Method for preparing superfine high-purity terbium oxide through low-temperature calcination

The conversion reaction in the presence of surfactant was achieved by room temperature solid phase reaction method, and terbium oxalate or terbium carbonate with controllable particle size was solved, which was solved by the problem of large particle size and wide distribution of existing terbium oxide powder, achieving high The preparation of pure and ultra-fine terbium oxide powder reduces production costs and improves the controllability of the process.

CN118993126APending Publication Date: 2024-11-22GUANGXI UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410412265.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing terbium oxide preparation method, the precipitation method obtains powders with large particle size and wide particle size distribution. The sol-gel method is complex and has high cost. The template method is not suitable for large-scale production, making it difficult to obtain high-purity, ultra-fine, and particles. Terbium oxide powder with narrow diameter distribution.

Method used

The room temperature solid phase reaction method is used to mix the ball mill terbium salt and the reactant in the presence of a surfactant to convert the reaction under supersaturation to produce terbium oxalate or terbium carbonate with a controllable particle size, followed by calcination at low temperature. It forms ultrafine terbium oxide powder with narrow particle size distribution.

Benefits of technology

It realizes the preparation of ultra-fine, high-purity terbium oxide powder with simple operation, low cost and easy to control, and the particle size is controllable and suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004779585140000051
    Figure BDA0004779585140000051
  • Figure BDA0004779585140000061
    Figure BDA0004779585140000061
  • Figure HDA0004779585150000011
    Figure HDA0004779585150000011
Patent Text Reader

Abstract

The invention discloses a method for preparing superfine high-purity terbium oxide through low-temperature calcination. The method comprises the following steps: carrying out a room-temperature solid-phase reaction on terbium salt containing crystal water and a reactant oxalate or carbonate in the presence of a surfactant through ball milling; and removing water-soluble inorganic matters by washing, and drying to obtain terbium oxalate, terbium carbonate or a mixture of terbium oxalate and terbium carbonate. And carrying out high-temperature calcination on terbium oxalate, terbium carbonate or a mixture of terbium oxalate and terbium carbonate to obtain superfine and high-purity cubic crystal Tb2O3. By adopting the preparation method, the cubic crystal type superfine high-purity terbium oxide with the average crystallite size (nm) of 12.4-40.5 and the purity of 99.99% can be obtained. The particle size and purity of Tb2O3 are easy to control, the preparation process is simple, and large-scale production is easy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth material preparation, in particular to a method for preparing ultrafine high-purity terbium oxide by low-temperature calcination. Background Art

[0002] Terbium oxide has two crystal forms and three compositions, namely cubic Tb 2 O 3 , cubic Tb 4 O 7 , triclinic TbO 1.81 .Tb 2 O 3 The oxidation number of Tb is +3, and Tb 4 O 7 and TbO 1.81 Tb contains +3 and +4 oxidation numbers. 2 O 3 With magneto-optical effect [Tb 2 O 3 It has the highest Verdet constant in the visible and near-infrared range, which is more than three times higher than the Verdet constant of TGG (terbium gallium garnet) in the applicable wavelength range], high thermal shock resistance, high hardness, corrosion resistance, and high melting point (2400°C), so Tb 2 O 3 The material is used to make magneto-optical glass, phosphor, and magneto-optical storage; Tb 2 O 3 It can also be used as a dopant for energy storage positive electrode materials to improve some defects in positive electrode materials and improve the cycle performance of batteries. In addition, terbium oxide powder can be pressed and sintered to make varistor materials with low transition voltage, strong energy absorption capacity and good dielectric properties.

[0003] The performance of related materials prepared with terbium oxide depends on the purity, particle size and particle size distribution of terbium oxide. Terbium oxide powder with high purity, ultrafine and narrow particle size distribution is conducive to the preparation of high-performance terbium oxide-based materials. In addition, a simple and low-cost terbium oxide preparation process can reduce the cost of preparing high-performance terbium oxide-based materials. At present, several methods for preparing terbium oxide powder have been publicly reported, including precipitation method, sol-gel method, template method such as a method for preparing three-dimensional ordered macroporous praseodymium oxide and terbium oxide with mesoporous pore walls. The precipitation method has the advantages of simple process, easy control of conditions, and easy large-scale production, but the terbium oxide obtained by this method has a large particle size and a wide particle size distribution. Although the particle size of terbium oxide is still at the micron level after ball milling, the sintering activity is not high. The sol-gel method uses organic matter and terbium ion chelation polycondensation to form a precursor, and then calcines the precursor to form terbium oxide. The advantage of this method is that it is easy to obtain ultrafine terbium oxide, but the disadvantage is that the process is complicated and not conducive to large-scale production. The template method uses a soft template, i.e., a surfactant or a hard template such as polymethyl methacrylate, to prepare terbium oxide Tb with a large specific surface area and a three-dimensional ordered macroporous structure of mesoporous pore walls. 4 O 7 The disadvantage of this method is that it is costly and difficult to produce on a large scale. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a method for preparing ultrafine high-purity terbium oxide by low-temperature calcination, which utilizes a simple room temperature solid-phase reaction method, in the presence of a surfactant, by ball milling a mixture of a terbium salt and a reactant, so that the terbium salt and the reactant are always in a supersaturated state to undergo a conversion reaction to generate terbium oxalate or terbium carbonate with controllable particle size and small particle size, thereby creating conditions for the subsequent thermal decomposition of terbium oxalate or terbium carbonate into ultrafine terbium oxide powder with a narrow particle size distribution, while reducing production costs.

[0005] The present invention achieves the above-mentioned purpose by adopting the following technical scheme: A method for preparing ultrafine high-purity terbium oxide by low-temperature calcination, comprising the following steps:

[0006] (1) placing terbium salt and reactant in a ball mill according to the stoichiometric ratio, adding surfactant and water, and subjecting to ball milling reaction at room temperature to prepare a reaction product A, wherein the ball milling time is 1 to 2 hours, the rotation speed is 400 to 420 rpm, and the amount of surfactant added is 0.2 to 0.6% of the mass of the terbium salt;

[0007] (2) washing the reaction product A with water to remove soluble inorganic salts, and drying to obtain a reaction product B, wherein the drying temperature is 50 to 110° C. and the drying time is 1 to 5 hours;

[0008] (3) The reaction product B is calcined at 500-700° C. in an air atmosphere for 3-4 hours, and then naturally cooled to room temperature to obtain an ultrafine, high-purity cubic terbium oxide powder.

[0009] The terbium salt is terbium salt powder containing crystal water.

[0010] The terbium salt is selected from one or more of terbium sulfate, terbium nitrate, terbium chloride, and terbium acetate; the reactant is one or more of sodium oxalate, potassium oxalate, ammonium oxalate, sodium carbonate, sodium bicarbonate, potassium carbonate, and ammonium carbonate; and the surfactant is selected from one or more of coconut oil alkylamide, Tween series, OP series, ethylene glycol, polyethylene glycol series, polyether series, and sorbic acid glycerol.

[0011] The surfactant is polyethylene glycol-400 or coconut oil alkylamide.

[0012] When the surfactant is polyethylene glycol-400, the surfactant is added at 0.2-0.6% of the mass of the terbium salt.

[0013] When the surfactant is coconut oil alkylamide, it is added at 0.5% of the mass of the terbium salt.

[0014] The ultrafine high-purity terbium oxide has a cubic crystal structure, an average crystallite size (nm) of 12.4-40.5, and a purity of 99.99%.

[0015] Compared with the prior art, the outstanding advantages of the present invention are:

[0016] Through room temperature solid phase reaction, in the presence of a surfactant, by ball milling a mixture of terbium salt and reactant, the terbium salt and reactant are always in a supersaturated state to undergo a conversion reaction to generate terbium oxalate, terbium carbonate or a mixture of the two with smaller particle sizes, thereby creating conditions for subsequent thermal decomposition into ultrafine terbium oxide powder with a narrow particle size distribution.

[0017] The method of the invention is simple to operate, the reaction conditions are easy to control, the cost is low, and ultrafine and high-purity terbium oxide powder can be easily obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the X-ray diffraction (XRD) pattern of terbium oxalate prepared in Example 1 of the present invention.

[0019] Figure 2 This is a scanning electron microscope (SEM) image of the terbium oxalate prepared in Example 1 of the present invention.

[0020] Figure 3 This is the X-ray diffraction (XRD) pattern of terbium oxide prepared in Example 1 of the present invention.

[0021] Figure 4 This is a scanning electron microscope (SEM) image of the terbium oxide prepared in Example 1 of the present invention.

[0022] Figure 5This is the X-ray diffraction (XRD) pattern of terbium oxide prepared in Example 2 of the present invention.

[0023] Figure 6 This is a scanning electron microscope (SEM) image of the terbium oxide prepared in Example 2 of the present invention.

[0024] Figure 7 This is the X-ray diffraction (XRD) pattern of terbium oxide prepared in Example 3 of the present invention.

[0025] Figure 8 This is a scanning electron microscope (SEM) image of the terbium oxide prepared in Example 3 of the present invention.

[0026] Fig. 9 This is the X-ray diffraction (XRD) pattern of terbium oxide prepared in Example 4 of the present invention.

[0027] Fig.10 This is a scanning electron microscope (SEM) image of the terbium oxide prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the preferred embodiments of the present invention are further described in detail in conjunction with the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0029] Example 1

[0030] This embodiment is an example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0031] 10.00 g of 0.02207 mol Tb(NO 3 ) 3 6H 2 O, 4.658 g of 0.03476 mol (5% excess) Na 2 C 2 O 4 The powder was placed in a ball mill, 0.20 g of polyethylene glycol-400 was added, 1.0 mL of water was added as a solvent, and the raw material was ball milled at a speed of 420 rpm for 1 hour for room temperature solid phase reaction. The soluble inorganic salts in the reaction mixture were washed with water and the precipitate was collected by filtration. The precipitate was dried at 60°C for 2 hours to obtain terbium oxalate, the precursor of terbium oxide. Finally, terbium oxalate was placed in a muffle furnace and calcined at 500°C for 3 hours. The calcined product was naturally cooled to about 40°C to obtain terbium oxide powder. The XRD pattern of the obtained terbium oxalate is shown below. Figure 1 As shown, after retrieval, it is Tb 2 (C2 O 4 ) 3 10H 2 O. According to the Scherrer formula [D = Kλ / (βcosθ)], terbium oxalate (Tb 2 (C 2 O 4 ) 3 10H 2 The average crystallite size of the nanostructured carbon nanotubes was 54.9 nm. Figure 2 The scanning electron microscope (SEM) image of terbium oxalate is shown. Figure 2 Tb can be seen in 2 (C 2 O 4 ) 3 10H 2 O particles are flake-shaped, with particle sizes ranging from 200nm to 450nm. Figure 3 The XRD pattern of terbium oxide powder is shown. Figure 3 Cubic Tb 2 O 3 The characteristic diffraction peaks of the nanostructured carbon nanotubes are shown in Figure 2, and the average crystallite size is 12.5 nm. Figure 4 Shows Tb 2 O 3 SEM images of particles. Figure 4 Tb can be seen in 2 O 3 The particles are irregular in shape and the particle size ranges from 50nm to 600nm. 2 O 3 The particles are formed by agglomeration of many smaller microcrystalline particles. The purity of terbium oxide is 99.99%.

[0032] Example 2

[0033] This embodiment is another example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0034] 10.00 g of 0.02207 mol Tb(NO 3 ) 3 6H 2 O, 4.658 g of 0.03476 mol (5% excess) Na 2 C 2 O 4The powder was placed in a ball mill, 0.2 g of polyethylene glycol-400 was added, 1.0 mL of water was added as a solvent, the raw material was ball milled at a speed of 420 rpm for 1 h for room temperature solid phase reaction, the soluble inorganic salts in the reaction mixture were washed with water, and the precipitate was collected by filtration, and the precipitate was dried at 60°C for 2 h to obtain terbium oxalate, the precursor of terbium oxide. Finally, terbium oxalate was placed in a muffle furnace and calcined at 600°C for 3 h, and the calcined product was naturally cooled to about 40°C to obtain terbium oxide powder. Figure 5 The XRD pattern of terbium oxide powder is shown. Figure 5 Cubic Tb 2 O 3 The characteristic diffraction peaks of the nanostructured carbon nanotubes are shown in Figure 2, and the average crystallite size is 20.6 nm. Figure 6 Shows Tb 2 O 3 SEM images of particles. Figure 6 Tb can be seen in 2 O 3 The particles are irregular in shape and the particle size ranges from 50nm to 600nm. 2 O 3 The particles are formed by soft agglomeration of many smaller microcrystalline particles. The purity of terbium oxide is 99.99%

[0035] Example 3

[0036] This embodiment is another example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0037] 10.00 g of 0.02207 mol Tb(NO 3 ) 3 6H 2 O, 4.658 g of 0.03476 mol (5% excess) Na 2 C 2 O 4 The powder was placed in a ball mill, 0.2 g of polyethylene glycol-400 was added, 1.0 mL of water was added as a solvent, the raw material was ball milled at a speed of 420 rpm for 1 h for room temperature solid phase reaction, the soluble inorganic salts in the reaction mixture were washed with water and the precipitate was collected by filtration, and the precipitate was dried at 60°C for 2 h to obtain terbium oxalate, a precursor of terbium oxide. Finally, terbium oxalate was placed in a muffle furnace and calcined at 700°C for 3 h, and the calcined product was naturally cooled to about 40°C to obtain terbium oxide powder. Figure 7 The XRD pattern of terbium oxide powder is shown. Figure 7 Cubic Tb 2 O 3 The characteristic diffraction peaks of the nanostructured carbon nanotubes are shown in Figure 2, and the average crystallite size is 39.7 nm. Figure 8 Shows Tb2 O 3 SEM images of particles. Figure 8 Tb can be seen in 2 O 3 The particles are irregular polyhedrons with a particle size ranging from 40nm to 100nm. The purity of terbium oxide is 99.99%

[0038] Example 4

[0039] This embodiment is another example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0040] 10.00 g of 0.02678 mol TbCl 3 6H 2 O, 5.651 g of 0.04218 mol (5% excess) Na 2 C 2 O 4 The powder was placed in a ball mill, 0.3 g of polyethylene glycol-400 was added, 1.0 mL of water was added as a solvent, the raw material was ball milled at a speed of 400 rpm for 2 h for room temperature solid phase reaction, the soluble inorganic salts in the reaction mixture were washed with water and the precipitate was collected by filtration, and the precipitate was dried at 75 ° C for 1.5 h to obtain terbium oxalate, the precursor of terbium oxide. Finally, terbium oxalate was placed in a muffle furnace and calcined at 700 ° C for 4 h, and the calcined product was naturally cooled to about 40 ° C to obtain terbium oxide powder. Fig. 9 The XRD pattern of terbium oxide powder is shown. Figure 7 Cubic Tb 2 O 3 The characteristic diffraction peak of the quartz crystal is 40.5 nm in average size. Fig.10 Shows Tb 2 O 3 SEM images of particles. Fig.10 Tb can be seen in 2 O 3 The particles are irregular polyhedrons with a particle size ranging from 40nm to 100nm. The purity of terbium oxide is 99.99%.

[0041] Example 5

[0042] This embodiment is the fifth example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0043] 10.00 g of 0.02207 mol Tb(NO 3 ) 3 6H 2 O, 3.684 g of 0.03476 mol (5% excess) Na 2CO 3 The powder was placed in a ball mill, 0.5 g of coconut oil alkylamide was added, 1.5 mL of water was added as a solvent, and the raw material was ball milled at a speed of 425420 rpm for 1 h for room temperature solid phase reaction. The soluble inorganic salts in the reaction mixture were washed with water and the precipitate was collected by filtration. The precipitate was dried at 90 ° C for 1.5 h to obtain terbium carbonate, the precursor of terbium oxide. Finally, terbium carbonate was placed in a muffle furnace and calcined at 500 ° C for 3 h. The calcined product was naturally cooled to about 40 ° C to obtain cubic phase Tb 2 O 3 , the average crystallite size is 12.4nm. The purity of terbium oxide is 99.99%.

[0044] Example 6

[0045] This embodiment is the sixth example of the method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to the present invention, comprising the following steps:

[0046] 10.00 g of 0.01333 mol Tb 2 (SO 4 ) 3 8H 2 O, 5.615 g of 0.04190 mol (5% excess) Na 2 C 2 O 4 The powder was placed in a ball mill, 0.6 g of polyethylene glycol-400 was added, 1.0 mL of water was added as a solvent, the raw material was ball milled at a speed of 400 rpm for 2 h for room temperature solid phase reaction, the soluble inorganic salts in the reaction mixture were washed with water and the precipitate was collected by filtration, and the precipitate was dried at 75 ° C for 1.5 h to obtain terbium oxalate, the precursor of terbium oxide. Finally, terbium oxalate was placed in a muffle furnace and calcined at 600 ° C for 3 h. The calcined product was naturally cooled to about 40 ° C to obtain a cubic phase Tb 2 O 3 , the average crystallite size is 21.0nm. The purity of terbium oxide is 99.99%.

[0047] Table 1 Crystalline size of terbium oxide prepared under different technical conditions

[0048]

[0049]

[0050] From the cubic terbium oxide (Tb 2 O 3 ) powder crystallite size changes, it can be seen that terbium oxide (Tb 2 O 3) The crystallite size of the particles mainly depends on the calcination temperature. As the calcination temperature increases, the cubic Tb 2 O 3 The crystallite size of the powder increases. Therefore, calcining the precursor at a lower calcination temperature (e.g., 500°C) can obtain cubic Tb with a smaller crystallite size. 2 O 3 , while reducing the energy consumption of preparing terbium oxide.

Claims

1. A method for preparing ultrafine high-purity terbium oxide by low-temperature calcination, It is characterized in that The steps include: (1) placing terbium salt and reactant in a ball mill according to the stoichiometric ratio, adding surfactant and water, and subjecting to ball milling reaction at room temperature to prepare a reaction product A, wherein the ball milling time is 1 to 2 hours, the rotation speed is 400 to 420 rpm, and the amount of surfactant added is 0.2 to 0.6% of the mass of the terbium salt; (2) washing the reaction product A with water to remove soluble inorganic salts, and drying to obtain a reaction product B, wherein the drying temperature is 50 to 110° C. and the drying time is 1 to 5 hours; (3) The reaction product B is calcined at 500-700° C. in an air atmosphere for 3-4 hours, and then naturally cooled to room temperature to obtain an ultrafine, high-purity cubic terbium oxide powder.

2. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 1, It is characterized in that The terbium salt is terbium salt powder containing crystal water.

3. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 1, It is characterized in that The terbium salt is selected from one or more of terbium sulfate, terbium nitrate, terbium chloride, and terbium acetate; the reactant is one or more of sodium oxalate, potassium oxalate, ammonium oxalate, sodium carbonate, sodium bicarbonate, potassium carbonate, and ammonium carbonate; and the surfactant is selected from one or more of coconut oil alkylamide, Tween series, OP series, ethylene glycol, polyethylene glycol series, polyether series, and sorbic acid glycerol.

4. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 1, It is characterized in that The surfactant is polyethylene glycol-400 or coconut oil alkylamide.

5. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 4, It is characterized in that When the surfactant is polyethylene glycol-400, the surfactant is added at 0.2-0.6% of the mass of the terbium salt.

6. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 4, It is characterized in that When the surfactant is coconut oil alkylamide, it is added at 0.5% of the mass of the terbium salt.

7. The method for preparing ultrafine high-purity terbium oxide by low-temperature calcination according to claim 1, It is characterized in that The average crystallite size (nm) of the ultrafine high-purity terbium oxide is 12.4-40.5, and the purity is 99.99%.