Preparation method and application of spherical ytterbium silicate spraying powder

Directly sintering Yb2O3 and SiO2 powders through spray drying technology, solving the existing cumbersome processes and impurities problems, improving the purity and production efficiency of sprayed powders with ytterbium silicate, suitable for high-temperature thermal barrier coating materials, meeting the high-temperature environment high efficiency coating material requirements.

CN118993093APending Publication Date: 2024-11-22中稀金龙(长汀)稀土有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410994490.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the process of preparing ytterbium silicate spray powder is cumbersome and easy to introduce impurities, resulting in low yields of finished products and unable to effectively meet the needs of high-efficiency coating materials in high temperature environments.

Method used

The Yb2O3 and SiO2 powder mixture is directly agglomerated and sintered by spray drying technology, eliminating the ball milling and drying steps. By adjusting the slurry pH and controlling the spray granulation conditions, a high-purity spherical ytterbium silicate spray powder is prepared.

Benefits of technology

The purity and production efficiency of the product are improved and the preparation steps are reduced. The obtained spherical ytterbium silicate spray powder is suitable for use in high-temperature thermal barrier coating materials, with higher stability and corrosion resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method and application of spherical ytterbium silicate spraying powder, and the preparation method comprises the following steps: (1) adding high-purity water and polyvinyl alcohol into Yb2O3 powder and SiO2 powder, stirring, and adjusting the pH value of slurry to 11-12 by using ammonia water; and (2) preparing agglomerated powder from the material obtained in the step (1) by using spray drying equipment. And (3) heating the agglomerated powder obtained in the step (2) to 1450-1550 DEG C in an air furnace, preserving heat for 3-6 hours, and then cooling to room temperature along with the furnace to obtain the spherical ytterbium silicate spraying powder. According to the preparation method, the materials are directly mixed through spray granulation, the steps of ball-milling mixing and drying in the early stage are omitted, and the mixture obtained after spray granulation is directly sintered into a phase, so that organic impurities can be fully removed, and the product purity is improved; and agglomeration sintering and phase synthesis are combined, so that the preparation steps are reduced, and the production efficiency is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth functional materials, and specifically relates to a preparation method and application of spherical ytterbium silicate spray powder. Background Art

[0002] Aircraft engines are the core of the modern aviation industry. After more than a hundred years of development, they have become mature products with extremely high reliability. With the advancement of technology, contemporary aircraft engines are developing towards high thrust-to-weight ratio, high bypass ratio and high thermal efficiency. In order to meet the current development needs, the surface temperature of the hot end components of the new generation of aircraft engines can reach 1400℃. However, the lag in the development of high-temperature structural materials has limited the further improvement of engine efficiency.

[0003] At present, silicon carbide composite materials are gradually replacing traditional nickel-based alloys due to their advantages such as high temperature resistance and high strength, and are used in the hot end components of high thrust-to-weight ratio aircraft engines. However, a large amount of water vapor generated during the combustion of aviation fuel will react with silicon carbide, causing continuous corrosion of silicon carbide ceramics, thereby sharply reducing its performance. In order to improve the stability and life of the silicon carbide ceramic matrix in the service environment, it is necessary to coat its surface with environmental barrier coatings (EBC) to isolate corrosive gases and enhance the oxidation resistance and erosion resistance of the hot end components.

[0004] Currently, the most widely used thermal barrier coating material is BSAS (Ba1-xSrxAl2Si2O8), which can work safely for a long time below 1300℃. However, in order to pursue higher operating temperatures (>1400℃), a new generation of thermal barrier coating materials needs to be developed. Rare earth silicates are considered to be the most likely materials to replace BSAS due to their excellent properties such as high melting point, low thermal conductivity and corrosion resistance. In particular, yttrium silicate, ytterbium silicate and lutetium silicate, these three materials have good high temperature phase stability and excellent thermodynamic properties, and are the best candidate materials.

[0005] CN109837496A discloses a method for preparing ytterbium silicate (Yb2SiO5) plasma spray powder. The method involves mixing commercially available Yb2O3 and SiO2 powders and then ball milling them, synthesizing Yb2SiO5 by solid phase reaction, and then preparing Yb2SiO5 agglomerated powder by spray drying, and then screening the particle size to obtain plasma spray powder with a particle size range of 10 to 35 μm. The process includes the steps of mixing and ball milling of raw materials, drying, solid phase synthesis, screening, ball milling slurry preparation, spray granulation and re-screening. The process is relatively cumbersome and easy to introduce impurities, resulting in low yield of finished products. Summary of the invention

[0006] The present invention aims to overcome the defects of the prior art and provide a method for preparing spherical ytterbium silicate spray powder.

[0007] Another object of the present invention is to provide an application of the spherical ytterbium silicate spray powder prepared by the above preparation method.

[0008] The technical solution of the present invention is as follows:

[0009] A method for preparing spherical ytterbium silicate spray powder comprises the following steps:

[0010] (1) Weigh Yb2O3 powder with a D50 of 2.0-2.8 μm and a D90 of 5.1-6.4 μm and SiO2 powder with a D50 of 2.0-2.6 μm and a D90 of 6.0-6.8 μm in a molar ratio of 1.05-2.05:1, add high-purity water and polyvinyl alcohol, stir for 0.8-1.2 h, and adjust the pH of the slurry to 11-12 with aqueous ammonia.

[0011] (2) using a spray drying device to prepare agglomerated powder from the material obtained in step (1), wherein the atomizer speed is 18000-23000 r / min, the inlet temperature of the high-temperature dry air is controlled at 170-220° C., and the outlet temperature is controlled at 90-120° C.

[0012] (3) The agglomerated powder obtained in step (2) is heated to 1450-1550° C. in an air furnace for 3-6 hours, and then cooled to room temperature in the furnace to obtain a spherical ytterbium silicate spray powder mainly in the Yb2SiO5 phase or the Yb2Si2O7 phase.

[0013] In a preferred embodiment of the present invention, the purity standard of the Yb2O3 powder is 4N or 5N.

[0014] In a preferred embodiment of the present invention, the SiO2 powder is analytically pure.

[0015] In a preferred embodiment of the present invention, the polyvinyl alcohol is PVA1788.

[0016] In a preferred embodiment of the present invention, the purity standard of the Yb2O3 powder is 4N or 5N, the SiO2 powder is analytically pure, and the polyvinyl alcohol is PVA1788.

[0017] In a preferred embodiment of the present invention, in step (1), the mass of the high-purity water is 80-200% of the total mass of the Yb2O3 powder and the SiO2 powder.

[0018] Further preferably, in step (1), the mass of the polyvinyl alcohol is 2-5% of the total mass of the Yb2O3 powder and the SiO2 powder.

[0019] In a preferred embodiment of the present invention, the heating rate in step (3) is 5-10°C / min.

[0020] Application of the spherical ytterbium silicate spray powder prepared by the above preparation method in the preparation of thermal barrier coating materials.

[0021] A thermal barrier coating material, the raw material of which includes spherical ytterbium silicate spray powder obtained by the above preparation method.

[0022] The beneficial effects of the present invention are:

[0023] 1. The present invention directly mixes materials by spray granulation, thereby eliminating the previous ball milling mixing and drying steps, and directly sintering the mixture obtained after spray granulation into a phase, which can fully remove organic impurities, thereby improving product purity.

[0024] 2. The present invention combines agglomeration and sintering with physical synthesis, which reduces the preparation steps and effectively improves production efficiency. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0026] Embodiment 1:

[0027] (1) Weigh 4N Yb2O3 with a D50 of 2.3 μm and a D90 of 5.3 μm and analytically pure SiO2 with a D50 of 2.1 μm and a D90 of 6.3 μm (500 g in total) in a molar ratio of 1.05:1, add 500 g of high-purity water and 15 g of binder polyvinyl alcohol (PVA1788), stir for 1 h, and adjust the pH of the slurry to 11 with 25 wt% ammonia water.

[0028] (2) The material obtained in step (1) is used to prepare agglomerated powder by using a spray drying device, wherein the atomizer speed is 21000 r / min, the inlet temperature of the high-temperature dry air is controlled at 175° C., and the outlet temperature is controlled at 90° C.

[0029] (3) The agglomerated powder obtained in step (2) is placed in a crucible, heated to 1500° C. at a heating rate of 5° C. / min in an air furnace and kept at that temperature for 3 h, and then cooled to room temperature in the furnace to obtain spherical ytterbium silicate spray powder.

[0030] The spherical ytterbium silicate spray powder prepared in this embodiment is mainly Yb2SiO5 phase through X-ray diffraction analysis, and the purity is 99.98%. The powder is screened by particle size to obtain powder suitable for plasma spraying with a particle size range of 17-53 μm.

[0031] Embodiment 2:

[0032] (1) Weigh 4N Yb2O3 with a D50 of 2.5 μm and a D90 of 5.9 μm and analytically pure SiO2 with a D50 of 2.0 μm and a D90 of 6.0 μm (500 g in total) in a molar ratio of 1.05:1, add 800 g of high-purity water and 18 g of binder polyvinyl alcohol (PVA1788), stir for 1 h, and adjust the pH of the slurry to 11 with 25 wt% ammonia water.

[0033] (2) The material obtained in step (1) is used to prepare agglomerated powder by using a spray drying device, wherein the atomizer speed is 18000 r / min, the inlet temperature of the high-temperature dry air is controlled at 185° C., and the outlet temperature is controlled at 100° C.

[0034] (3) The agglomerated powder obtained in step (2) is placed in a crucible, heated to 1500° C. at a heating rate of 5° C. / min in an air furnace and kept at this temperature for 3.5 h, and then cooled to room temperature in the furnace to obtain spherical ytterbium silicate spray powder.

[0035] The spherical ytterbium silicate spray powder prepared in this embodiment is mainly Yb2SiO5 phase through X-ray diffraction analysis, and the purity is 99.96%. The powder is screened by particle size to obtain powder suitable for plasma spraying with a particle size range of 17-53 μm.

[0036] Embodiment 3:

[0037] (1) Weigh 4N Yb2O3 with a D50 of 2.8 μm and a D90 of 6.4 μm and analytically pure SiO2 with a D50 of 2.6 μm and a D90 of 6.8 μm (500 g in total) in a molar ratio of 1.05:1, add 1000 g of high-purity water and 25 g of binder polyvinyl alcohol (PVA1788), stir for 1 h, and adjust the pH of the slurry to 12 with 25 wt% ammonia water.

[0038] (2) The material obtained in step (1) is used to prepare agglomerated powder by using a spray drying device, wherein the atomizer speed is 23000 r / min, the inlet temperature of the high-temperature dry air is controlled at 205° C., and the outlet temperature is controlled at 110° C.

[0039] (3) The agglomerated powder obtained in step (2) is placed in a crucible, heated to 1500° C. at a heating rate of 5° C. / min in an air furnace and kept at that temperature for 5 h, and then cooled to room temperature in the furnace to obtain spherical ytterbium silicate spray powder.

[0040] The spherical ytterbium silicate spray powder prepared in this embodiment is mainly Yb2SiO5 phase through X-ray diffraction analysis, and the purity is 99.97%. The powder is screened by particle size to obtain powder suitable for plasma spraying with a particle size range of 17-53 μm.

[0041] Embodiment 4:

[0042] (1) 5N Yb2O3 with a D50 of 2.5 μm and a D90 of 5.7 μm and analytically pure SiO2 with a D50 of 2.5 μm and a D90 of 6.7 μm were weighed in a molar ratio of 1.05:1 (500 g in total), 600 g of high-purity water and 12 g of binder polyvinyl alcohol (PVA1788) were added, and the mixture was stirred for 1 h, and the pH of the slurry was adjusted to 11 with 25 wt% ammonia water.

[0043] (2) The material obtained in step (1) is used to prepare agglomerated powder by using a spray drying device, wherein the atomizer speed is 22000 r / min, the inlet temperature of the high-temperature dry air is controlled at 195° C., and the outlet temperature is controlled at 105° C.

[0044] (3) The agglomerated powder obtained in step (2) is placed in a crucible, heated to 1500° C. at a heating rate of 5° C. / min in an air furnace and kept at that temperature for 6 h, and then cooled to room temperature in the furnace to obtain spherical ytterbium silicate spray powder.

[0045] The spherical ytterbium silicate spray powder prepared in this embodiment is mainly Yb2SiO5 phase through X-ray diffraction analysis, and the purity is 99.95%. The powder is screened by particle size to obtain powder suitable for plasma spraying with a particle size range of 17-53 μm.

[0046] Embodiment 5:

[0047] (1) 5N Yb2O3 with a D50 of 2.0 μm and a D90 of 5.1 μm and analytically pure SiO2 with a D50 of 2.0 μm and a D90 of 6.0 μm were weighed in a molar ratio of 2.05:1 (500 g in total), 800 g of high-purity water and 20 g of binder polyvinyl alcohol (PVA1788) were added, and the mixture was stirred for 1 h, and the pH of the slurry was adjusted to 12 with 25 wt% ammonia water.

[0048] (2) The material obtained in step (1) is used to prepare agglomerated powder by using a spray drying device, wherein the atomizer speed is 22000 r / min, the inlet temperature of the high-temperature dry air is controlled at 220° C., and the outlet temperature is controlled at 120° C.

[0049] (3) The agglomerated powder obtained in step (2) is placed in a crucible, heated to 1500° C. at a heating rate of 5° C. / min in an air furnace and kept at that temperature for 6 h, and then cooled to room temperature in the furnace to obtain spherical ytterbium silicate spray powder.

[0050] The spherical ytterbium silicate spray powder prepared in this embodiment is mainly Yb2Si2O7 phase through X-ray diffraction analysis, and the purity is 99.92%. The powder is sieved by particle size to obtain powder suitable for plasma spraying with a particle size range of 17-53 μm.

[0051] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing spherical ytterbium silicate spray powder, characterized in that: The steps include: (1) Weighing Yb2O3 powder with a D50 of 2.0-2.8 μm and a D90 of 5.1-6.4 μm and SiO2 powder with a D50 of 2.0-2.6 μm and a D90 of 6.0-6.8 μm in a molar ratio of 1.05-2.05:1, adding high-purity water and polyvinyl alcohol, stirring for 0.8-1.2 h, and adjusting the pH of the slurry to 11-12 with ammonia water; (2) using a spray drying device to prepare agglomerated powder from the material obtained in step (1), wherein the atomizer speed is 18000-23000 r / min, the inlet temperature of the high-temperature dry air is controlled at 170-220° C., and the outlet temperature is controlled at 90-120° C.; (3) The agglomerated powder obtained in step (2) is heated to 1450-1550° C. in an air furnace for 3-6 hours, and then cooled to room temperature in the furnace to obtain a spherical ytterbium silicate spray powder mainly in the Yb2SiO5 phase or the Yb2Si2O7 phase.

2. The preparation method according to claim 1, characterized in that: The purity standard of the Yb2O3 powder is 4N or 5N.

3. The preparation method according to claim 1, characterized in that: The SiO2 powder is analytically pure.

4. The preparation method according to claim 1, characterized in that: The polyvinyl alcohol is PVA1788.

5. The preparation method according to claim 1, characterized in that: The purity standard of the Yb2O3 powder is 4N or 5N, the SiO2 powder is analytically pure, and the polyvinyl alcohol is PVA1788.

6. The preparation method according to any one of claims 1 to 5, characterized in that: In the step (1), the mass of the high-purity water is 80-200% of the total mass of the Yb2O3 powder and the SiO2 powder.

7. The preparation method according to claim 6, characterized in that: In the step (1), the mass of the polyvinyl alcohol is 2-5% of the total mass of the Yb2O3 powder and the SiO2 powder.

8. The preparation method according to claim 1, characterized in that: The heating rate in step (3) is 5-10°C / min.

9. Use of the spherical ytterbium silicate spray powder prepared by the preparation method according to any one of claims 1 to 8 in the preparation of thermal barrier coating materials.

10. A thermal barrier coating material, characterized in that: The raw material comprises spherical ytterbium silicate spray powder obtained by the preparation method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of ytterbium silicate plasma spaying powder

    CN109837496A

  • Preparation method of nano-structure ytterbium silicate feed suitable for plasma spraying

    CN111410201A

  • Ytterbium silicate spheroidized powder and plasma in-situ synthesis preparation method thereof

    CN113955763A

  • Spraying particles and manufacturing method thereof

    US20200190334A1