Near-infrared absorbing glass and near-infrared cut-off filter

By optimizing the composition and process of the glass, the problem that the near-infrared cutoff filter is difficult to maintain high visible light transmittance and weather resistance when improving the near-infrared cutoff capability and thinning, and the excellent performance of the near-infrared absorbing glass is achieved.

CN118993534APending Publication Date: 2024-11-22HOYA CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411197549.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-12-27
Filing Date
2020-12-25
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

While the existing near-infrared cutoff filters improve the near-infrared cutoff capability and thinning, it is difficult to maintain high visible light transmittance and weather resistance. The increase in Cu ion concentration will lead to the generation of Cu+, affecting the transmittance and durability.

Method used

By configuring the complex-shaped glass skeleton of P2O5 in the glass, the intermediate components are reduced, the generation of Cu+ is inhibited, and melted/formed at lower temperatures is performed, and the Cu ions content and other components ratios are optimized to achieve excellent near-infrared rays Cutoff capability, high visible light transmittance and weather resistance.

Benefits of technology

It realizes near-infrared absorption glass with excellent near-infrared cutoff capability, high visible light transmittance, excellent weather resistance and melting properties. It is suitable for thin-walled near-infrared cutoff filters, improving the performance and visible light transmittance of the imaging element.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993534A_ABST
    Figure CN118993534A_ABST
Patent Text Reader

Abstract

The present invention relates to a near-infrared absorbing glass which contains at least P ions, Cu ions, O ions, one or more ions selected from the group consisting of Li, Na and K ions, and one or more ions selected from the group consisting of Mg, Ca, Sr and Ba ions as constituent ions, the Cu ions being 15.0 cation% or less, the P ions being 55.0 cation% or less, and the cation ratio ((Al ions + P ions) / (Mg ions + Ca ions + Sr ions + Ba ions + Zn ions + Cu ions)) being 5.300 or less. The cation ratio ((Mg ion + Ca ion + Sr ion + Ba ion) / (Li ion + Na ion + K ion)) is 0.100 or more, the average valence of cations other than Cu ions and P is less than 1.500, the O ion is 85.0 anion% or more, and the ratio (O ion / P ion) is 3.300 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of December 25, 2020, application number 202080090602.4, and invention name “Near-infrared absorption glass and near-infrared cut-off filter”. Technical Field

[0002] The present invention relates to near infrared absorbing glass and a near infrared cutoff filter. Background Art

[0003] The near infrared cut filter has the function of filtering out the unnecessary near infrared light (wavelength 700-1200nm) within the sensitivity wavelength range of the imaging element in order to make the light entering the imaging element such as CCD and CMOS reach the light wavelength distribution equivalent to the relative visibility curve of humans. Generally speaking, the near infrared cut filter is mostly set in front of the imaging element.

[0004] Near-infrared cut filters are widely used in which a near-infrared absorbing glass is used as a base material and a polished flat plate is used.

[0005] Near infrared absorbing glass generally contains Cu ions. An example of the spectral transmission characteristics of near infrared absorbing glass is shown in Figure 1 It should be noted that Figure 1 The light absorption characteristics near the wavelength of 700 to 1200 nm are determined by the Cu ions (Cu 2+ Among them, phosphate glass containing Cu ions can display Cu ions (Cu 2+ ) has near-infrared absorption properties and is therefore useful as glass for near-infrared cutoff filters (see, for example, Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2019-38719

[0009] exist Figure 1 In the transmittance curve after the wavelength of 600nm, the wavelength at which the transmittance reaches 50% is called the "half-value", which has become one of the main standards for near-infrared cut-off filters. The half-value varies depending on the specifications of the filter, but is mostly set in the wavelength range of 600nm to 650nm. As a general method to achieve the desired half-value, there are methods such as adjusting the thickness of the glass substrate according to the Lambert-Beer law, or adjusting the Cu ion (Cu) content in the glass. 2+ ) concentration in any condition. Summary of the invention

[0010] Problems to be solved by the invention

[0011] The near infrared cut filter is required to have not only excellent ability to cut near infrared rays (ie, to have a desired half value and low near infrared transmittance) but also high transmittance for visible light (wavelength 400 to 600 nm).

[0012] In addition, in recent years, the camera element modules installed in smartphones and the like have been required to be both small and high-performance, so the thickness of the near-infrared cut filter has been required to be thinner. In order to achieve thinning while maintaining the ability to filter out near-infrared rays, it is necessary to increase the Cu ion (Cu 2+ However, it is known that if the ratio of the Cu component in the glass raw material is simply increased for this purpose, the Cu 2+ The reduced Cu + Increase, especially the transmittance decreases near the wavelength of 400nm.

[0013] Furthermore, in order to maintain transmittance characteristics in various usage environments, the near infrared cut filter is desired to have high chemical durability (that is, excellent weather resistance) in a high temperature and high humidity environment.

[0014] In view of the above circumstances, an object of one embodiment of the present invention is to provide a near-infrared absorbing glass having excellent near-infrared cutting ability, high visible light transmittance, and excellent weather resistance, and a near-infrared cut filter made of the near-infrared absorbing glass.

[0015] Solutions to the problem

[0016] The present inventors have studied glass compositions from the following two viewpoints in order to improve visible light transmittance.

[0017] (1) A glass composition that can achieve a desired half-value and sufficient near-infrared cutoff capability even with a smaller Cu content than before.

[0018] (2) In order to suppress the melting of Cu + The formation of glass compositions at lower temperatures makes it effective to melt / form the glass, so the solubility of the raw material batch is better than that of conventional glass compositions.

[0019] Regarding (1), the present inventors found that by assuming that 2+ The glass skeleton of the complex of P2O5 is arranged around it, and the average valence of the intermediate components other than these glass skeletons, that is, the monovalent and divalent ions, is reduced, which can inhibit the flow of electrons into Cu 2+ , i.e. inhibiting Cu + The generation of Cu 2+By shifting the light absorption wavelength region to a shorter wavelength, the amount of Cu required to achieve the desired half value can be reduced.

[0020] Regarding (2), the present inventors have found that by reducing the proportion of glass network forming components such as Al and P to a certain ratio or less, the solubility of the glass raw material batch can be improved, thereby enabling melting and molding at a lower temperature than before.

[0021] The present inventors have found that by setting the ratio of O to P in the entire glass to a certain ratio or more, the amount of Cu required to achieve a desired half value can be reduced, and the formation of POP crosslinks that have poor water resistance can be suppressed to improve weather resistance.

[0022] That is, one embodiment of the present invention relates to a near-infrared absorbing glass (hereinafter, also referred to as “glass”) containing at least the following ions as constituent ions:

[0023] P ions,

[0024] Cu ions,

[0025] O ions,

[0026] One or more ions selected from Li ions, Na ions and K ions, and

[0027] One or more ions selected from Mg ions, Ca ions, Sr ions and Ba ions,

[0028] in,

[0029] In the glass composition expressed in cation %,

[0030] The content of Cu ions is less than 15.0 cation %,

[0031] The content of P ions is less than 55.0 cation %,

[0032] The cation ratio ((Al ion + P ion) / (Mg ion + Ca ion + Sr ion + Ba ion + Zn ion + Cu ion)) of the total content of Al ion and P ion to the total content of Mg ion, Ca ion, Sr ion, Ba ion, Zn ion and Cu ion is 5.300 or less,

[0033] The cation ratio of the total content of Mg ions, Ca ions, Sr ions and Ba ions to the total content of Li ions, Na ions and K ions ((Mg ions + Ca ions + Sr ions + Ba ions) / (Li ions + Na ions + K ions)) is 0.100 or more,

[0034] The average valence of cations other than Cu ions and P ions is less than 1.500.

[0035] In the glass composition expressed in anion %,

[0036] The content of O ions is 85.0% or more of anions, and

[0037] The ratio of the content of O ions to the content of P ions (O ions / P ions) is 3.300 or more.

[0038] The near-infrared absorbing glass having the above-mentioned glass composition can have excellent near-infrared cutting ability, high visible light transmittance, and excellent weather resistance and solubility.

[0039] Effects of the Invention

[0040] According to one embodiment of the present invention, a near-infrared absorbing glass having excellent near-infrared cutoff capability, high visible light transmittance, and excellent weather resistance and solubility can be provided. Furthermore, according to one embodiment of the present invention, a near-infrared cutoff filter made of such near-infrared absorbing glass can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 An example of the spectral transmission characteristics of the near-infrared absorbing glass is shown. DETAILED DESCRIPTION

[0042] [Near infrared absorbing glass]

[0043] In the present invention and this specification, near-infrared absorbing glass refers to glass having the property of absorbing at least the entire region or part of the wavelength of the near-infrared wavelength region (wavelength 700 to 1200 nm). In addition, the near-infrared absorbing glass of one embodiment of the present invention may be an oxide glass because it contains O ions (oxygen ions) as constituent ions. Oxide glass refers to glass whose main network-forming component is an oxide. Furthermore, the near-infrared absorbing glass of one embodiment of the present invention may be a phosphate glass because it contains O ions (oxygen ions) and P ions (phosphorus ions) as constituent ions.

[0044] Hereinafter, the near-infrared absorbing glass will be described in more detail.

[0045] <Glass composition>

[0046] In the present invention and this specification, the content and total content of cations (cationic components) are expressed as cation % unless otherwise specified, and the content and total content of anions (anionic components) are expressed as anion % unless otherwise specified.

[0047] Here, "cation %" refers to a value calculated by "(number of cations of interest / total number of cations in glass component)×100", and refers to the molar percentage of the amount of cations of interest relative to the total amount of cations.

[0048] In addition, "anion %" is a value calculated by "(number of anions of interest / total number of anions in glass component)×100", and means the molar percentage of the amount of anions of interest relative to the total amount of anions.

[0049] The molar ratio of the contents of the cations is equal to the content ratio of the cations of interest expressed as cation %, and the molar ratio of the contents of the anions is equal to the content ratio of the anions of interest expressed as anion %.

[0050] The molar ratio of the content of cations to the content of anions is the ratio of the contents (expressed in mol %) of the components of interest when the total amount of all cations and all anions is taken as 100 mol %.

[0051] The content of each component can be quantified by a known method, such as inductively coupled plasma emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), ion chromatography, etc. The content of each element (mass %) contained in the glass can be determined by dividing the content of the element (mass %) by the atomic weight, and the cation % and anion % can be determined from this value.

[0052] In the present invention and this specification, "the content of a component is 0% or is not contained or introduced" means that the component is not substantially contained, but inclusion of the component at an inevitable impurity level is permitted. The inevitable impurity level means, for example, less than 0.01%.

[0053] Regarding the valence of cations, in order to obtain an average valence as described in detail later, the formal valence of each cation is used. The formal valence refers to the valence required for the oxide of the cation of interest to maintain electrical neutrality when the valence of the oxygen ion (anion) constituting the oxide is set to -2, and can be clearly determined from the chemical formula of the oxide. For example, in order to maintain the O contained in the chemical formula of the oxide CuO, 2- The electronegativity of Cu is +2. For example, regarding P ions, in order to maintain the O contained in the chemical formula of the oxide P2O5, 2- The charge of P is neutral, and the valence of P is +5. If we summarize it, the cation A X O YThe formal valence of is "+2X / Y". Therefore, when analyzing the glass composition, it is also possible not to analyze the valence of the cation. In addition, regarding the valence of the anion (for example, the valence of the oxygen ion is -2), it is also a formal valence based on the idea that the oxygen ion accepts two electrons and takes a closed shell structure. Therefore, when analyzing the glass composition, it is also possible not to analyze the valence of the anion. In addition, as mentioned above, Cu 2+ Part of it may become Cu during melting + However, since its amount is very small, when calculating the average valence, the valence of Cu can all be regarded as +2.

[0054] (Cationic)

[0055] P ions are network-forming components of glass. From the viewpoint of improving weather resistance and improving solubility, the P ion content of the above-mentioned glass is 55.0% or less, preferably 53.0% or less, more preferably 51.0% or less, further preferably 50.0% or less, further more preferably 49.0% or less, further more preferably 48.0% or less, further more preferably 47.0% or less, further more preferably 46.0% or less, further more preferably 45.0% or less, further more preferably 44.0% or less. Since the above-mentioned glass contains P ions as constituent ions, the P ion content exceeds 0%. From the viewpoint of improving the resistance to devitrification during glass melting and improving the mechanical strength of the glass, the P ion content is preferably 30.0% or more, more preferably 32.0% or more, further preferably 34.0% or more, further more preferably 36.0% or more, further preferably 38.0% or more, further more preferably 39.0% or more, further more preferably 40.0% or more, further more preferably 41.0% or more. The formal valence of the P ion is +5.

[0056] Cu ions are components that contribute to imparting near-infrared cutoff capability to glass. From the viewpoint of improving visible light transmittance, the Cu ion content of the above-mentioned glass is 15.0% or less, preferably 13.0% or less, more preferably 11.0% or less, and further preferably 9.0% or less. Since the above-mentioned glass contains Cu ions as constituent ions, the Cu ion content exceeds 0%. In order to have sufficient near-infrared cutoff capability, the Cu ion content is preferably 0.5% or more, more preferably 1.5% or more, and further preferably 2.5% or more.

[0057] As will be described in detail later, the glass can be used as glass for a near-infrared cut filter having a thickness of 0.25 mm or less in one embodiment.

[0058] As glass suitable for a thinner near-infrared cutoff filter within the above-mentioned thickness range (hereinafter also referred to as "glass I"), the Cu ion content is preferably 1.5% or more, and more preferably in the order of 1.7% or more, 1.9% or more, 2.1% or more, 2.3% or more, 2.5% or more, 2.7% or more, 2.9% or more, 3.1% or more, 3.3% or more, 3.5% or more, 3.7% or more, 3.9% or more, 4.1% or more, 4.5% or more, 4.7% or more, 4.9% or more, and 5.1% or more.

[0059] In addition, from the viewpoint of further improving the visible light transmittance in the near-infrared cutoff filter, the Cu ion content of glass I is preferably 15.0% or less, and more preferably 13.0% or less, 11.0% or less, 10.0% or less, 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, 6.5% or less, and 6.0% or less.

[0060] By multiplying the above preferred range by (0.11 / d), the preferred value of Cu ions to be contained in glass suitable for a near infrared cut filter having a desired thickness can be obtained. d is the thickness for which the preferred value of Cu ions is to be obtained, and the unit is mm.

[0061] In addition, regarding glass suitable for thicker near-infrared cutoff filters in the thickness range of less than 0.25 mm (hereinafter also referred to as "glass II"), in one embodiment, the preferred range of Cu ions can be calculated by multiplying the above-mentioned preferred range by (0.11 / d).

[0062] In addition, regarding glass II, in one embodiment, the Cu ion content is preferably 0.5% or more, and more preferably in the order of 0.7% or more, 0.9% or more, 1.1% or more, 1.3% or more, 1.5% or more, 1.7% or more, 1.9% or more, 2.1% or more, 2.3% or more, and 2.5% or more. In addition, from the viewpoint of further improving the visible light transmittance in such a near-infrared cutoff filter, in one embodiment, the Cu ion content of glass II is preferably 10.0% or less, and more preferably in the order of 9.0% or less, 8.5% or less, 8.0% or less, 7.5% or less, 7.0% or less, 6.5% or less, 6.0% or less, 5.5% or less, 5.0% or less, 4.5% or less, 4.0% or less, and 3.5% or less. The formal valence of Cu ion is +2.

[0063] The Li ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. Li ion is a component that has the effect of improving the devitrification resistance of the glass during melting / molding. From the viewpoint of improving the solubility of the glass, the Li ion content is preferably 10.0% or more, more preferably 12.0% or more, further preferably 13.0% or more, further more preferably 14.0% or more, further more preferably 15.0% or more, further more preferably 16.0% or more, further more preferably 17.0% or more, further more preferably 18.0% or more, further more preferably 20.0% or more, further more preferably 20.5% or more, further more preferably 21.0% or more, and further more preferably in the order of 21.5% or more, 22.0% or more, 22.5% or more, 23.0% or more, 23.5% or more, 24.0% or more, 24.5% or more, 25.0% or more, 25.5% or more, and 26.0% or more. In addition, from the viewpoint of improving the chemical durability and / or processability of the glass, or increasing the liquidus viscosity of the glass, the Li ion content is preferably 32.0% or less, more preferably 31.0% or less, further preferably 30.5% or less, further more preferably 30.0% or less, further preferably 29.5% or less, further preferably 29.0% or less, further preferably 28.5% or less, further preferably 28.0% or less, and particularly preferably 27.5% or less. The formal valence of the Li ion is +1. In one embodiment, from the above viewpoint, it is preferred to make "Li ion content>Na ion content", and it is preferred to make "Li ion content>K ion content".

[0064] The Na ion content of the glass may be 0%, 0% or more, or more than 0%. Na ions are also a component that improves the solubility of the glass. In one embodiment, Li or K is preferably used mainly. Specifically, from the viewpoint of improving the devitrification resistance of the glass, improving the viscosity at the liquidus temperature, and improving the chemical durability and / or processability, the Na ion content is preferably 30.0% or less, more preferably 28.0% or less, further preferably 27.0% or less, further more preferably 25.0% or less, further more preferably 23.0% or less, further more preferably 21.0% or less, further more preferably 19.0% or less, further more preferably 17.0% or less, further more preferably 15.0% or less, further more preferably 13.0% or less, and further more preferably in the order of 11.0% or less, 10.0% or less, 9.0% or less, 8.0% or less, 7.0% or less, 6.0% or less, 5.0% or less, 4.0% or less, 3.0% or less, 2.0% or less, 1.0% or less, and 0.5% or less. The formal valence of the Na ion is +1. In one embodiment, from the above viewpoint, it is preferable that "Na ion content <Li ion content" and it is preferable that "Na ion content <K ion content" be set.

[0065] The K ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. K ions are also components that have the effect of improving the solubility of the glass and further improving the resistance to devitrification during melting / molding. From these viewpoints, the K ion content is preferably 3.0% or more, more preferably 4.0% or more, further preferably 5.0% or more, further more preferably 6.0% or more, further more preferably 7.0% or more, further more preferably 8.0% or more, further more preferably 9.0% or more, and further more preferably 10.0% or more. On the other hand, from the viewpoint of improving the viscosity at the liquidus temperature of the glass, chemical durability and / or processability, the K ion content is preferably 20.0% or less, more preferably 19.0% or less, further preferably 17.0% or less, further more preferably 15.0% or less, further more preferably 14.5% or less, further more preferably 14.0% or less, further more preferably 13.5% or less, further more preferably 13.0% or less, further more preferably 12.5% ​​or less, and particularly preferably 12.3% or less. The formal valence of K ion is +1. In one embodiment, from the above viewpoint, it is preferable that "K ion content <Li ion content" and it is preferable that "K ion content >Na ion content".

[0066] The glass contains one or more ions selected from Li ions, Na ions, and K ions as constituent ions. That is, the glass may contain only Li ions in one embodiment, only Na ions in another embodiment, only K ions in another embodiment, Li ions and Na ions in another embodiment, Li ions and K ions in another embodiment, Na ions and K ions in another embodiment, and Li ions, Na ions, and K ions in another embodiment.

[0067] The glass may further contain other alkali metal ions in addition to Li ions, Na ions and K ions. Examples of other alkali metal ions include Cs ions. The Cs ion content of the glass may be 0%, 0% or more, or more than 0%. The formal valence of the Cs ion is +1.

[0068] From the viewpoint of reducing the average valence and improving the visible light transmittance, the total content of Li ions, Na ions and K ions is preferably 19.0% or more, more preferably 21.0% or more, further preferably 23.0% or more, further more preferably 25.0% or more, further more preferably 27.0% or more, still further preferably 28.0% or more, still further preferably 29.0% or more, still further preferably 30.0% or more, still further preferably 30.5% or more, still further preferably 31.0% or more, and further preferably 32.0% or more, 32.5% or more, 33.0% or more, 33.5% or more, 34.0% or more, 34.5% or more, 35.0% or more, 35.5% or more, 36.0% or more, 36.5% or more, 37.0% or more, 37.5% or more, 38.0% or more, 38.5% or more, 39.0% or more, and 39.1% or more in this order. In addition, from the viewpoint of further improving weather resistance, suppressing a decrease in the glass transition temperature, and / or suppressing a decrease in viscosity at a liquidus temperature, the total content of Li ions, Na ions, and K ions is preferably 56.0% or less, more preferably 54.0% or less, further preferably 52.0% or less, further more preferably 50.0% or less, further preferably 48.0% or less, still further preferably 46.0% or less, still further preferably 45.0% or less, and further preferably 44.0% or less, 43.0% or less, 42.5% or less, 42.0% or less, 41.5% or less, 41.0% or less, 40.5% or less, 40.0% or less, and 39.5% or less in this order.

[0069] The Mg ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. From the viewpoint of suppressing the decrease in the liquidus viscosity of the glass, reinforcing the mechanical strength of the glass, and / or reinforcing the chemical resistance, the Mg ion content is preferably 0.3% or more, more preferably 0.5% or more, further preferably 0.8% or more, further more preferably 1.1% or more, and further more preferably 1.3% or more. In addition, from the viewpoint of further improving the resistance to devitrification during melt forming, the Mg ion content is preferably 7.0% or less, more preferably 6.0% or less, further preferably 5.0% or less, further more preferably 4.0% or less, further preferably 3.5% or less, further preferably 3.0% or less, further preferably 2.5% or less, further preferably 2.0% or less, and further preferably 1.8% or less. The formal valence of the Mg ion is +2. In one embodiment, from the above viewpoint, it is preferred that "Mg ion content <Ca ion content" and "Mg ion content <Ba ion content" are preferably made.

[0070] The Ca ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. From the viewpoint of suppressing the decrease in the liquidus viscosity of the glass, reinforcing the mechanical strength of the glass, and reinforcing the chemical resistance, the Ca ion content is preferably 1.3% or more, more preferably 1.5% or more, further preferably 1.7% or more, further more preferably 1.9% or more, further more preferably 2.1% or more, further more preferably 2.3% or more, further more preferably 2.5% or more, and particularly preferably 2.7% or more. In addition, from the viewpoint of further improving the resistance to devitrification during melting / molding, the Ca ion content is preferably 9.0% or less, more preferably 8.0% or less, further preferably 7.0% or less, further more preferably 6.0% or less, further preferably 5.0% or less, further preferably 4.5% or less, further preferably 4.2% or less, further preferably 3.9% or less, further preferably 3.7% or less, and particularly preferably 3.5% or less. The formal valence of the Ca ion is +2. In one embodiment, from the above viewpoint, it is preferable to set "Ca ion content>Mg ion content" and it is preferable to set "Ca ion content>Sr ion content".

[0071] The Sr ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. From the viewpoint of suppressing the decrease in the liquidus viscosity of the glass, reinforcing the mechanical strength of the glass, and reinforcing the chemical resistance, the Sr ion content is preferably 0.2% or more, more preferably 0.4% or more, further preferably 0.6% or more, further more preferably 0.8% or more, and further more preferably 0.9% or more. In addition, from the viewpoint of further improving the resistance to devitrification during melt molding, the Sr ion content is preferably 4.0% or less, more preferably 3.5% or less, further preferably 3.3% or less, further more preferably 3.1% or less, further preferably 2.7% or less, further preferably 2.5% or less, further preferably 2.3% or less, further preferably 2.1% or less, further preferably 1.9% or less, further preferably 1.7% or less, and particularly preferably 1.5% or less. The formal valence of the Sr ion is +2. In one embodiment, from the above viewpoint, it is preferable that "Sr ion content <Ca ion content" and it is preferable that "Sr ion content <Ba ion content" be satisfied.

[0072] The Ba ion content of the glass may be 0%, 0% or more, or more than 0%. From the viewpoint of suppressing the decrease in the liquidus viscosity of the glass, reinforcing the mechanical strength of the glass, and reinforcing the chemical resistance, the Ba ion content is preferably 1.5% or more, more preferably 2.5% or more, further preferably 2.9% or more, further more preferably 3.1% or more, further more preferably 3.3% or more, and further more preferably 3.5% or more. In addition, from the viewpoint of further improving the devitrification resistance during melting / molding, the Ba ion content is preferably 10.0% or less, more preferably 9.5% or less, further preferably 9.0% or less, further more preferably 8.5% or less, further preferably 8.0% or less, further more preferably 7.5% or less, further more preferably 7.0% or less, further more preferably 6.5% or less, further more preferably 6.0% or less, further more preferably 5.6% or less, further more preferably 5.3% or less, and further more preferably in the order of 5.0% or less, 4.7% or less, 4.5% or less, and 4.3% or less. The formal valence of Ba ion is +2. In one embodiment, from the above viewpoint, it is preferable that "Ba ion content>Ca ion content" and it is preferable that "Ba ion content>Sr ion content".

[0073] The glass contains one or more ions selected from Mg ions, Ca ions, Sr ions, and Ba ions. From the viewpoint of reducing the average valence and improving the visible light transmittance, the total content of Mg ions, Ca ions, Sr ions, and Ba ions is preferably small.

[0074] From the above viewpoints and the viewpoint of further improving solubility, the total content of Mg ions, Ca ions, Sr ions and Ba ions is preferably 20.0% or less, more preferably 19.0% or less, further preferably 18.0% or less, further more preferably 17.5% or less, further preferably 17.0% or less, further preferably 16.5% or less, further more preferably 16.0% or less, further preferably 15.5% or less, further preferably 15.0% or less, further preferably 14.5% or less, further preferably 14.0% or less, and further preferably in the order of 13.5% or less, 13.0% or less, 12.5% ​​or less, 12.0% or less, 11.0% or less, 10.5% or less, and 10.0% or less. In addition, from the viewpoint of suppressing the decrease in liquidus temperature and improving weather resistance, the total content of Mg ions, Ca ions, Sr ions and Ba ions is preferably 3.0% or more, more preferably 4.0% or more, further preferably 4.5% or more, further more preferably 5.0% or more, further preferably 5.5% or more, further preferably 6.0% or more, further preferably 6.5% or more, further preferably 7.0% or more, further preferably 7.5% or more, and further preferably 8.0% or more, 8.5% or more, and 9.0% or more in this order.

[0075] From the viewpoint of suppressing the decrease in viscosity at liquidus temperature, improving mechanical strength and / or suppressing the decrease in glass transition temperature, the cation ratio of the total content of Mg ions, Ca ions, Sr ions and Ba ions to the total content of Li ions, Na ions and K ions ((Mg ions + Ca ions + Sr ions + Ba ions) / (Li ions + Na ions + K ions)) of the above-mentioned glass is 0.100 or more, preferably 0.105 or more, more preferably 0.110 or more, further preferably 0.115 or more, further more preferably 0.120 or more, further preferably 0.125 or more, further preferably 0.130 or more, and further preferably in the order of 0.160 or more, 0.180 or more, 0.200 or more, and 0.220 or more. From the viewpoint of improving the formability of the glass, it is preferred to suppress the decrease in viscosity at liquidus temperature. In addition, from the viewpoint of further improving solubility and / or visible light transmittance, the above-mentioned cation ratio ((Mg ion + Ca ion + Sr ion + Ba ion) / (Li ion + Na ion + K ion)) is preferably 0.650 or less, more preferably 0.620 or less, further preferably 0.590 or less, further more preferably 0.560 or less, further preferably 0.530 or less, further preferably 0.500 or less, further preferably 0.460 or less, further preferably 0.430 or less, further preferably 0.400 or less, further preferably 0.370 or less, and further preferably in the order of 0.350 or less, 0.320 or less, 0.310 or less, 0.300 or less, 0.295 or less, 0.290 or less, 0.287 or less, and 0.285 or less.

[0076] In addition, since the melting temperature of glass can be increased, Cu + The formation becomes easy and the visible light transmittance decreases, so the cation ratio is preferably within the above range.

[0077] The Al ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. From the viewpoint of suppressing the decrease in Tg and improving the mechanical strength and weather resistance, the Al ion content is preferably 1.0% or more, more preferably 1.3% or more, further preferably 1.5% or more, further more preferably 1.7% or more, further preferably 1.9% or more, further preferably 2.1% or more, further preferably 2.3% or more, further preferably 2.5% or more. In addition, from the viewpoint of further improving the solubility of the raw materials and further suppressing the Cu +From the viewpoint of the formation of the Al ion, the Al ion content is preferably 8.0% or less, more preferably 7.0% or less, further preferably 6.5% or less, further more preferably 6.0% or less, further preferably 5.5% or less, further preferably 5.3% or less, further preferably 5.0% or less, further preferably 4.7% or less, further preferably 4.5% or less, further preferably 4.0% or less, 2.5% or less, 2.0% or less. The formal valence of the Al ion is +3. From the viewpoint of reducing the average valence and improving the visible light transmittance, it is also preferred that the Al ion content is small.

[0078] From the viewpoint of improving the thermal stability and mechanical strength of the glass, the total content of Al ions and P ions (Al ions + P ions) of the above-mentioned glass is preferably 40.0% or more, more preferably 41.0% or more, further preferably 42.0% or more, further more preferably 42.5% or more, further preferably 43.0% or more, further preferably 44.0% or more, further preferably 44.5% or more, further preferably 45.0% or more. In addition, from the viewpoint of further improving the solubility of the raw materials and further suppressing the Cu + From the perspective of the generation of, the above-mentioned total content (Al ions + P ions) is preferably 55.0% or less, more preferably 54.0% or less, further preferably 53.0% or less, further more preferably 52.0% or less, further preferably 51.0% or less, further preferably 50.0% or less, further preferably 49.5% or less, further preferably 49.0% or less, further preferably 48.5% or less, further preferably 48.0% or less, further preferably 47.0% or less, 46.5% or less, 46.2% or less, and 46.0% or less.

[0079] The Zn ion content of the above-mentioned glass may be 0%, 0% or more, or more than 0%. From the viewpoint of lowering the Tg of the glass, as for the Zn ion content, Zn may be introduced to replace the above-mentioned Mg and / or Ca and / or Sr and / or Ba within a range that does not significantly affect the effects exerted by the various components. However, from the viewpoint of improving weather resistance, the Zn ion content is preferably 8.7% or less, more preferably 8.5% or less, further preferably 8.3% or less, further more preferably 8.0% or less, further preferably 7.7% or less, further preferably 7.5% or less, further preferably 7.3% or less, further preferably 7.1% or less, further preferably 6.5% or less, further preferably 6.0% or less, and further preferably in the order of 5.5% or less, 5.0% or less, 4.0% or less, 3.0% or less, 2.0% or less, and 1.0% or less. The formal valence of the Zn ion is +2.

[0080] From the viewpoint of improving weather resistance, the cation ratio of Zn ions to the total content of Mg ions, Ca ions, Sr ions, Ba ions and Zn ions in the above-mentioned glass (Zn ions / (Mg ions + Ca ions + Sr ions + Ba ions + Zn ions)) is preferably 0.600 or less, more preferably 0.580 or less, further preferably 0.570 or less, further more preferably 0.560 or less, and further preferably in the order of 0.550 or less, 0.540 or less, 0.530 or less, 0.520 or less, 0.510 or less, 0.505 or less, 0.500 or less, 0.498 or less, 0.496 or less, 0.400 or less, 0.300 or less, 0.200 or less, 0.100 or less, 0.080 or less, 0.060 or less, 0.040 or less, and 0.020 or less. In addition, the above-mentioned cation ratio (Zn ion / (Mg ion+Ca ion+Sr ion+Ba ion+Zn ion)) may be 0 or 0.000.

[0081] From improving the solubility of raw materials and inhibiting Cu + From the perspective of the formation of, the cation ratio of the total content of Al ions and P ions in the above-mentioned glass to the total content of Mg ions, Ca ions, Sr ions, Ba ions, Zn ions and Cu ions ((Al ions + P ions) / (Mg ions + Ca ions + Sr ions + Ba ions + Zn ions + Cu ions)) is 5.3 or less, preferably 5.1 or less, more preferably 4.9 or less, further preferably 4.7 or less, further more preferably 4.5 or less, and further preferably in the order of 4.3 or less, 4.1 or less, 3.9 or less, 3.7 or less, 3.5 or less, 3.3 or less, and 3.1 or less. In addition, from the viewpoint of improving the thermal stability and mechanical strength of the glass, the above-mentioned cation ratio ((Al ions + P ions) / (Mg ions + Ca ions + Sr ions + Ba ions + Zn ions + Cu ions)) is preferably greater than 1.6, more preferably greater than 1.63, further preferably greater than 1.65, and further preferably greater than 1.68, greater than 1.7, greater than 1.75, greater than 1.8, greater than 1.85, greater than 2.00, greater than 2.20, greater than 2.40, greater than 2.60, and greater than 2.80 in the order of greater than 1.68, greater than 1.7, greater than 1.75, greater than 1.8, greater than 1.85, greater than 2.00, greater than 2.20, greater than 2.40, greater than 2.60, and greater than 2.80.

[0082] The above glass may further optionally contain one or more of the following cations as cations.

[0083] The introduction of a small amount of rare earth ions such as Y ions, La ions, Gd ions, and Yb ions into the glass can contribute to further improvement of weather resistance, improvement of chemical resistance, suppression of reduction in glass transition temperature, and / or suppression of reduction in viscosity at liquidus temperature. The content of these rare earth ions can be 0%, 0% or more, or more than 0%, or less than 3.0%, less than 2.0%, less than 1.0%, or less than 0.5%. The formal valence of Y ions, La ions, Gd ions, and Yb ions is +3.

[0084] Ti, Zr, Nb, W, and Bi are components which contribute to improving the weather resistance and chemical resistance of glass and to suppressing a decrease in Tg and a decrease in liquidus viscosity by adding a small amount thereof.

[0085] The Ti ion content may be 0%, 0% or more, or more than 0%, preferably 3.0% or less, more preferably 2.0% or less, further preferably 1.0% or less, and further more preferably 0.5% or less. The formal valence of the Ti ion is +4.

[0086] The Zr ion content may be 0%, 0% or more, or more than 0%, preferably 3.0% or less, more preferably 2.0% or less, further preferably 1.0% or less, and further more preferably 0.5% or less. The formal valence of Zr ions is +4.

[0087] The Nb ion content may be 0%, 0% or more, or more than 0%, preferably 3.0% or less, more preferably 2.0% or less, further preferably 1.0% or less, and further more preferably 0.5% or less. The formal valence of the Nb ion is +5.

[0088] The W ion content may be 0%, 0% or more, or more than 0%, preferably 3.0% or less, more preferably 2.0% or less, further preferably 1.0% or less, and further more preferably 0.5% or less. The formal valence of the W ion is +6.

[0089] The Bi ion content may be 0%, 0% or more, or more than 0%, preferably 3.0% or less, more preferably 2.0% or less, further preferably 1.0% or less, and further more preferably 0.5% or less. The formal valence of the Bi ion is +3.

[0090] From the viewpoint of improving visible light transmittance, the average valence of cations other than Cu ions and P ions in the above-mentioned glass is less than 1.500, preferably less than 1.490, more preferably less than 1.480, further preferably less than 1.470, further more preferably less than 1.460, further preferably less than 1.450, further preferably less than 1.440, further preferably less than 1.430, and further preferably less than 1.420, less than 1.410, less than 1.400, less than 1.390, less than 1.380, less than 1.370, less than 1.360, and less than 1.350 in this order. In addition, from the viewpoint of suppressing the decrease in viscosity at the liquidus temperature, the average valence of cations other than Cu ions and P ions is preferably 1.100 or more, more preferably 1.1500 or more, further preferably 1.200 or more, further preferably 1.250 or more, further more preferably 1.270 or more, further preferably 1.280 or more, further preferably 1.290 or more, further preferably 1.300 or more. For example, when the thickness of the glass or the wavelength at which the transmittance is 50% is adjusted to change the Cu concentration, the composition may be readjusted with reference to the above average valence.

[0091] The above average valence can be obtained as the value obtained by dividing the sum of "the content of each cation in cation % × the formal valence of its cation" by the sum of the content of cations in cation % other than Cu and P, for cations other than Cu and P. For example, for a glass containing A cations (formal valence a, content A% in cation %), B cations (formal valence b, content B% in cation %) and C cations (formal valence c, total content C% in cation %) in addition to Cu and P ions, the above average valence is obtained as "(A×a+B×b+C×c) / (A+B+C)".

[0092] For the above-mentioned glass, when the thickness of the glass and the wavelength at which the transmittance is 50% are adjusted to change the Cu concentration, the average valence of Cu ions may also be referred to. With regard to cations other than P ions only (therefore including Cu ions), from the viewpoint of further improving the visible light transmittance, the average valence of cations obtained in the same manner as above is preferably 1.550 or less, more preferably 1.540 or less, further preferably 1.530 or less, further more preferably 1.520 or less, further preferably 1.510 or less, and further preferably 1.500 or less, and further preferably in the order of 1.490 or less, 1.480 or less, 1.470 or less, 1.460 or less, 1.450 or less, 1.440 or less, 1.430 or less, 1.420 or less, 1.410 or less, and 1.400 or less. In addition, from the viewpoint of suppressing the decrease in viscosity at the liquidus temperature, the average valence of cations other than P ions alone is preferably 1.300 or more, more preferably 1.310 or more, further preferably 1.320 or more, further more preferably 1.330 or more, further preferably 1.340 or more, further preferably 1.350 or more, and further preferably 1.360 or more.

[0093] (Anion type)

[0094] The glass contains O ions as constituent ions. From the viewpoint of facilitating homogenization during glass melting and improving productivity, the O ion content is 85.0% or more, preferably 90.0% or more, more preferably 95.0% or more, further preferably 98.0% or more, and further more preferably 99.0% or more. In particular, from the viewpoint of suppressing volatilization during glass melting, improving productivity, and suppressing the generation of harmful gases during manufacturing, the O ion content is preferably 100%. It should be noted that the formal valence of the O ion is -2.

[0095] The glass may contain only O ions as anions in one embodiment, and may contain one or more other anions in addition to O ions in another embodiment. Other anions include F ions, Cl ions, Br ions, I ions, etc. It should be noted that the formal valence of F ions, Cl ions, Br ions, and I ions is -1.

[0096] From the viewpoint of improving the homogeneity and strength of the glass, the content of F ions is preferably 15.0% or less, more preferably 10.0% or less, further preferably 5.0% or less, further more preferably 2.0% or less, and further preferably 1.0% or less. In particular, from the viewpoint of suppressing volatilization during glass melting, improving productivity, and suppressing the generation of harmful gases during manufacturing, F ions may not be contained.

[0097] From the viewpoint of improving weather resistance, the ratio of the O ion content to the P ion content of the above-mentioned glass (O ion / P ion) is 3.300 or more, preferably 3.310 or more, more preferably 3.320 or more, further more preferably 3.330 or more, and further preferably in the order of 3.340 or more, 3.350 or more, 3.360 or more, 3.370 or more, 3.380 or more, 3.390 or more, 3.400 or more, 3.410 or more, 3.420 or more, 3.430 or more, 3.440 or more, 3.450 or more, and 3.460 or more. In addition, from the viewpoint of further improving the resistance to devitrification during melting / molding of the glass and the near-infrared cutting ability, the above ratio (O ion / P ion) is preferably 3.580 or less, more preferably 3.570 or less, further preferably 3.560 or less, further more preferably 3.550 or less, further preferably 3.540 or less, and still further preferably 3.530 or less, and further preferably in the order of 3.520 or less, 3.510 or less, 3.500 or less, and 3.490 or less.

[0098] The glass is preferably basically composed of the above components, but may contain other components within a range that does not hinder the effects of the above components. In addition, the glass may contain inevitable impurities.

[0099] Pb, As, Cd, Tl, Be, and Se are all toxic. Therefore, the glass preferably does not contain these elements as glass components.

[0100] U, Th, and Ra are all radioactive elements. Therefore, the glass preferably does not contain these elements as glass components.

[0101] V, Cr, Mn, Fe, Co, Ni, Pr, Nd, Pm, Sm, Eu, Tb, Dy, Ho, Er, Tm, and Ce can increase the coloring of the glass and become a source of fluorescence. Therefore, in the above-mentioned glass, the total content of these elements in terms of oxide conversion on an oxide glass basis is preferably set to 10 mass ppm or less, and it is more preferable that these elements are not contained as glass components.

[0102] Ge, Ta, and Gd are expensive raw materials, and therefore, the glass preferably does not contain these elements as glass components.

[0103] Sb (Sb2O3), Sn (SnO2), Ce (CeO2), and SO3 are elements that can be optionally added and function as clarifiers. Among them, Sb (Sb2O3) is a clarifier with a significant clarification effect.

[0104] Sn (SnO2) and Ce (CeO2) have a smaller clarification effect than Sb (Sb2O3). If these clarifiers are added in large amounts, there is a tendency to cause the coloring of the glass to become stronger. Therefore, when adding clarifiers, it is preferred to add Sb (Sb2O3) while taking into account the effect of coloring caused by the addition.

[0105] The contents of the components that can function as a clarifier described below are values ​​converted into oxides.

[0106] The content of Sb2O3 is expressed as a percentage of addition. That is, when the total content of all glass components other than Sb2O3, SnO2, CeO2 and SO3 in terms of oxide is set to 100.0 mass%, the content of Sb2O3 can be less than 1.0 mass%, less than 0.5 mass%, less than 0.3 mass%, less than 0.2 mass%, less than 0.15 mass%, less than 0.1 mass% or less than 0.1 mass% in one embodiment. In one embodiment, the content of Sb2O3 can be 0 mass%. In another embodiment, the content of Sb2O3 can exceed 0 mass%. By suppressing the formation of Cu in the melt, the content of Sb2O3 can be reduced to 0 mass%. 2+ From the viewpoint of improving visible light transmittance by coloring due to reduction, the Sb2O3 content is preferably greater than 0 mass%, and is more preferably in the order of 0.01 mass% or more, 0.03 mass% or more, 0.05 mass% or more, 0.08 mass% or more, and 0.10 mass% or more.

[0107] The content of SnO2 is also expressed as an added ratio. That is, when the total content of all glass components other than SnO2, Sb2O3, CeO2 and SO3 in terms of oxides is set to 100.0 mass%, the content of SnO2 is preferably less than 2.0 mass%, more preferably less than 1.0 mass%, further preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of SnO2 may also be 0 mass%. By making the content of SnO2 within the above range, the clarity of the glass can be improved.

[0108] The content of CeO2 is also expressed as an added ratio. That is, when the total content of all glass components other than CeO2, Sb2O3, SnO2 and SO3 in terms of oxide is set to 100.0 mass%, the content of CeO2 is preferably less than 2.0 mass%, more preferably less than 1.0 mass%, further preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of CeO2 may also be 0 mass%. By making the content of CeO2 within the above range, the clarity of the glass can be improved.

[0109] The content of SO3 is also expressed as the added ratio. 3、When the total content of all glass components other than Sb2O3, SnO2, and CeO2 in terms of oxides is set to 100.0 mass%, the content of SO3 is preferably less than 2.0 mass%, more preferably less than 1.0 mass%, further preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of SO3 may also be 0 mass%. By setting the content of SO3 to the above range, the clarity of the glass can be improved.

[0110] <Glass Properties>

[0111] (Transmittance characteristics)

[0112] The glass is suitable as a glass for a near infrared cut filter. The near infrared cut capability can be determined by the wavelength at which the spectral transmittance is 50% at a wavelength of 600 nm or longer, i.e., the half value, or by the transmittance T1200 at a wavelength of 1200 nm.

[0113] In addition, the above-mentioned glass can also show high visible light transmittance. Regarding the visible light transmittance, the transmittance T400 at a wavelength of 400 nm can be used as an index.

[0114] As will be described in detail later, the glass can be used as glass for a near-infrared cut filter having a thickness of 0.25 mm or less in one embodiment.

[0115] As a glass (glass I) suitable for a thinner near-infrared cutoff filter within the above-mentioned thickness range, as a transmittance characteristic converted to a thickness of 0.11 mm, the half value is preferably below 650nm, and further preferably below 647nm, below 645nm, below 643nm, below 641nm, below 640nm, below 639nm, and below 638nm.

[0116] Regarding glass I, as a transmittance characteristic converted to a thickness of 0.11 mm, the half value is preferably above 600 nm, and more preferably in the order of above 610 nm, above 613 nm, above 615 nm, above 617 nm, above 620 nm, above 623 nm, above 625 nm, and above 628 nm.

[0117] Regarding glass I, as the transmittance characteristics converted to a thickness of 0.11 mm, the transmittance T1200 at a wavelength of 1200 nm is preferably 42.0% or less, and further preferably in the order of 41.0% or less, 40.0% or less, 39.0% or less, 38.5% or less, 38.0% or less, 37.5% or less, 37.0% or less, 36.5% or less, 36.0% or less, 35.5% or less, and 35.0% or less.

[0118] Regarding glass I, as a transmittance characteristic converted to a thickness of 0.11 mm, the transmittance T1200 at a wavelength of 1200 nm can be, for example, greater than 10.0%, greater than 12.0% or greater than 14.0%. Since a lower transmittance can mean a better near-infrared cutoff ability, it is also preferably lower than the above-mentioned example values.

[0119] In addition, as glass I, as the transmittance characteristics converted to a thickness of 0.11 mm, the transmittance T400 at a wavelength of 400 nm is preferably 68.0% or more, more preferably 70.0% or more, and further more preferably 71.0% or more, 72.0% or more, 73.0% or more, 74.0% or more, 75.0% or more, 76.0% or more, 77.0% or more, 78.0% or more, 79.0% or more, and 80.0% or more.

[0120] Regarding glass I, as a transmittance characteristic converted to a thickness of 0.11 mm, the transmittance T400 at a wavelength of 400 nm can be, for example, less than 98.0%, less than 97.0% or less than 96.0%. Since a higher transmittance can mean better visible light transmittance, it is also preferably higher than the above-mentioned example values.

[0121] In addition, as a glass (glass II) suitable for a thicker near-infrared cutoff filter within the above-mentioned thickness range, as a transmittance characteristic converted to a thickness of 0.21 mm, the half value is preferably below 650nm, and further preferably below 647nm, below 645nm, below 643nm, below 641nm, below 640nm, below 639nm, and below 638nm.

[0122] Regarding glass II, as the transmittance characteristic converted to a thickness of 0.21 mm, the half value is preferably above 600 nm, and more preferably in the order of above 610 nm, above 613 nm, above 615 nm, above 617 nm, above 620 nm, above 623 nm, above 625 nm, and above 628 nm.

[0123] Regarding glass II, as the transmittance characteristics converted to a thickness of 0.21 mm, the transmittance T1200 at a wavelength of 1200 nm is preferably less than 42.0%, and further preferably less than 41.0%, less than 40.0%, less than 39.0%, less than 38.5%, less than 38.0%, less than 37.5%, less than 37.0%, less than 36.5%, less than 36.0%, less than 35.5%, and less than 35.0%.

[0124] Regarding glass II, as a transmittance characteristic converted to a thickness of 0.21 mm, the transmittance T1200 at a wavelength of 1200 nm can be, for example, above 10.0%, above 12.0% or above 14.0%. Since a lower transmittance means a better near-infrared cutoff ability, it is also preferably lower than the above-mentioned example value.

[0125] In addition, as glass II, as the transmittance characteristics converted to a thickness of 0.21 mm, the transmittance T400 at a wavelength of 400 nm is preferably 68.0% or more, more preferably 70.0% or more, and further preferably 71.0% or more, 72.0% or more, 73.0% or more, 74.0% or more, 75.0% or more, 76.0% or more, 77.0% or more, 78.0% or more, 79.0% or more, and 80.0% or more.

[0126] Regarding glass II, as a transmittance characteristic converted to a thickness of 0.21 mm, the transmittance T400 at a wavelength of 400 nm can be, for example, less than 98.0%, less than 97.0% or less than 96.0%. Since a higher transmittance means better visible light transmittance, it is also preferably higher than the above-mentioned example values.

[0127] The above-mentioned transmittance characteristics are values ​​obtained by the following method.

[0128] The glass sample was processed so as to have parallel and optically polished planes, and the external transmittance at a wavelength of 200 to 1200 nm was measured. It should be noted that the external transmittance also includes the reflection loss of light on the test surface.

[0129] The intensity of light incident vertically on one plane after optical polishing is defined as intensity A, and the intensity of light emitted from the other plane is defined as intensity B, and the spectral transmittance B / A is calculated. The wavelength at which the spectral transmittance is 50% for wavelengths above 600 nm is defined as the half-value λ. T 50. The spectral transmittance at a wavelength of 400 nm is set to T400, and the spectral transmittance at a wavelength of 1200 nm is set to T1200. In addition, when the glass to be measured is not glass of the converted thickness, the thickness of the glass can be set to d, and the transmittance at each wavelength λ can be converted by the following formula, and the half value λ can be calculated based on the converted transmittance characteristics. T Conversion values ​​of T50, T400 and T1200.

[0130] T(λ)=(1-R(λ)) 2 ×exp(log e ((T0(λ) / 100) / (1-R(λ)) 2 )×d / d0)×100

[0131] Where, T(λ): converted transmittance at wavelength λ (%), T0(λ): measured transmittance at wavelength λ (%), d: glass thickness (mm), d0: converted thickness (mm), R(λ) = ((n(λ) - 1) / (n(λ) + 1)) 2 represents the reflectivity at a wavelength λ, and n(λ): the refractive index at a wavelength λ. Here, calculations were performed assuming that n(λ)=1.51680 and R(λ)=0.042165 are constants.

[0132] (Weather resistance)

[0133] The glass having the above-described composition can exhibit excellent weather resistance. For example, the weather resistance can be evaluated by the method described in the examples described later as an index, and the evaluation result is preferably ◎ or ○, and more preferably ◎.

[0134] (Solubility)

[0135] The glass having the above-described composition can also exhibit excellent solubility. Regarding the solubility, for example, the evaluation result of the solubility evaluated by the method described in the Examples described later can be used as an index, and the evaluation result is preferably ○.

[0136] (Glass transition temperature Tg, convergence temperature Tm of endothermic reaction)

[0137] The glass transition temperature of the above-mentioned glass is not particularly limited. From the viewpoint of imparting processability and / or heat resistance in subsequent steps, Tg is preferably 300°C or higher, and more preferably 310°C or higher, 320°C or higher, 330°C or higher, 340°C or higher, and 350°C or higher in this order.

[0138] On the other hand, from the viewpoint of reducing the burden on the annealing furnace and the molding device, Tg is preferably 500°C or less, and further preferably in the order of 490°C or less, 480°C or less, 470°C or less, 460°C or less, 450°C or less, 440°C or less, 430°C or less, 420°C or less, 410°C or less, 400°C or less, and 390°C or less.

[0139] The convergence temperature Tm of the endothermic reaction of the above-mentioned glass is not particularly limited, and there is a tendency that the lower the Tm, the better the solubility. In addition, there is a tendency that the better the solubility, the more the visible light transmittance of the glass can be improved. From these viewpoints, Tm is preferably below 870°C, and further preferably in the order of below 860°C, below 850°C, below 840°C, below 830°C, below 820°C, below 810°C, below 800°C, below 790°C, below 780°C, below 770°C, below 760°C, and below 750°C.

[0140] (proportion)

[0141] The near infrared cut filter is preferably lightweight because it contributes to the lightness of the element or device provided with the filter. From this point of view, the specific gravity of the glass is preferably 3.50 or less, and more preferably 3.45 or less, 3.40 or less, 3.35 or less, 3.30 or less, 3.25 or less, 3.20 or less, 3.15 or less, 3.10 or less, and 3.05 or less.

[0142] The specific gravity may be, for example, 2.5 or more or 2.6 or more. From the above viewpoint, the specific gravity is preferably lower, and therefore, it is also preferably lower than the values ​​exemplified here.

[0143] <Glass Manufacturing Method>

[0144] The above-mentioned glass can be obtained by mixing, melting and molding various glass raw materials. For the production method, reference can also be made to the description described below.

[0145] The near-infrared absorbing glass is suitable as glass for near-infrared cut-off filters. In addition, the near-infrared absorbing glass can also be applied to optical elements (lenses, etc.) other than near-infrared cut-off filters, and can also be applied to various glass products and can be variously deformed.

[0146] [Near infrared cut filter]

[0147] One embodiment of the present invention relates to a near infrared cut filter (hereinafter, also simply referred to as a “filter”) made of the above-mentioned near infrared absorbing glass.

[0148] The glass constituting the above-mentioned optical filter is as described above.

[0149] A specific example of the method for producing the optical filter will be described below, but the following production method is for illustrative purposes only and does not limit the present invention.

[0150] For molten glass, glass raw materials such as phosphates, oxides, carbonates, nitrates, sulfates, and fluorides are appropriately used, and the raw materials are weighed and mixed in a manner to achieve the desired composition, and then melted in a melting container such as a platinum crucible, for example, at 800°C to 1000°C. At this time, in order to suppress the volatilization of volatile components, a lid such as platinum can also be used. In addition, the melting can be carried out in the atmosphere, and in order to suppress the change in the valence of Cu, an oxygen atmosphere can also be formed, or oxygen bubbling can be carried out in the molten glass. The glass in the molten state becomes a homogenized molten glass with fewer bubbles (preferably without bubbles) by stirring and clarifying.

[0151] After stirring and clarifying the molten glass, the glass is made to flow out and formed into a desired shape. When the glass is made to flow out, it is preferred that the glass is cooled to a temperature near the liquidus temperature and the viscosity of the glass is increased, so that convection of the flowing glass is not easy to occur and wave lines are not easy to occur.

[0152] As a glass forming method, known methods such as casting, pipe outflow, rolling, pressing, etc. can be used. The formed glass is transferred to an annealing furnace preheated to near the glass transition temperature and slowly cooled to room temperature. In this way, a near infrared cutoff filter can be manufactured.

[0153] An example of a molding method is described below. A mold consisting of a flat and horizontal bottom surface, a pair of side walls sandwiching the bottom surface and facing each other in parallel, and a weir plate located between the pair of side walls and closing one side opening is prepared. Homogenized molten glass is injected into the mold at a constant outflow rate from a platinum alloy pipe. The cast molten glass is spread out in the mold and molded into a glass plate that is limited to a certain width by a pair of side walls. The molded glass plate is continuously pulled out from the opening of the mold. Here, by appropriately setting the molding conditions such as the shape, size, and outflow rate of the molten glass of the mold, it is possible to mold a large and thick glass block. The molded glass mold is transferred to an annealing furnace preheated to near the glass transition temperature and slowly cooled to room temperature. The glass molded body after the strain is removed by slow cooling is subjected to mechanical processing such as slicing, grinding, and polishing. In this way, a near-infrared cutoff filter in a shape corresponding to the purpose, such as a plate shape or a lens shape, can be obtained. Alternatively, a method may be adopted in which a preform made of the above glass is formed, heated, softened, and then press-formed (particularly, a precision press-forming method in which the final product is press-formed without subjecting the optical functional surface to mechanical processing such as grinding and polishing). An optical multilayer film may also be formed on the surface of the optical filter as required.

[0154] The near infrared cut filter can have both excellent near infrared cut capability and high visible light transmittance. With such a near infrared cut filter, the color sensitivity of the semiconductor imaging element can be well corrected.

[0155] In addition, the near infrared cut filter can be applied to a camera device by combining it with a semiconductor image sensor. The semiconductor image sensor has a semiconductor imaging element such as a CCD or CMOS installed in the component, and the light receiving part is covered by a light-transmitting member. The light-transmitting member can be used as a near infrared cut filter at the same time, or the light-transmitting member and the near infrared cut filter can be different members.

[0156] The imaging device may include an optical element such as a lens or a prism on the light receiving surface of the semiconductor image sensor for forming an image of the object to be imaged.

[0157] Furthermore, according to the above-mentioned near infrared cut filter, it is possible to provide an imaging device capable of performing color sensitivity correction well and obtaining an image with excellent image quality.

[0158] The above-mentioned near-infrared cut-off filter can be a near-infrared cut-off filter with a thickness of less than 0.25mm in one embodiment. In recent years, due to the emergence of smart phones, the tendency to reduce the thickness of the camera of the imaging element is significant, and with this, the near-infrared cut-off filter is also expected to exert performance with a thinner thickness. As such a near-infrared cut-off filter, the above-mentioned near-infrared cut-off filter is also preferred. The thickness of the above-mentioned near-infrared cut-off filter can be less than 0.24mm, less than 0.23mm, less than 0.22mm, less than 0.21mm, less than 0.20mm, less than 0.19mm, less than 0.18mm, less than 0.17mm, less than 0.16mm, less than 0.15mm, less than 0.14mm, less than 0.13mm or less than 0.12mm. The thickness of the above-mentioned near-infrared cut-off filter can be, for example, 0.21mm or 0.11mm. In addition, the thickness of the near infrared cut filter can be, for example, 0.50 mm or more, but is not limited thereto. In the present invention and this specification, "thickness" refers to the thickness of the sample in the area where the transmittance is measured, and can be measured by a thickness gauge, a micrometer, etc. For example, the thickness of the approximate center of the position where the transmitted light passes can be measured, or the thickness of multiple points can be measured within the light spot of the transmitted light and the average value can be taken.

[0159] The near infrared cutoff capability of the near infrared cutoff filter is preferably 0.2000 mol / m from the viewpoint of obtaining a near infrared cutoff filter having a more excellent near infrared cutoff capability. 2 Above, further 0.2100 mol / m2 Above, 0.2200mol / m 2 Above, 0.2300mol / m 2 Above, 0.2400mol / m 2 Above, 0.2500mol / m 2 Above, 0.2600mol / m 2 Above, 0.2700mol / m 2 Above, 0.2800mol / m 2 Above, 0.2900mol / m 2 Above, 0.3000mol / m 2 Above, 0.3100mol / m 2 Above, 0.3150mol / m 2 Above, 0.3200mol / m 2 Above, 0.3250mol / m 2 The above order is more preferable.

[0160] In addition, from the viewpoint of obtaining a near-infrared cut filter showing a higher visible light transmittance, the value calculated by "thickness x Cu concentration" is preferably 1.000 mol / m 2 Below, further 0.9800 mol / m 2 Below, 0.9600mol / m 2 Below, 0.9400mol / m 2 Below, 0.9200mol / m 2 Below, 0.9000mol / m 2 Below, 0.8800mol / m 2 Below, 0.8600mol / m 2 Below, 0.8400mol / m 2 Below, 0.8200mol / m 2 Below, 0.8000mol / m 2 Below, 0.7800mol / m 2 Below, 0.7600mol / m 2 Below, 0.7400mol / m 2 Below, 0.7200mol / m 2 Below, 0.7000mol / m 2 Below, 0.6800mol / m 2 Below, 0.6600mol / m 2 Below, 0.6400mol / m 2 Below, 0.6200mol / m 2Below, 0.6000mol / m 2 Below, 0.5800mol / m 2 Below, 0.5600mol / m 2 Below, 0.5400mol / m 2 Below, 0.5200mol / m 2 Below, 0.5000mol / m 2 Below, 0.4800mol / m 2 Below, 0.4600mol / m 2 Below, 0.4800mol / m 2 Below, 0.4200mol / m 2 Below, 0.4100mol / m 2 Below, 0.4000mol / m 2 Below, 0.3900mol / m 2 Below, 0.3800mol / m 2 Below, 0.3700mol / m 2 Below, 0.3600mol / m 2 Below, 0.3500mol / m 2 The following order is more preferred.

[0161] The calculation method of the above-mentioned “thickness×Cu concentration” will be described.

[0162] "Thickness x Cu concentration" =

[0163] (Specific gravity of its composition) / (Molecular weight of its composition)×(Cation % of Cu ions / 100)×d / 10×10 4

[0164] The unit is mol / m 2 , d is the thickness (mm).

[0165] Regarding (molecular weight of its composition) in the above formula, the calculation method is described.

[0166] (Molecular weight of the composition) is a value obtained by summing up (molecular weight of each component based on cations)×(cation % of each component / 100) of all components constituting the composition, and the unit is g / mol.

[0167] In addition, regarding the above-mentioned (molecular weight of each component based on cations), the calculation method is described. (Molecular weight of each component based on cations) = (atomic weight of the element forming its cation) + (atomic weight of oxygen × coefficient corresponding to the valence)

[0168] The coefficients corresponding to the valence are as follows.

[0169] If the formal valence is +1, the coefficient is 0.5

[0170] If the formal valence is +2, the coefficient is 1.0

[0171] If the formal valence is +3, the coefficient is 1.5

[0172] If the formal valence is +4, the coefficient is 2.0

[0173] If the formal valence is +5, the coefficient is 2.5

[0174] If the formal valence is +6, the coefficient is 3.0

[0175] Regarding the transmittance characteristics of the near infrared cut filter, the above description related to glass I and glass II can be referred to. In addition, regarding the physical properties of the near infrared cut filter, the above description related to the near infrared absorbing glass can also be referred to.

[0176] Example

[0177] Hereinafter, the present invention will be described in more detail with reference to the examples, but the present invention is not limited to the examples.

[0178] [Examples 1 to 81, Comparative Examples A to F]

[0179] As glass raw materials, phosphates, fluorides, carbonates, nitrates, oxides, etc. are weighed and mixed in such a way that 150 g to 300 g of glass of the composition shown in Table 1 can be obtained, and then placed in a platinum crucible or a quartz crucible, melted at 800°C to 1000°C for 60 minutes to 180 minutes, stirred to degas and homogenize, and then poured into a preheated mold and formed into a given shape. The obtained glass molding is transferred to an annealing furnace heated to near the glass transition temperature and slowly cooled to room temperature. A test piece is cut out from the obtained glass, and after mirror polishing on both sides to a thickness of about 0.2 mm, various evaluations are performed by the following methods.

[0180] [Evaluation method]

[0181] <Transmittance characteristics>

[0182] The transmittance of each test piece at a wavelength of 200 to 1200 nm was measured using a spectrophotometer. Based on the measurement results, the half value (unit: nm), the transmittance T1200 (unit: %) at a wavelength of 1200 nm, and the transmittance T400 (unit: %) at a wavelength of 400 nm were calculated by converting the values ​​into a thickness of 0.11 mm or a thickness of 0.21 mm.

[0183] <Glass transition temperature Tg, convergence temperature Tm of endothermic reaction>

[0184] The glass transition temperature Tg and the temperature Tm at which the endothermic reaction due to melting converged were measured at a temperature increase rate of 10°C / min using a differential scanning calorimeter (DSC8270) manufactured by Rigaku Corporation.

[0185] <Specific Gravity>

[0186] The specific gravity was measured by the Archimedean method.

[0187] <Weather resistance>

[0188] Each test piece was kept in a constant temperature and humidity chamber at a temperature of 85°C and a relative humidity of 85% for 168 hours. Then, each test piece was visually evaluated under a fluorescent lamp. Based on the evaluation results, weather resistance was evaluated according to the following criteria.

[0189] ◎: No denaturation was observed on the surface.

[0190] ○: Fogging was observed on the surface, but no deliquescence was observed.

[0191] ×: Deliquescence occurred.

[0192] <Meltability>

[0193] Using the same formula as the glass raw material used for the preparation of the test piece, the raw materials (mixture) were weighed and mixed to obtain only 200 g of glass after melting, and then placed in a platinum crucible or a silica glass crucible and melted at 1000° C. for 60 minutes. The results of visual observation were evaluated as "○" when a molten liquid was obtained without unmelted liquid, and "×" when unmelted liquid was present.

[0194] The above results are shown in Table 1 (Table 1-1 to Table 1-6), Table 2 (Table 2-1 to Table 2-6), and Table 3 (Table 3-1 to Table 3-6. In the tables, the unit of the (total) content of cations is cation %, and the unit of the (total) content of anions is anion %.

[0195]

[0196]

[0197]

[0198]

[0199]

[0200]

[0201]

[0202]

[0203]

[0204]

[0205]

[0206]

[0207]

[0208]

[0209]

[0210]

[0211]

[0212]

[0213] As glass raw materials, phosphates, fluorides, carbonates, nitrates, oxides, etc. are weighed and mixed in such a way that 150 g to 300 g of glass having a composition of Example 64 in Table 1 containing Sb2O3 expressed as 0.080 mass % as an external addition ratio is obtained, and then put into a platinum crucible or a quartz crucible, melted under the same melting conditions as Example 64, and stirred to degas and homogenize, and then poured into a preheated mold and formed into a given shape. The obtained glass molding is transferred to an annealing furnace heated to near the glass transition temperature and slowly cooled to room temperature. A test piece is cut out from the obtained glass, and after mirror polishing on both sides to a thickness of about 0.2 mm, the transmittance characteristics are evaluated by the above method. The evaluation results are: based on the value at a thickness of 0.11 mm (converted), the transmittance T1200 at a wavelength of 1200 nm is 27.9%, and the transmittance T400 at a wavelength of 400 nm is 87.4%. By comparing the above evaluation results with the evaluation results of Example 64, it can be confirmed that the addition of Sb2O3 can suppress coloring and improve the visible light transmittance.

[0214] Finally, the above methods are summarized.

[0215] According to one embodiment, there is provided a near-infrared absorbing glass comprising at least P ions, Cu ions, O ions, one or more ions selected from Li ions, Na ions, and K ions, and one or more ions selected from Mg ions, Ca ions, Sr ions, and Ba ions as constituent ions, wherein, in the glass composition expressed as cation %, the content of Cu ions is 15.0 cation % or less, the content of P ions is 55.0 cation % or less, and the cation ratio of the total content of Al ions and P ions to the total content of Mg ions, Ca ions, Sr ions, Ba ions, Zn ions, and Cu ions ((Al ions + P ions) / (Mg ions + Ca ions)) is 1.5 cation %. The glass composition is expressed in terms of anion %, the content of O ions is more than 85.0 anion %, and the ratio of the content of O ions to the content of P ions (O ions / P ions) is more than 3.300.

[0216] The glass may be a near-infrared absorbing glass having excellent near-infrared cutting capability, high visible light transmittance, and excellent weather resistance and solubility.

[0217] In one embodiment, in the glass composition represented by cation % of the glass, the content of P ions may be 30.0 cation % or more and 50.0 cation % or less.

[0218] In one embodiment, in the glass composition represented by cation % of the glass, the content of Li ions may be 10.0 cation % or more.

[0219] In one embodiment, in the glass composition represented by cation % of the glass, a content of Cu ions may be 2.1 cation % or more and 15.0 cation % or less.

[0220] In one embodiment, the ratio (O ion / P ion) may be 3.400 or more.

[0221] In one embodiment, in the glass composition of the above-mentioned glass expressed as cation %, the cation ratio of Zn ions to the total content of Mg ions, Ca ions, Sr ions, Ba ions and Zn ions (Zn ions / (Mg ions+Ca ions+Sr ions+Ba ions+Zn ions)) can be less than 0.600.

[0222] In one embodiment, in the glass composition represented by anion % of the glass, the content of O ions may be 90.0 anion % or less.

[0223] In one embodiment, in the above glass, as a transmittance characteristic converted to a thickness of 0.11 mm, a transmittance T1200 at a wavelength of 1200 nm may be 42.0% or less.

[0224] In one embodiment, in the above glass, as a transmittance characteristic converted to a thickness of 0.11 mm, a transmittance T400 at a wavelength of 400 nm may be 68.0% or more.

[0225] In one embodiment, in the above glass, as a transmittance characteristic converted to a thickness of 0.21 mm, a transmittance T1200 at a wavelength of 1200 nm may be 42.0% or less.

[0226] In one embodiment, in the above glass, as a transmittance characteristic converted to a thickness of 0.21 mm, a transmittance T400 at a wavelength of 400 nm may be 68.0% or more.

[0227] According to one embodiment, there is provided a near infrared cut filter made of the near infrared absorbing glass.

[0228] In one embodiment, the near infrared cut filter may have a thickness of 0.25 mm or less.

[0229] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.11 mm, a wavelength at which the transmittance reaches 50% at a wavelength of 600 nm or longer may be in the range of 600 nm to 650 nm.

[0230] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.11 mm, a transmittance T1200 at a wavelength of 1200 nm may be 42.0% or less.

[0231] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.11 mm, a transmittance T400 at a wavelength of 400 nm may be 68.0% or more.

[0232] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.21 mm, the wavelength at which the transmittance reaches 50% at a wavelength of 600 nm or longer may be in the range of 600 nm to 650 nm.

[0233] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.21 mm, a transmittance T1200 at a wavelength of 1200 nm may be 42.0% or less.

[0234] In one embodiment, in the near infrared cut filter, as a transmittance characteristic converted to a thickness of 0.21 mm, a transmittance T400 at a wavelength of 400 nm may be 68.0% or more.

[0235] It should be understood that the embodiments disclosed this time are all exemplary and not restrictive. The scope of the present invention is defined by the claims rather than the above description, and is intended to include all modifications within the meaning and scope equivalent to the claims.

[0236] For example, by adjusting the composition of the glass composition exemplified above as described in the specification, the near infrared absorbing glass according to one embodiment of the present invention can be obtained.

[0237] Furthermore, it is of course possible to arbitrarily combine two or more of the features described as examples or as preferred ranges in the specification.

Claims

1. A near infrared absorbing glass comprising at least the following ions as constituent ions: P ions, Cu ions, O ions, One or more ions selected from Li ions, Na ions and K ions, and One or more ions selected from Mg ions, Ca ions, Sr ions and Ba ions, in, In the glass composition expressed in cation %, The content of Cu ions is less than 15.0 cation %, The content of P ions is less than 55.0 cation %, The cation ratio ((Al ion + P ion) / (Mg ion + Ca ion + Sr ion + Ba ion + Zn ion + Cu ion)) of the total content of Al ion and P ion to the total content of Mg ion, Ca ion, Sr ion, Ba ion, Zn ion and Cu ion is 5.300 or less, The cation ratio of the total content of Mg ions, Ca ions, Sr ions and Ba ions to the total content of Li ions, Na ions and K ions ((Mg ions + Ca ions + Sr ions + Ba ions) / (Li ions + Na ions + K ions)) is 0.100 or more, The average valence of cations other than Cu ions and P ions is less than 1.

500. In the glass composition expressed in anion %, The content of O ions is 85.0% or more of anions, and The ratio of the content of O ions to the content of P ions (O ions / P ions) is 3.300 or more.

2. The near infrared absorbing glass according to claim 1, wherein In the glass composition expressed as cation %, the content of P ions is 30.0 cation % or more and 50.0 cation % or less.

3. The near infrared absorbing glass according to claim 1 or 2, wherein: In the glass composition expressed as cation %, the content of Li ions is 10.0 cation % or more.

4. The near infrared absorbing glass according to any one of claims 1 to 3, wherein In the glass composition expressed as cation %, the content of Cu ions is 2.1 cation % or more and 15.0 cation % or less.

5. The near infrared absorbing glass according to any one of claims 1 to 4, wherein In the glass composition expressed as cation %, the content of Ba ions is 3.75 cation % or more.

6. The near infrared absorbing glass according to any one of claims 1 to 5, wherein In the glass composition expressed as cation %, the total content of Al ions and P ions (Al ions+P ions) is 45.0 cation % or more.

7. The near infrared absorbing glass according to any one of claims 1 to 6, wherein The ratio (O ion / P ion) is 3.400 or more.

8. The near infrared absorbing glass according to any one of claims 1 to 7, wherein In the glass composition expressed as cation %, the cation ratio of Zn ions to the total content of Mg ions, Ca ions, Sr ions, Ba ions and Zn ions (Zn ions / (Mg ions+Ca ions+Sr ions+Ba ions+Zn ions)) is 0.600 or less.

9. The near infrared absorbing glass according to any one of claims 1 to 8, wherein In the glass composition expressed as anion %, the content of F ions is 10.0 anion % or less.

10. The near infrared absorbing glass according to any one of claims 1 to 9, wherein As the transmittance characteristics converted to a thickness of 0.11 mm, the wavelength at which the transmittance reaches 50% at a wavelength of 600 nm or more is in the range of 600 nm to 650 nm, the transmittance T1200 at a wavelength of 1200 nm is less than 42.0%, and the transmittance T400 at a wavelength of 400 nm is more than 68.0%.

11. The near infrared absorbing glass according to any one of claims 1 to 9, wherein As the transmittance characteristics converted to a thickness of 0.21 mm, the wavelength at which the transmittance reaches 50% at a wavelength of 600 nm or more is in the range of 600 nm to 650 nm, the transmittance T1200 at a wavelength of 1200 nm is less than 42.0%, and the transmittance T400 at a wavelength of 400 nm is more than 68.0%. 12 . A near infrared cut filter, comprising the near infrared absorbing glass according to claim 1 . 13 . The near infrared cut filter according to claim 12 , which has a thickness of 0.25 mm or less.

14. The near infrared cut filter according to claim 12 or 13, wherein: As the transmittance characteristics converted to a thickness of 0.11 mm, after a wavelength of 600 nm, the wavelength at which the transmittance reaches 50% is in the range of 600 nm-650 nm, the transmittance T1200 at a wavelength of 1200 nm is less than 42.0%, and the transmittance T400 at a wavelength of 400 nm is more than 68.0%.

15. The near infrared cut filter according to claim 12 or 13, wherein: As the transmittance characteristics converted to a thickness of 0.21 mm, after a wavelength of 600 nm, the wavelength at which the transmittance reaches 50% is in the range of 600 nm-650 nm, the transmittance T1200 at a wavelength of 1200 nm is less than 42.0%, and the transmittance T400 at a wavelength of 400 nm is more than 68.0%.

Citation Information

Patent Citations

  • Near infrared cutoff filter glass

    CN107850711A

  • Glass, glass product and preparation method of glass product

    CN110255897A

  • Near-infrared absorption glass, element and filter and process for manufacturing molded product of the glass

    JP2004083290A

  • Near-infrared light cutting filter glass

    JP2011168455A