearing direction of intermittent loading and unloading of larch wood is radial pressure.

10. The method for impregnating a wood surface layer with a wax emulsion according to claim 1, characterized in that: The step 4 is as follows: taking the wood out of the wax emulsion and wiping the wax emulsion on the surface of the wood; then, placing the wood in an electric constant temperature air drying oven for drying at a drying temperature of 50° C. During the drying process, the moisture content of the wood is measured every 0.5 hours until the moisture content of the wood is reduced to A0, and then the drying is stopped.

Citation Information

Patent Citations

  • Solid wood floor processing technology for impregnation modified fast growing wood floor heating

    CN107856160A

  • Treatment process for improving stability of wooden material

    CN108748505A