Carbon-based porous material suitable for capturing carbon dioxide by electrochemical method, and preparation method and application of carbon-based porous material

By using nitrogen-doped carbon-based porous materials prepared by high-temperature treatment as catalysts in electrochemical method, the problem of low catalyst activity in electrochemical mediated amine regeneration capture technology is solved, and the capture efficiency and electrochemical performance of carbon dioxide are improved , reduces energy consumption.

CN118993031AActive Publication Date: 2024-11-22HUANENG CLEAN ENERGY RES INST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411302311.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-22
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

The existing electrochemically mediated amine regeneration capture technology has low catalyst activity under high current density conditions, resulting in large energy consumption and affecting the carbon dioxide capture efficiency.

Method used

The nitrogen-doped carbon-based porous materials were prepared by pyrolysis treatment in a high-temperature tube furnace. It was used as a catalyst for electrochemical carbon dioxide capture. The one-step synthesis of nitrogen-doped carbon materials was achieved through in-situ synthesis, which improved the Specific surface area and adsorption capacity of the material.

Benefits of technology

The adsorption capacity and electrochemical performance of carbon-based porous materials are improved, the capture efficiency of carbon dioxide is enhanced, the energy consumption under high current density is reduced, and the efficient electrochemical carbon dioxide capture is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993031A_ABST
    Figure CN118993031A_ABST
Patent Text Reader

Abstract

The invention provides a carbon-based porous material suitable for carbon dioxide capture by an electrochemical method, and a preparation method and application thereof, and belongs to the technical field of electrochemistry. The preparation method comprises the following steps: putting urea powder into a high-temperature tubular furnace, and introducing nitrogen to treat for 0.5-1.5 hours; the preparation method comprises the following steps: carrying out pyrolysis treatment on urea powder in an argon atmosphere at a preset temperature for 0.5-1.5 h, cooling, and grinding to obtain the nitrogen-doped carbon-based porous material. An in-situ synthesis method is adopted, urea serves as a nitrogen source precursor and a carbon source precursor at the same time in the preparation process, high-temperature treatment is conducted in an inert environment, and therefore one-step synthesis of the nitrogen-doped carbon material is achieved, and the material has the large specific surface area so as to be high in adsorption capacity and can effectively adsorb carbon dioxide gas molecules to the surface; the performance and the application range of the carbon material in the aspects of catalysis, adsorption, electrochemistry and the like are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure belongs to the field of electrochemical technology, and specifically relates to a carbon-based porous material suitable for electrochemical carbon dioxide capture, a preparation method, and an application thereof. Background Art

[0002] Under the background of "dual carbon", one of the directions of carbon neutral transformation for industries that are difficult to decarbonize, such as steel mills, cement plants and chemical plants, is electrification. The traditional chemical absorption carbon capture method uses low-grade heat to steam desorb carbon dioxide under high temperature (120-150°C). This technology is highly mature and widely used, but it also faces the problems of high solvent heat loss, affecting the low-load operation depth and peak-shaving flexibility of power plants, and higher application costs in heavy industries without residual heat sources.

[0003] In contrast, the electrochemical mediated amine regeneration capture technology is to introduce electrolytes and electrode materials that have strong adsorption effects on absorbents, and then release carbon dioxide through an electrochemical process to achieve rich liquid regeneration. Although this technology can be plug-and-play through pure electric drive, which greatly reduces operating costs, it is more suitable for peak-shaving power plants, power plants in coastal areas with high steam prices, and heavy industries with highly integrated energy. However, the catalyst activity currently used in this method is low, and the energy consumption is large under high current density conditions, which in turn affects the capture efficiency of electrochemical carbon dioxide. Summary of the invention

[0004] The present disclosure aims to solve at least one of the technical problems existing in the prior art and to provide a carbon-based porous material suitable for electrochemical carbon dioxide capture and a preparation method and application thereof.

[0005] In one aspect of the present disclosure, a method for preparing a carbon-based porous material suitable for electrochemical carbon dioxide capture is provided, the preparation method comprising:

[0006] Place urea powder in a high-temperature tube furnace and introduce nitrogen for 0.5 to 1.5 hours;

[0007] The urea powder is pyrolyzed in an argon atmosphere at a preset temperature for 0.5 to 1.5 hours, and then cooled and ground to obtain a nitrogen-doped carbon-based porous material.

[0008] Optionally, the preset temperature is 750-850°C.

[0009] Optionally, the content of the urea powder is 5 to 15 parts by mass.

[0010] In another aspect of the present disclosure, a carbon-based porous material suitable for electrochemical carbon dioxide capture is provided, which is prepared by the preparation method described above.

[0011] Optionally, the carbon-based porous material has a three-dimensional structure of spherically stacked structures.

[0012] Optionally, the size of the carbon-based porous material is 20 nm to 5 μm.

[0013] Another aspect of the present disclosure provides an application of a carbon-based porous material, wherein the carbon-based porous material described above is used as a catalyst in electrochemical carbon dioxide capture.

[0014] Optionally, the application process includes:

[0015] The carbon-based porous material described above is added to a mixed solution of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution, and subjected to ultrasonic treatment to form a mixed suspension;

[0016] The mixed suspension is dropped onto the surface of the electrode substrate to obtain the electrode material.

[0017] Optionally, the volume ratio of the tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution is (8-9):(9-10):1.

[0018] Optionally, the solid-liquid ratio of the carbon-based porous material to the perfluorosulfonic acid resin solution is 1:(9-10) mg / μL.

[0019] The present disclosure proposes a carbon-based porous material suitable for electrochemical carbon dioxide capture and a preparation method and application. Among them, the preparation method of the carbon-based porous material suitable for electrochemical carbon dioxide capture includes: placing urea powder in a high-temperature tubular furnace, introducing nitrogen for treatment for 0.5 to 1.5 hours; pyrolyzing the urea powder in an argon atmosphere at a preset temperature for 0.5 to 1.5 hours, and then cooling and grinding to obtain a nitrogen-doped carbon-based porous material. The present disclosure adopts an in-situ synthesis method to use urea as both a nitrogen source and a carbon source precursor during the preparation process, and performs high-temperature treatment under an inert environment, thereby realizing a one-step synthesis of nitrogen-doped carbon materials. The material has a large specific surface area and thus a strong adsorption capacity, and can effectively adsorb carbon dioxide gas molecules to the surface, effectively improving the performance and use range of carbon materials in catalysis, adsorption, electrochemistry, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flowchart of a method for preparing a carbon-based porous material suitable for electrochemical carbon dioxide capture according to an embodiment of the present disclosure;

[0021] Figure 2 A flowchart of forming an electrode material from a carbon-based porous material according to another embodiment of the present disclosure;

[0022] Figure 3(A) and (B) are scanning electron microscope images of the carbon-based porous material of Example 1 of the present disclosure;

[0023] Figure 4 It is the average current density result of Example 1 of the present disclosure. DETAILED DESCRIPTION

[0024] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.

[0025] like Figure 1 As shown, in one aspect of the present disclosure, a method S100 for preparing a carbon-based porous material suitable for electrochemical carbon dioxide capture is provided, comprising steps S110-

[0026] S120:

[0027] S110, placing urea powder in a high temperature tube furnace, introducing nitrogen gas for treatment at 0.5~

[0028] 1.5h.

[0029] Specifically, 5 to 15 parts by mass of urea powder are weighed and evenly placed in a crucible, and then the crucible containing the urea powder is placed in the heat source center of a high-temperature tube furnace. Argon is introduced at a flow rate of 20 sccm, and nitrogen is introduced in advance for 0.5 to 1.5 h to remove the air in the furnace to complete the pyrolysis preparation for the next step.

[0030] In some preferred embodiments, the content of urea powder is 5g, 8g, 10g, 13g, 15g, etc. Of course, urea powder with other contents can also be selected according to actual needs.

[0031] In other preferred embodiments, the time for introducing nitrogen is 0.5 h, 1 h, or 1.5 h.

[0032] S120, pyrolyzing the urea powder in an argon atmosphere at a preset temperature for 0.5 to 1.5 hours, and then cooling and grinding the powder to obtain a nitrogen-doped carbon-based porous material.

[0033] Specifically, argon gas was continuously introduced into the high-temperature tube furnace at a flow rate of 20 sccm, and the heating program was set as follows: heating to 750-850°C at a rate of 5°C / min, constant temperature treatment was performed under this temperature condition for 0.5-1.5h, naturally cooled to room temperature, ground and bottled for standby use, and named as NC material.

[0034] In some preferred embodiments, the temperature is raised to a preset temperature, preferably 750°C, 780°C, 800°C, 820°C, or 850°C.

[0035] In other preferred embodiments, the constant temperature treatment time is preferably 0.5h, 1h, or 1.5h.

[0036] In this embodiment, through the in-situ synthesis method, urea is used as both a nitrogen source and a carbon source precursor during the preparation process, and is subjected to high temperature treatment under an inert environment, thereby achieving a one-step synthesis of nitrogen-doped carbon materials, and the synthesis process is simple.

[0037] It should be understood that the carbon-based porous material synthesized in this embodiment has a large specific surface area and thus has a strong adsorption capacity, and can effectively adsorb carbon dioxide gas molecules to the surface. Secondly, nitrogen doping can enhance the surface polarity of the carbon material, improve the surface wettability, and modify the electronic properties of the surface, thereby improving the performance and application range of the carbon material in catalysis, adsorption, electrochemistry, etc.

[0038] In another aspect of the present disclosure, a carbon-based porous material suitable for electrochemical carbon dioxide capture is provided, which is prepared by the preparation method described above. For the specific preparation process, please refer to the above description and will not be repeated here.

[0039] The carbon-based porous material obtained in this embodiment has a three-dimensional structure of spherical stacking, and its diameter ranges from tens of nanometers to several micrometers.

[0040] In some preferred embodiments, the size of the carbon-based porous material is 20 nm to 5 μm.

[0041] In this embodiment, the three-dimensional carbon-based porous material can provide a larger electrochemical surface area and more chemically active sites, thereby improving the performance of electrochemical carbon dioxide capture.

[0042] Another aspect of the present disclosure provides an application of a carbon-based porous material, wherein the carbon-based porous material described above is used as a catalyst in electrochemical carbon dioxide capture.

[0043] It should be noted that in this embodiment, the carbon-based porous material is coated on the electrode surface as a catalyst, and carbon dioxide is adsorbed based on its large specific surface area and a large number of active sites, such as Figure 2 As shown, the application process S200 includes the following steps S210 to S220:

[0044] S210, adding the carbon-based porous material described above to a mixed solution of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution, and performing ultrasonic treatment to form a mixed suspension.

[0045] In some preferred embodiments, the solid-to-liquid ratio of the carbon-based porous material to the perfluorosulfonic acid resin is 1:(9-10) mg / μL.

[0046] As a further preferred embodiment, the content of the carbon-based porous material is preferably 3 to 8 mg, for example, 3 mg, 4 mg, 5 mg, 6 mg, 8 mg, and correspondingly, the volume of the perfluorosulfonic acid resin solution is preferably 30 to 80 μL.

[0047] As a further preferred embodiment, the content of the carbon-based porous material is preferably 5 mg, and correspondingly, the volume of the perfluorosulfonic acid resin is preferably 50 μL.

[0048] In other preferred embodiments, the volume ratio of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution is (8-9):(9-10):1.

[0049] As a further preferred embodiment, the volumes of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution are 240-720 μL, 270-800 μL and 30-80 μL respectively.

[0050] As a further preferred embodiment, the volumes of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution are preferably 400-500 μL, 450-550 μL and 40-60 μL, respectively.

[0051] As a further preferred solution, when the volume of the perfluorosulfonic acid resin solution is preferably 50 μL, the volumes of tetrahydrofuran and 2-propanol may be preferably 450 μL and 500 μL. Of course, in other embodiments, these components may also be added in other volumes, which are not specifically limited.

[0052] It should be noted that the perfluorosulfonic acid resin solution may be a Nafion perfluorinated resin solution with a concentration of 5 wt %, which can further improve the carbon dioxide capture capability.

[0053] It should be further explained that, in step S210, the time of ultrasonic treatment is not specifically limited, as long as the mixed solution can be mixed evenly, for example, 20-40 minutes.

[0054] In other preferred embodiments, ultrasonic treatment is performed for 30 minutes to uniformly mix the components to form a mixed suspension solution.

[0055] S220, dropping the mixed suspension onto the surface of the electrode substrate to obtain an electrode material.

[0056] It should be noted that the present embodiment does not specifically limit the type of the electrode substrate, for example, carbon paper, carbon cloth, carbon felt, etc.

[0057] In some preferred embodiments, the carbon paper may preferably be AvCarb MGL190, MGL370, MGL280, and the like.

[0058] It should be further noted that the present embodiment does not specifically limit the size of the electrode substrate, for example, 1×1 cm 2 Of course, for those skilled in the art, materials such as carbon paper of other sizes can also be provided.

[0059] It should be understood that when the prepared electrode material is applied to electrochemical carbon dioxide capture, in the electrochemical carbon dioxide capture experiment, ethylenediamine solution is used as the electrolyte, the carbon-based porous material on the surface of the electrode material is used as the catalyst, and the average current density is 2.5 mA / cm 2 , achieving efficient electrochemical carbon dioxide capture.

[0060] In this embodiment, when ethylenediamine is used as the electrolyte, it has two capture points (—NH2), so that it can have a higher carbon capture efficiency and further synergize with the carbon-based porous material to increase the carbon capture efficiency.

[0061] The preparation method and application of carbon-based porous materials will be further explained below in conjunction with several specific examples:

[0062] Example 1

[0063] The method for preparing the carbon-based porous material in this example includes the following steps:

[0064] S1. Weigh 10g of urea powder and place it evenly in a crucible, which is then placed at the heat source center of a high-temperature tube furnace. Argon is introduced at a flow rate of 20sccm for 1 hour in advance to remove air from the furnace.

[0065] S2. Continuously introduce argon gas into the high-temperature tube furnace at a flow rate of 20 sccm, set the heating program as follows: increase the temperature to 800°C at a rate of 5°C / min, maintain a constant temperature at 800°C for 1 hour, and naturally cool to room temperature to obtain a carbon-based porous material.

[0066] like Figure 3 As shown, the carbon-based porous material obtained in Example 1 presents a three-dimensional structure, and the formed spherical structures are stacked to increase its specific surface area.

[0067] Furthermore, the obtained carbon-based porous material is coated on the surface of the electrode, comprising:

[0068] S3, 5 mg of the prepared carbon-based porous material was added to 450 μL of tetrahydrofuran, 500 μL of 2-propanol and 50 μL of a 5 wt% Nafion perfluororesin mixed solution, and a uniform mixed suspension solution was formed after ultrasonication for 30 minutes. Then, the suspension solution was added dropwise onto AvCarb MGL370 carbon paper (1×1 cm 2 ) surface, thereby preparing the electrode material.

[0069] Furthermore, if Figure 4 As shown in Figure 2, in the electrochemical carbon dioxide capture using carbon-based porous materials as catalysts, the average current density is 2.5 mA / cm 2 , achieving low-energy digestion at high current density, thereby realizing efficient electrochemical carbon dioxide capture.

[0070] Example 2

[0071] The method for preparing the carbon-based porous material in this example includes the following steps:

[0072] S1. Weigh 5 g of urea powder and place it evenly in a crucible, which is then placed at the heat source center of a high-temperature tube furnace. Argon is introduced at a flow rate of 20 sccm for 1 hour in advance to remove air from the furnace.

[0073] S2. Continuously introduce argon gas into the high-temperature tube furnace at a flow rate of 20 sccm, set the heating program as follows: increase the temperature to 850°C at a rate of 5°C / min, maintain a constant temperature at 850°C for 0.5h, and naturally cool to room temperature to obtain a carbon-based porous material.

[0074] The carbon-based porous material obtained in Example 2 also presents a three-dimensional structure, and the formed spherical structures are stacked to increase their specific surface area.

[0075] Furthermore, the obtained carbon-based porous material is coated on the surface of the electrode, comprising:

[0076] S3, 3 mg of the prepared carbon-based porous material was added to 400 μL of tetrahydrofuran, 450 μL of 2-propanol and 40 μL of a 5 wt% Nafion perfluororesin mixed solution, and a uniform mixed suspension solution was formed after ultrasonication for 30 minutes. Then, the suspension solution was added dropwise onto AvCarb MGL370 carbon paper (1×1 cm 2 ) surface, thereby preparing the electrode material.

[0077] Furthermore, in the electrochemical carbon dioxide capture using carbon-based porous materials as catalysts, the average current density was 2.2 mA / cm 2 , achieving low-energy digestion at high current density, thereby realizing efficient electrochemical carbon dioxide capture.

[0078] Example 3

[0079] The method for preparing the carbon-based porous material in this example includes the following steps:

[0080] S1. Weigh 15g of urea powder and place it evenly in a crucible, which is then placed at the heat source center of a high-temperature tube furnace. Argon is introduced at a flow rate of 20sccm for 1 hour in advance to remove air from the furnace.

[0081] S2. Continuously introduce argon gas into the high-temperature tube furnace at a flow rate of 20 sccm, set the heating program as follows: increase the temperature to 750°C at a rate of 5°C / min, maintain a constant temperature at 750°C for 1.5 hours, and naturally cool to room temperature to obtain a carbon-based porous material.

[0082] The carbon-based porous material obtained in Example 3 also presents a three-dimensional structure, and the formed spherical structures are stacked to increase their specific surface area.

[0083] Furthermore, the obtained carbon-based porous material is coated on the surface of the electrode, comprising:

[0084] S3, 8 mg of the prepared carbon-based porous material was added to 550 μL of tetrahydrofuran, 650 μL of 2-propanol and 60 μL of a 5 wt% Nafion perfluororesin mixed solution, and a uniform mixed suspension solution was formed after ultrasonication for 30 minutes. Then, the suspension solution was added dropwise onto AvCarb MGL370 carbon paper (1×1 cm 2 ) surface, thereby preparing the electrode material.

[0085] Furthermore, in the electrochemical carbon dioxide capture using carbon-based porous materials as catalysts, the average current density was 2.4 mA / cm 2 , achieving low-energy digestion at high current density, thereby realizing efficient electrochemical carbon dioxide capture.

[0086] Comparative Example 1

[0087] The electrode material forming process of this example includes the following specific steps:

[0088] 400 μL of tetrahydrofuran, 450 μL of 2-propanol and 40 μL of 5 wt% Nafion perfluororesin mixed solution were ultrasonicated for 30 minutes to form a uniform mixed suspension solution. Then, the suspension solution was added dropwise onto AvCarb MGL370 carbon paper (1×1 cm 2 ) surface, thereby preparing the electrode material.

[0089] Furthermore, in electrochemical CO2 capture, the average current density was 0.9 mA / cm 2 , the current density is low and the energy consumption is large, thereby reducing the capture efficiency of carbon dioxide.

[0090] In summary, it can be seen from the results of Examples 1-3 and Comparative Example 1 that in the electrochemical carbon dioxide capture without the addition of carbon-based porous materials, the current density is low, the energy consumption is large, and the capture efficiency is low. This shows that the carbon-based porous material of this embodiment is used for electrochemical carbon dioxide capture, which can effectively improve the capture efficiency of carbon dioxide.

[0091] The present disclosure provides a carbon-based porous material for electrochemical carbon dioxide capture and a preparation method and application thereof, which has the following beneficial effects:

[0092] First, the present disclosure adopts an in-situ synthesis method, in which urea is used as both a nitrogen source and a carbon source precursor during the preparation process, and is subjected to high-temperature treatment under an inert environment, thereby achieving a one-step synthesis of nitrogen-doped carbon materials. The process is simple and easy to operate, and the components of the required precursors are simple.

[0093] Second, the carbon-based porous material disclosed in the present invention has a large specific surface area, and thus has a strong adsorption capacity, and can effectively adsorb carbon dioxide gas molecules to the surface, thereby improving the ability to capture carbon dioxide. At the same time, the material is doped with nitrogen, which can enhance the surface polarity of the carbon material, improve the surface wettability, and modify the electronic results of the surface, thereby improving the performance and application range of the carbon material in catalysis, adsorption, electrochemistry, etc.

[0094] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. A method for preparing a carbon-based porous material suitable for electrochemical carbon dioxide capture, characterized in that: The preparation method comprises: Place urea powder in a high-temperature tube furnace and introduce nitrogen for 0.5 to 1.5 hours; The urea powder is pyrolyzed in an argon atmosphere at a preset temperature for 0.5 to 1.5 hours, and then cooled and ground to obtain a nitrogen-doped carbon-based porous material.

2. The preparation method according to claim 1, characterized in that: The preset temperature is 750-850°C.

3. The preparation method according to claim 1, characterized in that: The content of the urea powder is 5 to 15 parts by mass.

4. A carbon-based porous material suitable for electrochemical carbon dioxide capture, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 3.

5. The carbon-based porous material according to claim 4, characterized in that: The carbon-based porous material presents a three-dimensional structure of spherical stacking.

6. The carbon-based porous material according to claim 4, characterized in that: The size of the carbon-based porous material is 20 nm to 5 μm.

7. An application of a carbon-based porous material, characterized in that: The carbon-based porous material according to any one of claims 4 to 6 is used as a catalyst in electrochemical carbon dioxide capture.

8. The use according to claim 7, characterized in that: The application process includes: Adding the carbon-based porous material to a mixed solution of tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution, and ultrasonically treating the mixture to form a mixed suspension; The mixed suspension is dropped onto the surface of the electrode substrate to obtain the electrode material.

9. The use according to claim 8, characterized in that: The volume ratio of the tetrahydrofuran, 2-propanol and perfluorosulfonic acid resin solution is (8-9):(9-10):

1.

10. The use according to claim 8, characterized in that: The solid-to-liquid ratio of the carbon-based porous material to the perfluorosulfonic acid resin solution is 1:(9-10) mg / μL.

Citation Information

Patent Citations

  • A method for preparing an in-situ nitrogen-doped carbon-coated lithium iron phosphate- cathode material

    CN109244395A

  • Preparation method of multipurpose oxygen-nitrogen co-doped waste biomass derived carbon material

    CN111153402A

  • Method for preparing non-layered two-dimensional transition metal compound by using bulk phase layered transition metal sulfide

    CN113479855A

  • Collecting and utilizing integrated system and method for treating carbon dioxide in industrial tail gas

    CN114522525A

  • Catalyst electroode, method for manufacturing the catalyst electrode, eletrochemical reactor comprising the same and system for reduction of carbon dioxide

    KR102409746B1