Preparation method of ultralow-energy-consumption LUHPC for novel door and window auxiliary frame

By using lightweight ultra-high performance concrete, combined with artificial lightweight shale clay sand and PVA fiber, the problems of low strength, poor durability and poor energy-saving and environmentally friendly doors and windows are solved, and high-strength, good thermal insulation and energy-saving are achieved. The environmentally friendly effect reduces energy consumption and maintenance costs.

CN118990732APending Publication Date: 2024-11-22CHINA THREE GORGES UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410922635.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing door and window frames have problems such as low strength, poor durability and poor energy-saving and environmentally friendly frames, especially the performance of traditional materials in high temperature environments and high maintenance costs.

Method used

Lightweight ultra-high performance concrete is used to prepare high compressive strength by using artificial lightweight shale clay sand and PVA fiber, combined with P·O52.5 cement, fly ash, silica fume and polycarboxylic acid water reducer , doors and windows with low thermal conductivity and heat transfer coefficients improve their strength, insulation performance and durability.

Benefits of technology

It realizes the high strength, good thermal insulation performance and energy-saving and environmentally friendly frames of doors and windows, reduces energy consumption and maintenance costs, and simplifies the construction process, adapts to various environmental conditions, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A novel door and window auxiliary frame ultra-low energy consumption LUHPC preparation method comprises the following steps that physical performance and chemical composition detection is conducted on raw materials needed by door and window auxiliary frame ultra-low energy consumption LUHPC, and it is ensured that all indexes of the raw materials meet standard requirements; the preparation method comprises the following steps: before preparation, weighing a small amount of materials which have the same proportion but are not doped with fibers, stirring and moistening a pot, weighing the mass of each material according to the designed mixing proportion, pouring the materials into a stirrer in sequence, stirring until slurry with certain fluidity is obtained, adding the fibers, and uniformly dispersing the fibers in the concrete; loading the concrete mixture into a mold brushed with a release agent in a layered manner, and placing a test block loaded with the mold on a concrete vibration table to be vibrated and compacted; covering the surface of the test piece with a plastic film in time for water retention maintenance after mold entering, moving the test piece into a room for maintenance, and removing the mold; after the test piece is demolded, putting the test piece into a standard curing box for curing; the problems that an existing door and window auxiliary frame is low in strength, poor in heat preservation and heat insulation performance and poor in energy-saving and environment-friendly effect are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of building materials, and specifically relates to a preparation method of a novel ultra-low energy consumption LUHPC (Lightweight Ultra-High Performance Concrete) for door and window frames. Background Art

[0002] The auxiliary frame of doors and windows, also called the secondary frame or auxiliary frame, is an auxiliary frame installed in the door and window openings. Its main function is to stabilize and protect the main frame, ensure the installation quality of doors and windows, and improve its anti-seepage, energy-saving and anti-deformation capabilities. In the field of construction, doors and windows are often one of the main parts that cause energy loss. Traditional door and window auxiliary frame structures often have problems with heat conduction and air leakage, which makes it difficult for buildings to stay warm in winter and cool in summer, thus seriously affecting indoor comfort and energy efficiency. The research on low-energy door and window frames is of vital importance, mainly in terms of energy conservation and carbon emission reduction. By improving thermal insulation performance, reducing heat conduction and air leakage, buildings can maintain indoor temperatures more effectively and reduce the need for heating and cooling. This not only reduces the energy consumption of buildings, but also helps to reduce carbon emissions, thereby combating climate change. To achieve this goal, we can effectively improve the energy performance of door and window frames and reduce energy consumption by introducing new materials, optimizing structural design, and improving sealing performance. This will make a positive contribution to the sustainable development of our construction industry.

[0003] For example, CN 111349292 A discloses a PVC-based profile for door and window frames and a preparation method thereof, wherein the PVC-based profile is composed of thermoplastic plastics (including PVC), plant fibers, fillers, silane coupling agents and additives. By using plant fibers and plastics of different types and mesh sizes, compatibility and mechanical properties can be improved. In addition, selecting suitable plastics can reduce water absorption, and adding suitable fillers can improve mechanical properties and heat resistance. However, the PVC-based profile is prone to decomposition and produces harmful gases when the ambient temperature is high, and the performance will also decline in a hotter environment. At the same time, the maintenance and repair of this material may require special techniques and materials, which may increase the long-term use cost.

[0004] For example, CN109422980A discloses an energy-saving and heat-insulating door and window frame material and its preparation method, which contains polyvinyl chloride, tung oil, propylene oxide, nano-ceramic hollow particles, wood powder, nano-titanium dioxide, modified shell powder, rosin, phosphite, composite flame retardant, silane coupling agent KH-550 and foaming agent. This material has the advantages of excellent mechanical impact resistance, high wear resistance, good corrosion resistance, low thermal conductivity, good thermal insulation, prevention of heat loss, energy saving and environmental protection, etc., but the material formula contains multiple ingredients, which will increase the complexity of production and processing and production costs, and has high requirements for production equipment and technology. If the material is damaged or needs to be replaced, the specific combination of ingredients may make repair and replacement complicated and expensive.

[0005] At present, according to the material classification of door and window auxiliary frames, there are steel auxiliary frames, aluminum alloy auxiliary frames, wood-plastic auxiliary frames, steel-plastic auxiliary frames, glass fiber reinforced plastic auxiliary frames, pure wood auxiliary frames, graphene polystyrene auxiliary frames, etc. These door and window auxiliary frames can improve the thermal insulation performance of doors and windows to a certain extent and reduce energy loss, but there are steel auxiliary frames that are easy to corrode and not energy-saving, aluminum alloy auxiliary frames with fast heat conduction, pure wood auxiliary frames with poor durability, and graphene polystyrene auxiliary frames with relatively high production costs. In view of the above situation and the fact that the performance of door and window auxiliary frames should meet the requirements of energy saving, high strength, and good durability, we propose a new preparation method for ultra-low energy consumption LUHPC for door and window auxiliary frames. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a new type of ultra-low energy consumption LUHPC for door and window auxiliary frames, so as to solve the problems of low strength, poor durability and poor energy-saving and environmental protection effects of existing door and window auxiliary frames. The door and window auxiliary frames made of lightweight ultra-high performance concrete have the advantages of high strength, good thermal insulation effect, and good energy-saving and environmental protection effect.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is a preparation method of a new type of ultra-low energy consumption LUHPC for door and window frames, comprising the following steps: Step 1: Conduct physical property and chemical composition tests on the raw materials required for the preparation of ultra-low energy consumption, lightweight and ultra-high performance concrete for door and window frames to ensure that all indicators of the raw materials meet the regulatory requirements; The physical properties and chemical composition tests are specifically: specific surface area, density, loss on ignition of P·O52.5 cement, fly ash, and silica fume; compressive strength, flexural strength, and setting time of P·O52.5 cement; fineness and bulk density of fly ash; alkali content and water demand ratio of silica fume; apparent density, bulk density, cylinder pressure strength, and water absorption of shale sand; density, water reduction rate, water bleeding rate ratio, and pH value of polycarboxylate water reducer; density, length, diameter, tensile strength, and elastic modulus of fibers; and at the same time, the chemical composition content of P·O52.5 cement, fly ash, and silica fume is tested respectively; Step 2: Before preparation, weigh a small amount of materials with the same mix ratio but without fibers, stir and lubricate the pot, weigh the mass of each material according to the designed mix ratio, pour them into the mixer in order, stir until the slurry has a certain fluidity, add fibers and evenly disperse them in the concrete; Step 3: Load the concrete mixture into the mold with release agent in layers, and place the molded test block on the concrete vibration table to vibrate and compact it; Step 4: After the mold is placed, the surface of the specimen is promptly covered with plastic film for water retention and curing, and the specimen is moved into a room at a temperature of 20±2℃ for curing for 24 hours before demolding; Step 5: After the specimen is demoulded, place it in a standard curing box and cure it using standard curing methods.

[0008] In the preferred scheme, the raw materials required for preparing the ultra-low energy consumption lightweight ultra-high performance concrete for the door and window frames in the Step 1 are P·O52.5 cement, silica fume, fly ash, shale ceramic sand, fiber, water and water reducer, the shale ceramic sand is artificial lightweight shale ceramic sand, and the designed mix ratios are 35%~40% by mass of P·O52.5 cement, 10%~15% by mass of fly ash, 8%~10% by mass of silica fume, 8%~14% by mass of water reducer, 1%~3% by mass of ceramic sand, 25%~35% by mass of fiber.

[0009] In a preferred embodiment, the order in which the materials are poured into the mixer in Step 2 is cementitious material, shale sand, a mixture of water and water reducing agent, and fiber.

[0010] In a preferred solution, the cementitious materials are P·O52.5 cement, silica fume and fly ash.

[0011] In a preferred embodiment, the particle size of the shale ceramic sand is in the range of 0-3 mm, and the water reducing agent used is a polycarboxylic acid water reducing agent, and the water reducing rate thereof is 25%-45%.

[0012] In the preferred scheme, the mass of each material is weighed according to the designed mix ratio in Step 2, poured into the mixer in order, and stirred to a slurry with a certain fluidity, that is, P·O52.5 cement, silica fume, fly ash and shale sand are added to the stirring pot, dry mixed for 3~5min, and then 2 / 3 of the mixture of water reducer and water is poured into the stirring pot, wet mixed for 2~3min, and finally the remaining water and water reducer are evenly poured into the stirring pot, and stirred to a slurry with a certain fluidity, and the fluidity is 160~170mm.

[0013] In a preferred embodiment, the fibers are added in Step 2 by slowly and evenly adding the fibers into a stirring pot and stirring for 5 minutes. During the stirring process, the stirring time can be appropriately shortened or increased according to the state of the mixture to ensure that the fibers are evenly dispersed in the concrete.

[0014] In a preferred embodiment, the fiber is PVA (Polyvinyl Alcohol) fiber.

[0015] In a preferred embodiment, the test block in Step 3 is vibrated on a vibration table for 2 minutes at a vibration frequency of 50 Hz until no more bubbles appear on the surface.

[0016] In the preferred solution, the indoor curing of the specimen in Step 5 adopts a standard curing method, that is, the curing temperature is 20±2°C, the curing humidity is above 95%, and the compressive strength of the specimen after curing is greater than 90MPa.

[0017] The invention provides a novel method for preparing ultra-low energy consumption LUHPC for door and window frames, which has the following beneficial effects: 1. The present invention uses artificial lightweight shale sand as light aggregate. Due to its low density and porous structure, it can effectively reduce the weight of door and window frames, has good thermal insulation performance, and helps to improve the energy efficiency of buildings; 2. The present invention uses PVA fiber as a reinforcing material. PVA fiber has high strength and modulus, can effectively disperse and absorb stress, prevent the generation and expansion of cracks, thereby improving the tensile and bending resistance of the door and window frames. The addition of PVA fiber with a lower density can reduce the deadweight of the door and window frames; 3. The lightweight ultra-high performance concrete prepared by the present invention has a fluidity of 160-170 mm, has good working performance, is easier to pour and vibrate during construction, reduces the labor intensity and time cost during pouring, and can better fill the template space, thereby reducing the generation of bubbles and voids, and improving the compactness and overall quality of the concrete; 4. The compressive strength of the lightweight ultra-high performance concrete prepared by the present invention is greater than 90MPa, which has sufficient compressive strength to support the weight of doors and windows, prevent them from deforming or sinking during use, and ensure that the integrity of the door and window structure is not destroyed under the effects of wind pressure, impact, etc.; 5. The thermal conductivity and heat transfer coefficient of the lightweight ultra-high performance concrete prepared by the present invention are both low, indicating that the door and window frames prepared with lightweight ultra-high performance concrete have good thermal insulation performance, improve energy-saving and environmental protection effects, and improve living comfort; 6. The lightweight ultra-high performance concrete door and window frames prepared by the present invention have low cost. Calculated based on the unit price of raw materials, the cost is 6.18 yuan / meter. At the same time, since lightweight ultra-high performance concrete has the advantages of high strength and good durability, it can effectively reduce the number of inspections and maintenance, thereby saving maintenance costs. In the long run, it has higher economic benefits.

[0018] 7. The present invention also performs well in weather resistance and corrosion resistance, can adapt to various harsh environmental conditions, and improves the service life of doors and windows; at the same time, its excellent sound insulation performance also greatly improves the quietness of the living environment; 8. The energy-saving design of the present invention significantly reduces energy consumption and saves a lot of energy costs; its unique green manufacturing process also reduces environmental pollution and meets the requirements of sustainable development; in addition, the door and window frames are easy to install and can be widely used in new buildings and old house renovation, with broad market prospects. DETAILED DESCRIPTION

[0019] Example 1 A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames comprises the following steps: Step 1: Conduct physical property and chemical composition tests on the raw materials needed to prepare ultra-low energy consumption, lightweight and ultra-high performance concrete for door and window frames to ensure that all indicators of the raw materials meet the specification requirements; The physical properties and chemical composition tests are specifically: specific surface area, density, loss on ignition of P·O52.5 cement, fly ash, and silica fume; compressive strength, flexural strength, and setting time of P·O52.5 cement; fineness and bulk density of fly ash; alkali content and water demand ratio of silica fume; apparent density, bulk density, cylinder pressure strength, and water absorption of shale sand; density, water reduction rate, water bleeding rate ratio, and pH value of polycarboxylate water reducer; density, length, diameter, tensile strength, and elastic modulus of fibers; and at the same time, the chemical composition content of P·O52.5 cement, fly ash, and silica fume is tested respectively; Step 2: Before preparation, weigh a small amount of materials with the same mix ratio but without fibers, stir and lubricate the pot, weigh the mass of each material according to the designed mix ratio, pour them into the mixer in order, stir until the slurry has a certain fluidity, add fibers and evenly disperse them in the concrete; Step 3: Load the concrete mixture into the mold with release agent in layers, and place the molded test block on the concrete vibration table to vibrate and compact it; Step 4: After the mold is placed, the surface of the specimen is promptly covered with plastic film for water retention and curing, and the specimen is moved into a room at a temperature of 20±2℃ for curing for 24 hours before demolding; Step 5: After the specimen is demoulded, place it in a standard curing box and cure it using standard curing methods.

[0020] In this embodiment, the raw materials required for preparing the ultra-low energy consumption lightweight ultra-high performance concrete for the door and window frames in Step 1 are P·O52.5 cement, silica fume, fly ash, shale ceramic sand, fiber, water and water reducer, the shale ceramic sand is artificial lightweight shale ceramic sand, and the designed mix ratios are 35%~40% by mass of P·O52.5 cement, 10%~15% by mass of fly ash, 8%~10% by mass of silica fume, 8%~14% by mass of water reducer, 1%~3% by mass of ceramic sand, 25%~35% by mass of fiber.

[0021] Furthermore, in the Step 2, the order in which the materials are poured into the mixer is the cementitious material, the shale sand, the mixture of water and the water reducing agent, and the fiber.

[0022] Furthermore, the cementitious materials are P·O52.5 cement, silica fume and fly ash.

[0023] Furthermore, the particle size range of the shale ceramic sand is 0-3 mm, and the water reducing agent used is a polycarboxylic acid water reducing agent, and its water reducing rate is 25%-45%.

[0024] Furthermore, in the Step 2, the mass of each material is weighed according to the designed mix ratio, poured into the mixer in order, and stirred to a slurry with a certain fluidity, that is, P·O52.5 cement, silica fume, fly ash and shale sand are added to the stirring pot, dry mixed for 3~5min, and then 2 / 3 of the mixture of water reducer and water is poured into the stirring pot, wet mixed for 2~3min, and finally the remaining water and water reducer are evenly poured into the stirring pot, and stirred to a slurry with a certain fluidity, and the fluidity is 160~170mm.

[0025] Furthermore, in the step 2, the fibers are added to the mixing pot slowly and evenly, and stirred for about 5 minutes. During the stirring process, the stirring time can be appropriately shortened or increased according to the state of the mixture to ensure that the fibers are evenly dispersed in the concrete.

[0026] Furthermore, the fiber is polyvinyl alcohol fiber PVA.

[0027] Furthermore, the test block in Step 3 is vibrated on a vibration table for 2 minutes at a vibration frequency of 50 Hz until no more bubbles appear on the surface.

[0028] Furthermore, the indoor curing of the specimens in Step 5 adopts a standard curing method, that is, the curing temperature is 20±2° C., the curing humidity is above 95%, and the compressive strength of the specimens after curing is greater than 90 MPa.

[0029] Example 2 In another preferred embodiment, on the basis of the above-mentioned embodiment 1, the mass of each material is weighed according to the designed mix ratio in Step 2, and the specific ratio of P·O52.5 cement, fly ash, silica fume, water, water reducing agent, shale ceramic sand, and PVA fiber in parts by weight is as shown in the following Table 1 Mix Ratio 1: Table 1 Mixing ratio 1 (unit: kg / m 3 )

[0030] The lightweight ultra-high performance concrete prepared by the above mix ratio 1 has a fluidity test of 140 mm, an average compressive strength (28 days) of 3 cubic test blocks of 100.3 MPa, and a thermal conductivity and heat transfer coefficient of 0.726 W / (m·K) and 0.269 W / (m 2 ·K).

[0031] Example 3 In another preferred embodiment, based on the above embodiment 2, the volume content of PVA fiber is changed to 1.5%, and other proportions remain unchanged, as shown in the following Table 2 Mixing Ratio 2: Table 2 Mix ratio 2 (unit: kg / m 3 )

[0032] The lightweight ultra-high performance concrete prepared by the above mix ratio 2 has a fluidity test of 120 mm, an average compressive strength (28 days) of 3 cubic test blocks of 116.3 MPa, and a thermal conductivity and heat transfer coefficient of 0.732 W / (m·K) and 0.270 W / (m 2 ·K).

[0033] Example 4 In another preferred embodiment, based on the above embodiment 1, the volume content of PVA fiber is changed to 2%, and other proportions remain unchanged, as shown in the following Table 3: Table 3 Mixing ratio 3 (unit: kg / m 3 )

[0034] The lightweight ultra-high performance concrete prepared by the above mix ratio 3 has a fluidity test of 110 mm, an average compressive strength (28 days) of 3 cubic test blocks of 105.5 MPa, and a thermal conductivity and heat transfer coefficient of 0.742 W / (m·K) and 0.270 W / (m 2 ·K).

[0035] Example 5 In another preferred embodiment, based on the above embodiment 1, the type of fiber is changed, the PVA fiber is changed to BF (Basalt Fiber) fiber, the fiber volume content is the same as 1%, and other proportions remain unchanged, as shown in the following Table 4 Mixing Ratio 4: Table 4 Mix ratio 4 (unit: kg / m 3 )

[0036] The lightweight ultra-high performance concrete prepared by the above mix ratio 4 has a fluidity test of 130 mm, an average compressive strength (28 days) of 3 cubic test blocks of 95.2 MPa, and a thermal conductivity and heat transfer coefficient of 0.763 W / (m·K) and 0.270 W / (m 2 ·K).

[0037] Example 6 In another preferred embodiment, based on the above embodiment 5, the fiber dosage is changed, and the volume dosage of BF (Basalt Fiber, basalt fiber) fiber is changed to 1.5%, and other proportions remain unchanged, as shown in the following Table 5 Mixing Ratio 5: Table 5 Mixing ratio 5 (unit: kg / m 3 )

[0038] The lightweight ultra-high performance concrete prepared by the above mix ratio 5 has a fluidity test of 125 mm, an average compressive strength (28 days) of 3 cubic test blocks of 100.8 MPa, and a thermal conductivity and heat transfer coefficient of 0.879 W / (m·K) and 0.271 W / (m 2 ·K).

[0039] Example 7 In another preferred embodiment, based on the above embodiment 5, the fiber dosage is changed, and the volume dosage of BF (Basalt Fiber, basalt fiber) fiber is changed to 2%, and other proportions remain unchanged, as shown in the following Table 6 Mixing Ratio 6: Table 6 Mixing ratio 6 (unit: kg / m 3 )

[0040] The lightweight ultra-high performance concrete prepared by the above mix ratio 6 has a fluidity test of 115 mm, an average compressive strength (28 days) of 3 cubic test blocks of 119.8 MPa, and a thermal conductivity and heat transfer coefficient of 0.889 W / (m·K) and 0.271 W / (m 2 ·K).

[0041] Example 8 In another preferred embodiment, based on the above embodiment 5, the type of fiber is changed, and the BF (Basalt Fiber) fiber is changed to glass fiber, and the fiber volume content is also 1%, as shown in the following Table 7 Mixing Ratio 7: Table 7 Mixing ratio 7 (Unit: kg / m 3 )

[0042] The lightweight ultra-high performance concrete prepared by the above mix ratio 7 has a fluidity test of 130 mm, an average compressive strength (28 days) of 3 cubic test blocks of 97.1 MPa, and a thermal conductivity and heat transfer coefficient of 0.892 W / (m·K) and 0.271 W / (m 2 ·K).

[0043] Example 9 In another preferred embodiment, on the basis of the above-mentioned embodiment 8, the fiber dosage is changed, the volume dosage of the glass fiber is changed to 1.5%, and other proportions remain unchanged, as shown in the following table 8: Table 8 Mixing ratio 8 (unit: kg / m 3 )

[0044] The lightweight ultra-high performance concrete prepared by the above mix ratio 8 has a fluidity test of 120 mm, an average compressive strength (28 days) of 3 cubic test blocks of 104.2 MPa, and a thermal conductivity and heat transfer coefficient of 0.897 W / (m·K) and 0.271 W / (m 2 ·K).

[0045] Example 10 In another preferred embodiment, on the basis of the above-mentioned embodiment 8, the fiber dosage is changed, the volume dosage of the glass fiber is changed to 2%, and other proportions remain unchanged, as shown in the following table 9: Table 9 Mixing ratio 9 (Unit: kg / m 3 )

[0046] The lightweight ultra-high performance concrete prepared by the above mix ratio 9 has a fluidity test of 110 mm, an average compressive strength (28 days) of 3 cubic test blocks of 99.5 MPa, and a thermal conductivity and heat transfer coefficient of 0.927 W / (m·K) and 0.271 W / (m 2 ·K).

[0047] The fluidity, compressive strength, thermal conductivity and heat transfer coefficient obtained from the above 9 implementation examples are summarized in Table 10. The specific parameters are shown in Table 10 below.

[0048] Table 10 Parameters in the embodiment

[0049] By comparing Examples 2 to 4, Examples 5 to 7, and Examples 8 to 10, it can be seen that when the same type of fiber is added to concrete as a reinforcing material, the fluidity of the concrete decreases with the increase in the fiber content; at the same volume content, the relationship of the influence of the fiber on the fluidity of the concrete is: BF (Basalt Fiber, basalt fiber) fiber = glass fiber > PVA fiber; as the volume content of the fiber increases, the relationship of the influence on the fluidity of the concrete is: PVA fiber > glass fiber > BF (Basalt Fiber, basalt fiber) fiber.

[0050] From the comparison of Examples 2-4, 5-7, and 8-10, it can be seen that when the same type of fiber is added to concrete as a reinforcing material, for PVA fiber and glass fiber, as the fiber content increases, the concrete strength first increases and then decreases, and the strength reaches a maximum value when the fiber content is 1.5%; for BF (Basalt Fiber, basalt fiber) fiber, the concrete strength increases with the increase of the fiber content, and the concrete strength reaches a maximum value when the content is 2%.

[0051] From the comparison of Examples 2 to 4, Examples 5 to 7, and Examples 8 to 10, it can be seen that when the same type of fiber is added to the concrete as a reinforcing material, the thermal conductivity of the concrete sample increases with the increase in the fiber content; at the same volume content, the influence of the fiber on the thermal conductivity of the concrete sample is as follows: glass fiber>BF (Basalt Fiber, basalt fiber) fiber>PVA fiber; as the volume content of the fiber increases, the influence on the thermal conductivity of the concrete sample is as follows: BF (Basalt Fiber, basalt fiber) fiber>glass fiber>PVA fiber.

[0052] The heat transfer coefficient calculation was carried out by taking the ultra-low energy consumption frame system composed of LUHPC frame (90 mm wide and 20 mm thick) + graphite EPS insulation module (55 mm thick inside and outside) as an example. The heat transfer coefficients calculated in Examples 2 to 10 all meet the requirements of less than 0.3 W / (m 2 ·K) specification requirements, the heat transfer coefficient of concrete mixed with PVA fiber is lower than that of concrete mixed with BF (Basalt Fiber) fiber and glass fiber, and the thermal insulation performance is better.

[0053] According to the above results, considering the working performance, mechanical properties, thermal properties and fiber cost, the LUHPC of mix ratio 2 of Example 3 was selected as the frame-attached mix ratio. From the fluidity, it can be seen that the working performance of this mix ratio is not good. The water-binder ratio was adjusted from 0.18 to 0.20, as shown in the following Table 11 Mix ratio 10.

[0054] Table 11 Mixing ratio 10

[0055] The lightweight ultra-high performance concrete prepared with the adjusted mix ratio has a fluidity test of 165 mm, an average compressive strength (28 days) of 3 cubic test blocks of 90.3 MPa, and thermal conductivity and heat transfer coefficients of 0.810 W / (m·K) and 0.271 W / (m 2 ·K).

[0056] The cost of a 1-meter LUHPC door and window frame (width 90 mm, thickness 20 mm) in the present invention is calculated based on the unit price of the materials. The unit prices of the various materials are shown in Table 12 below.

[0057] Table 12 Material unit price

[0058] Calculated based on the above material unit prices, the construction cost of 1 meter LUHPC is 6.18 yuan.

[0059] In summary, the invention proposes a novel method for preparing ultra-low energy consumption LUHPC for door and window auxiliary frames. The lightweight ultra-high performance concrete prepared by using P·O52.5 cement, ultra-fine fly ash (UFA) and silica fume (SF), artificial lightweight shale ceramics, fiber PVA, water and polycarboxylic acid high-performance water reducing agent can well meet the requirements of energy saving, high strength, good thermal insulation performance and good durability of door and window auxiliary frames. The invention solves the problems of low strength, poor thermal insulation and poor energy-saving and environmental protection effect of existing door and window auxiliary frames, and can effectively improve the energy consumption performance of door and window auxiliary frames and reduce energy consumption. In addition, the preparation method is simple to operate, low in cost and has a wide range of promotion and application prospects. At the same time, the invention also provides a new idea and method for the application of ultra-high performance concrete in the field of energy-saving door and window auxiliary frames. This will make a positive contribution to the sustainable development of our construction industry. While reducing costs, its performance is further improved, so that it can be more widely used in the construction field to achieve green, low-carbon and sustainable development of the construction industry.

Claims

1. A preparation method for a new type of ultra-low energy consumption LUHPC for door and window frames, It is characterized in that The following steps are involved: Step 1: Select the raw materials needed to prepare ultra-low energy consumption, lightweight and ultra-high performance concrete for door and window frames; Step 2: Before preparation, weigh a small amount of materials with the same mix ratio but without fibers, stir and lubricate the pot, weigh the mass of each material according to the designed mix ratio, pour them into the mixer in order, stir until the slurry has a certain fluidity, add fibers and evenly disperse them in the concrete; Step 3: Load the concrete mixture into the mold with release agent in layers, and place the molded test block on the concrete vibration table to vibrate and compact it; Step 4: After the mold is placed, the surface of the specimen is promptly covered with plastic film for water retention and curing, and the specimen is moved into a room at a temperature of 20±2℃ for curing before demolding; Step 5: After the specimen is demoulded, place it in a standard curing box and cure it using standard curing methods.

2. A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 1, Features: The raw materials required for preparing the ultra-low energy consumption, lightweight and ultra-high performance concrete for the door and window frames in the Step 1 are P·O52.5 cement, silica fume, fly ash, shale ceramic sand, fiber, water and water reducing agent. The shale ceramic sand is artificial lightweight shale ceramic sand. The designed mix proportions are 35% to 40% by mass of P·O52.5 cement, 10% to 15% by mass of fly ash, 8% to 10% by mass of silica fume, 8% to 14% by mass of water reducing agent, 1% to 3% by mass of ceramic sand, 25% to 35% by mass of ceramic sand and 0.5% to 2% by mass of fiber.

3. A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 2, Features: In the step 2, the order in which the materials are poured into the mixer is the cementitious material, the shale sand, the mixture of water and the water reducing agent, and the fiber.

4. The preparation method of a novel ultra-low energy consumption LUHPC for door and window frames according to claim 3, Features: The cementitious materials are P·O52.5 cement, silica fume and fly ash.

5. A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 4, Features: The particle size range of the shale ceramic sand is 0-3 mm, and the water reducer used is a polycarboxylic acid water reducer.

6. A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 5, Features: In the Step 2, the mass of each material is weighed according to the designed mix ratio, poured into the mixer in order, and stirred to a slurry with a certain fluidity, that is, P·O52.5 cement, silica fume, fly ash and shale sand are added to the mixing pot for dry mixing, and then 2 / 3 of the mixture of water reducer and water is poured into the mixing pot for wet mixing, and finally the remaining water and water reducer are evenly poured into the mixing pot, and stirred to a slurry with a certain fluidity.

7. A method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 6, Features: The fibers are added in Step 2 by slowly and evenly adding the fibers into a mixing pot and stirring. During the stirring process, the stirring time can be appropriately shortened or increased according to the state of the mixture to ensure that the fibers are evenly dispersed in the concrete.

8. The method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 7, Features: The fiber is polyvinyl alcohol fiber PVA.

9. The method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 1, Features: The test block in Step 3 is vibrated on a vibration table at a frequency of 50 Hz until no more bubbles appear on the surface.

10. The method for preparing a novel ultra-low energy consumption LUHPC for door and window frames according to claim 1, Features: The indoor curing of the specimens in Step 5 adopts a standard curing method, that is, the curing temperature is 20±2°C, the curing humidity is above 95%, and the compressive strength of the specimens after curing is greater than 90MPa.