Chemically strengthened glass ceramic as well as preparation method and application thereof

Through the glass ceramics with specific treatment of oxide raw materials, chemically strengthened glass ceramics with main crystal phases of sodium sulfate, sulfate and sodium silicate are formed, which solves the problem of insufficient mechanical and optical properties of glass ceramics in the prior art, and realizes the Higher drop resistance and optical performance meet the needs of modern electronic products and on-board equipment.

CN118993548AInactive Publication Date: 2024-11-22深圳市昊迦科技有限公司

Patent Information

Application Number
CN202411092649.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing glass-ceramic materials are difficult to meet the needs of mid-to-high-end 3C consumer electronics and smart automotive on-board display equipment for the mechanical and optical properties of cover glass.

Method used

The oxide raw materials of a specific proportion are melted, annealed, nuclearized and crystallized to control the crystal form and proportion of nanocrystals, and the tensile stress and optical properties of glass ceramics are improved through chemical strengthening treatment to form sodium sulfide, Chemically strengthened glass ceramics of the main crystal phase of trisilicolite and sodium silicate.

Benefits of technology

It achieves higher drop resistance and optical properties of chemically strengthened glass ceramics, can effectively suppress crack propagation, meet the needs of modern 3C consumer electronic products and vehicle display equipment, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993548A_ABST
    Figure CN118993548A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic glass, and particularly discloses chemically strengthened glass ceramic as well as a preparation method and application thereof. The preparation method comprises the following steps: uniformly mixing corresponding compound raw materials containing oxides, carrying out melt molding, and carrying out annealing treatment to obtain base glass; carrying out nucleation treatment and crystallization treatment on the base glass to obtain a glass ceramic precursor; carrying out chemical strengthening treatment on the glass ceramic precursor to obtain chemically strengthened glass ceramic; the oxides in the corresponding compound raw materials comprise the following components in percentage by mass: 40 to 55 percent of SiO2, 4 to 28 percent of Al2O3, 10 to 25 percent of Na2O, 1 to 7.5 percent of ZrO2, 1 to 2 percent of TiO2, 1 to 7 percent of P2O5, 0 to 2 percent of CaO, 1 to 8 percent of Li2O, 0 to 3 percent of K2O, 0.2 to 2 percent of SnO2 and 0 to 4 percent of B2O3. The chemically strengthened glass ceramic material prepared by the invention has excellent mechanical properties and optical properties, and can be applied to protective cover plates of consumer electronics and / or automobile vehicle-mounted display device screens.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of glass ceramics, and in particular to a chemically strengthened glass ceramic and a preparation method and application thereof. Background Art

[0002] With the advent of the era of the Internet of Everything, various 3C consumer electronics and smart cars have entered the lives of consumers. In order to enhance the user experience, the speed of updating, transformation and elimination of 3C consumer electronics and automotive equipment is also accelerating. In particular, in order to meet the requirements of the above products for thinness and lightness, the performance requirements for cover glass for display devices are gradually increasing. A kind of sodium nepheline (NaAlSiO 4 ), triclinic nepheline and sodium silicate (Na 4 SiO 4 ) as the main crystalline phase can achieve a crystallinity of more than 50wt%. When the thickness of the glass ceramic is 0.30-1.0mm, the transmittance, haze and color control B value in the 400-800nm ​​wavelength light band are close to those of commonly used strengthened glass, and ion exchange chemical strengthening can be performed using a molten salt bath to further improve its mechanical properties such as drop resistance and impact resistance, which has attracted widespread attention in the cover plate industry for display devices.

[0003] However, the glass ceramic materials in the prior art are difficult to meet the mechanical and optical performance requirements of cover glass for current mid-to-high-end 3C consumer electronic products and smart car-type on-board display devices. Therefore, the prior art needs to be improved. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present application is to provide a chemically strengthened glass-ceramic and a preparation method and application thereof, aiming to solve the problem of insufficient mechanical properties and optical properties of glass-ceramic.

[0005] The technical solution of this application is as follows:

[0006] In a first aspect of the present application, a method for preparing a chemically strengthened glass-ceramic is provided, comprising the steps of: uniformly mixing corresponding compound raw materials containing oxides, melting and forming, and performing annealing treatment to obtain a base glass; performing nucleation treatment and crystallization treatment on the base glass to obtain a glass-ceramic precursor; performing chemical strengthening treatment on the glass-ceramic precursor to obtain the chemically strengthened glass-ceramic; wherein the oxides in the raw materials, in terms of mass percentage, include: SiO 2 :40~55%,Al 2 O 3 :4~28%,Na 2 O: 10-25%, ZrO 2 :1~7.5%,TiO 2:1~2%,P 2 O 5 : 1~7%, CaO: 0~2%, Li 2 O: 1~8%, K 2 O: 0-3%, SnO 2 :0.2~2%,B 2 O 3 :0~4%;The chemically strengthened glass ceramics satisfy:0.255t≥DOL_0≥0.155t,400Mpa≥CS_50≥100Mpa,200Mpa≥|CT_AV|≥95Mpa,210Mpa≥|CT_CV|≥85Mpa,80000Mpa / mm≥CT_LD≥48000Mpa / mm,t is the thickness of the chemically strengthened glass ceramics, in mm;The chemically strengthened glass ceramics are in thickness When the thickness of the chemically strengthened glass-ceramic is between 0.5 and 1 mm, at least 10 glass-ceramic samples are taken with the same thickness and dropped on 120-mesh sandpaper in a fixed direction, with an average maximum drop height H ≥ 150 cm and an average impact energy E ≥ 0.3 joules. When the thickness of the chemically strengthened glass-ceramic is between 0.3 and 1.0 mm, for light with a wavelength of 400 to 800 nm, the transmittance of the chemically strengthened glass-ceramic is ≥ 89%, the haze is ≤ 0.15, and the color index LAB value |B| is ≤ 1.2.

[0007] Preferably, the oxides in the raw materials include, by mass percentage: SiO 2 :42~55%,Al 2 O 3 :5~28%,Na 2 O: 12-25%, ZrO 2 :1~7.5%,TiO 2 :1.2~2%,P 2 O 5 : 2~7%, CaO: 0.1~2%, Li 2 O: 3-8%, K 2 O: 0.1~3%, SnO 2 :0.5~2%,B 2 O 3 :1~4%.

[0008] Preferably, the oxides in the raw materials include, by mass percentage: SiO 2 :42~52%,Al 2 O 3 :6~28%,Na 2 O: 14-25%, ZrO 2 :1.5~7.5%,TiO 2 :1.4~2%,P2 O 5 : 3~7%, CaO: 0.2~2%, Li 2 O: 4-8%, K 2 O: 0.2~3%, SnO 2 :1~2%,B 2 O 3 :2~4%.

[0009] Preferably, a clarifier is added during the melt forming process, and the clarifier includes NaCl, Sb 2 O 3 、As 2 O 3 , nitrate, sulfate; the mass of the clarifier is 0.1-1% of the total mass of the raw materials.

[0010] Preferably, the temperature T of the annealing treatment satisfies the relationship: (T g -120)℃≤T≤(T g -60)℃, where T g is the transition temperature of the base glass; and the annealing treatment time is 6 to 168 hours.

[0011] Preferably, the basic glass is formed by one of the following processes: float process, overflow down-draw process, roller pressing process and casting process.

[0012] Preferably, the temperature of the nucleation treatment is (T g ±30)℃, where T g is the transition temperature of the base glass; the time of the nucleation treatment is 60 to 600 minutes, and the heating rate of the nucleation treatment is 3 to 20°C / min.

[0013] Preferably, the temperature of the crystallization treatment is (T p ±45)℃, where T p The temperature is the temperature at which the difference between the thermal analysis DSC curve of the base glass and the quasi-baseline is the largest; the time of the crystallization treatment is 10 to 360 minutes, and the heating rate of the crystallization treatment is 3 to 20° C. / min.

[0014] Preferably, the chemical strengthening treatment comprises the steps of: placing the glass ceramic precursor in a molten salt for 1 to 36 hours; the molten salt comprises at least one of sodium ions, lithium ions and potassium ions, and the temperature of the molten salt is 380 to 560°C.

[0015] Preferably, in terms of ion concentration, the concentration of lithium ions in the molten salt is 0 to 100 ppm, the concentration of sodium ions in the molten salt is ≥ 250,000 ppm, and the concentration of potassium ions in the molten salt is 10 to 25,000 ppm.

[0016] In a second aspect of the present application, a chemically strengthened glass-ceramic prepared by the above-mentioned method for preparing the chemically strengthened glass-ceramic is provided.

[0017] Preferably, the main crystalline phase of the chemically strengthened glass-ceramic includes at least one of triclinic nepheline, sodium nepheline and sodium silicate; the content of the main crystalline phase is ≥50wt%, and the average grain size of the main crystalline phase is ≤100nm.

[0018] The third aspect of the present application provides an application of the chemically strengthened glass ceramic prepared by the above-mentioned preparation method of the chemically strengthened glass ceramic in the preparation of protective cover plates for screens of consumer electronic products and / or automotive display devices.

[0019] Compared with the prior art, this application has the following advantages:

[0020] (1) The chemically strengthened glass ceramics in this application adopt a specific proportion of raw materials, and undergo melting, annealing, nucleation treatment, and crystallization treatment to control the crystal form, size, and proportion of the nanocrystalline in the entire glass ceramics, so that the main crystal phase has at least one of sodium nepheline, triclinic nepheline, and sodium silicate. Then, through chemical strengthening treatment, the mechanical properties of the glass ceramics such as tensile stress, stress layer depth, and compressive stress at a depth of 50 μm from the surface of the glass ceramics are improved, so that it has better anti-fall performance, and can effectively inhibit crack propagation, making it strong and durable.

[0021] (2) By controlling the nanocrystalline crystal form, size and chemical strengthening treatment of chemically strengthened glass-ceramics, the chemically strengthened glass-ceramics has a compressive stress layer on the surface formed by ion exchange and chemical strengthening, and a tensile stress layer inside. Since the tensile stress layer has not undergone ion exchange, its composition is the same as that of the transparent glass-ceramics before strengthening, thereby ensuring the optical properties of the chemically strengthened glass-ceramics, which can fully meet the current 3C consumer electronic products and vehicle-mounted display equipment requirements for optical properties.

[0022] (3) The raw materials used in the preparation method of the present application have a low content of lithium oxide, which reduces the preparation cost of glass ceramics and saves resources. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A differential scanning calorimetry graph of the chemically strengthened glass-ceramic provided in Test Example 1 of the present application;

[0024] Figure 2 This is a graph of light transmittance of chemically strengthened glass ceramics provided in Test Example 1 of this application;

[0025] Figure 3 This is the X-ray diffraction analysis diagram of the chemically strengthened glass-ceramic provided in Test Example 1 of this application. DETAILED DESCRIPTION

[0026] In order to make it easier to understand this application, some terms are first defined below. Additional definitions of the following terms and other terms are set forth throughout the specification. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as those commonly understood by those of ordinary skill in the art.

[0027] Basic glass: Glass that has not been nucleated, crystallized or chemically strengthened by ion exchange is made by uniformly mixing compounds containing various oxides (including silicon dioxide, aluminum oxide, sodium oxide, calcium oxide, etc.), melting them at high temperature, and then forming them by one of the following methods: float method, overflow down-draw method, roller pressing method or casting method.

[0028] Glass ceramics: also known as microcrystalline glass, is a type of solid composite material that contains both glass phase and crystal phase (microcrystalline phase, crystalline phase) and is prepared by subjecting base glass to a targeted controlled crystallization treatment.

[0029] Nucleation: The base glass is heat treated to make the nucleating material in the glass grow tiny crystal nuclei.

[0030] Crystallization: The base glass is grown into a certain crystal based on the crystal nucleus through heat treatment.

[0031] Crystalline phase: It is the microscopic structure of crystals and is a general term for parts composed of a large number of crystalline solid phases.

[0032] Crystallinity: It is used to indicate the proportion of the crystalline region in (chemically strengthened) glass-ceramics, generally based on the volume ratio of the crystalline phase in the entire glass-ceramics.

[0033] T g Temperature: It is the glass transition temperature, which refers to the temperature corresponding to the transition from glass state to highly elastic state. The glass transition temperature is an inherent property of glass ceramics, which directly affects the performance and process performance of glass ceramic materials.

[0034] DSC curve: Using differential scanning calorimetry to measure the heat flow difference between the sample and the reference sample under program-controlled temperature, the curve of the heat flow difference between the sample and the reference sample as it changes with temperature and time can reflect the enthalpy change of the sample as the temperature and time change. The DSC curve can quantitatively measure the crystallinity and crystallization kinetics of the sample.

[0035] T p Temperature: The temperature at which the difference between the thermal analysis DSC curve and the quasi-baseline is maximum.

[0036] CS (Compressive Stress): Surface compressive stress. After glass ceramics are chemically strengthened, alkali metal ions with smaller radius are replaced by alkali metal ions with larger radius. Due to the crowding effect of alkali metal ions with larger radius, compressive stress is generated on the glass surface. It is obtained by stress meter testing and the unit is MPa.

[0037] CS_50: Compressive stress at a depth of 50 μm from the glass surface, in MPa.

[0038] CT (Center Tension): Central tensile stress, the pressure generated from the center of the glass to the surrounding area, the unit is MPa.

[0039] CT_LD: tensile stress line density, the ratio of the tensile stress integral of the strengthened glass-ceramics measured by a stress meter such as SLP-2000 to the glass thickness, in MPa / mm.

[0040] |CT_AV|: The absolute value of the average tensile stress, specifically refers to the absolute value of the average value of all tensile stresses in the tensile stress layer, obtained by stress meter testing, in MPa.

[0041] DOL_0: Compression stress depth, or compressive stress layer depth, refers to the distance from any surface of the glass ceramic to the position close to the surface where the compressive stress is zero, obtained by stress meter testing, in μm.

[0042] |CT_CV|: Maximum central tensile stress or maximum tensile stress, specifically refers to the maximum value of all tensile stresses in the tensile stress layer, obtained by stress meter testing, the unit is MPa.

[0043] K-DOL: Depth of stress layer of compressive stress generated by potassium ions, in μm.

[0044] Transmittance (TR): The ratio of the radiant energy that is projected and transmitted through an object to the total radiant energy that is projected onto the object during the process of the incident light flux leaving the object from the illuminated surface or the incident surface of the medium to the other side.

[0045] Refractive index λ: The ratio of the speed of light in a vacuum to the speed of light in the medium.

[0046] Haze: A beam of parallel light from standard light source C is irradiated vertically onto a transparent or translucent film, sheet or plate. Due to scattering inside and on the surface of the material, part of the parallel light deviates from the incident direction by more than 2.5°. The percentage of the scattered light flux Td to the light flux T2 that passes through the material is an important parameter for the optical transparency of transparent or translucent materials.

[0047] LAB value: LAB is a color model based on physiological characteristics, where L represents brightness, A includes colors from dark green to gray to bright pink, and B includes colors from bright blue to gray to yellow. The B value in LAB can represent the deviation of an object between yellow and blue.

[0048] In order to make the purpose, technical solutions and advantages of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings and embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments of the present application, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the protection scope of the present application. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0049] It should be noted that if there are descriptions involving "first", "second", etc. in the implementation of this application, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or suggesting their relative importance and implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the fact that ordinary technicians in the field can implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0050] The reason why cover glass breaks during use is usually that the electronic product falls from a height, causing the glass to collide with a sharp object or passively receive the squeeze and impact of a sharp object. The local stress on the glass surface changes, and microcracks are formed around the squeeze and impact point. The cracks extend from the glass surface to the inside. When the cracks extend through the compressive stress layer on the glass surface to reach the tensile stress layer area, the cracks will quickly extend in the tensile stress area, causing the cracks to penetrate the entire glass, resulting in glass breakage and fracture. In the prior art, the absolute value of the maximum compressive stress on the surface of glass-ceramic obtained by a specific ion exchange chemical strengthening method is 1.8 to 2.2 times the absolute value of the maximum central tensile stress, and the CT maximum value reaches 140Mpa, while satisfying the following conditions CS_50 / (K-DOL×t)≥45Mpa / (μm˙mm), where t is the thickness of the glass-ceramic. However, these glass-ceramics still find it difficult to meet the requirements of the mechanical and optical properties of cover glass for current mid-to-high-end 3C consumer electronic products and smart car-type on-board equipment.

[0051] Based on this, in a first aspect of the embodiment of the present application, a method for preparing glass ceramics is provided, comprising the steps of:

[0052] S1. uniformly mixing corresponding compound raw materials containing oxides, melting and forming, and annealing to obtain basic glass;

[0053] S2, performing nucleation treatment and crystallization treatment on the base glass to obtain a glass ceramic precursor;

[0054] S3. Chemically strengthen the glass ceramic precursor to obtain chemically strengthened glass ceramic.

[0055] Among them, the oxides in the raw materials are expressed in mass percentage, including: SiO 2 :40~55%,Al 2 O 3 :4~28%,Na 2 O: 10-25%, ZrO 2 :1~7.5%,TiO 2 :1~2%,P 2 O 5 : 1~7%, CaO: 0~2%, Li 2 O: 1~8%, K 2 O: 0-3%, SnO 2 :0.2~2%,B 2 O 3 :0~4%.

[0056] In some embodiments, when the base glass is subjected to nucleation treatment and crystallization treatment, other heat treatments may be performed to obtain a glass-ceramic precursor. The chemical strengthening treatment is preferably an ion exchange chemical strengthening treatment.

[0057] By using raw materials in a specific proportion, after melting, annealing, nucleation treatment, and crystallization treatment, the crystal form, size, and proportion of the nanocrystalline in the entire glass ceramic are controlled, so that the main crystal phase has at least one of sodium nepheline, triclinic nepheline, and sodium silicate. Then, through chemical strengthening treatment, the mechanical properties of the glass ceramic, such as tensile stress, stress layer depth, and compressive stress at a depth of 50μm from the surface of the glass ceramic, are improved, so that it has better anti-fall performance, and can effectively inhibit crack propagation, and is strong and durable; at the same time, the preparation method improves the optical properties of the glass ceramic by controlling the crystal form, size, and chemical strengthening treatment of the nanocrystalline of the glass ceramic, which can fully meet the current 3C consumer electronics and vehicle-mounted display equipment for optical performance requirements. In addition, the content of lithium oxide in the raw materials used is low, which reduces the preparation cost of glass ceramics and saves resources.

[0058] Specifically, SiO 2As one of the main components of the network oxide of basic glass and glass ceramics, it is one of the important components that constitute the Si-O tetrahedron in the main body and form the network structure. Based on the raw materials (compounds) involved in the embodiments of the present application, wherein SiO 2 The mass fraction is 40-55wt%, for example, SiO 2 The mass fraction is 41wt%, 42wt%, 43wt%, 44wt%, 45wt%, 46wt%, 47wt%, 48wt%, 49wt%, 50wt%, 51wt%, 52wt%, 53wt%, 54wt%, 55wt% and any one of the ranges formed by any two of the above values. Preferably, it is 42-52wt%.

[0059] Al 2 O 3 It is an intermediate oxide in the formation of glass and is also a sodium nepheline (NaAlSiO 4 ), triclinic nepheline and other main components of the crystal form, can significantly improve the thermal stability of the basic glass and glass ceramics, at the same time, due to [AlO 4 ] than [SiO 4 ] has a large volume, which can provide more space for ion exchange. Therefore, Al 2 O 3 It can promote ion exchange. 2 O 3 It will increase the viscosity of the glass, which is not conducive to melting. Based on the raw materials involved in the embodiments of the present application, Al 2 O 3 The mass fraction is 4 to 28 wt%, for example, Al 2 O 3 The mass fraction is 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt% and any one of the ranges formed by any two of the above values. Preferably, it is 6-28wt%.

[0060] Na 2 O is sodium nepheline (NaAlSiO 4 ), triclinic sodium silicate (Na 4 SiO 4 ) and is also an important element in the subsequent chemical strengthening process. 2 O is a flux when the base glass is melted at high temperature, which can significantly reduce the melting temperature of the base glass.2 When the O content is higher than 25wt%, the chemical stability of the glass ceramic is significantly reduced. 2 The mass fraction of O is less than or equal to 25wt%, at which point the melting temperature can be kept within an appropriate range while ensuring good ion exchange properties. 2 The mass fraction of O is 10-25wt%, for example, Na 2 The mass fraction of O is 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt% and any one of the ranges formed by any two of the above values. Preferably, it is 14-25wt%.

[0061] ZrO 2 It is an intermediate oxide in the formation of glass, which can improve the chemical stability of glass, increase the hardness of glass and the ability of glass to resist scratches and drops. 2 Due to its high cationic charge and strong field, it has a great accumulation effect on the glass structure and is often used as a nucleating agent in glass ceramics. 2 It will significantly increase the viscosity of the glass and affect the forming ability of the glass. 2 The mass fraction is 1 to 7.5 wt%, for example, ZrO 2 The mass fraction is 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt% and any one of the ranges formed by any two of the above values. Preferably, it is 2-7.5wt%.

[0062] TiO 2 It is one of the nucleating agents for the nucleation and growth of crystals in glass ceramics. It can effectively promote the growth of crystal nuclei in the process of nucleation and crystallization of base glass, and at the same time improve the stability of glass. 2 The introduction of TiO 2 The introduction of TiO2 can easily cause phase separation in the base glass, leading to crystallization and affecting the formation of glass. 2 The mass fraction is 1-2wt%, for example, TiO 2The mass fraction is 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt% and any one of the ranges formed by any two of the above values, preferably 1.4-2wt%.

[0063] P 2 O 5 It can be used as a nucleating agent in base glass and glass ceramics to promote the phase separation and overall crystallization ability of the base glass. 2 O 5 If the concentration is too low, the base glass will not crystallize, but will only form crystals from the surface to the inside at a higher temperature and lower viscosity. 2 O 5 If the concentration is too high, it will be difficult to control devitrification during cooling during the basic glass formation process; the raw materials involved in the embodiments of the present application, P 2 O 5 The mass fraction is 1 to 7 wt%, for example, P 2 O 5 The mass fraction is 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt% and any one of the ranges formed by any two of the above values, preferably 3-7wt%.

[0064] CaO, as a network exo-oxide formed by glass, helps to reduce the viscosity of glass, inhibits glass crystallization during glass forming, and improves the low-temperature melting property of glass. However, excessive CaO will reduce the devitrification resistance of glass. By adding an appropriate amount of CaO, the viscosity of glass can be reduced without affecting the crystallization performance of glass. The raw materials involved in the embodiments of the present application have a mass fraction of CaO of 0 to 2wt%, for example, the mass fraction of CaO is 0wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.8wt%, 1wt%, 1.2wt%, 1.5wt%, 1.8wt%, 2wt% and any one of the ranges of any two of the above values. Preferably, it is 0.2 to 2wt%.

[0065] Li 2 O is an oxide with high alkali metal activity and is an external oxide of the glass network. As one of the additives to reduce the high temperature viscosity of the base glass, it can significantly improve the high temperature fluidity of the base glass. + In the glass ceramics provided in the present application, ion exchange chemical strengthening reaction can be involved to further enhance the mechanical properties of the glass ceramics. The raw materials involved in the embodiments of the present application, Li2 The mass fraction of O is 1 to 8 wt%, for example, Li 2 The mass fraction of O is 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt% and any one of the ranges formed by any two of the above values, preferably 4-8wt%.

[0066] K 2 O can reduce the high temperature viscosity of the base glass, significantly improve the formability and fluidity of the base glass at high temperature, and significantly reduce the crack incidence. 2 O can not only slow down the crystallization behavior during the glass ceramic molding process, but also promote the formation of sodium nepheline, triclinic nepheline or sodium silicate crystals during the crystallization process. 2 O content exceeds 2.5wt%, potassium feldspar and other crystalline phases will be generated, which will harm its mechanical strength and optical properties. 2 The mass fraction of O is 0-3wt%, for example, K 2 The mass fraction of O is 0wt%, 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 2wt%, 2.5wt%, 2.8wt%, 3wt% and any one of the ranges formed by any two of the above values. Preferably, it is 0.2-3wt%.

[0067] SnO 2 As a good clarifier in glass production, it can effectively homogenize the components of the precursor glass and reduce the formation of undesirable substances such as bubbles and stones. 2 The content is 0.2-2wt%, for example SnO 2 The mass fraction is 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt% and any one of the ranges formed by any two of the above values. Preferably, it is 1-2wt%.

[0068] B 2 O 3As the external oxide of the glass network, it is generally filled in the gaps of the silicon-oxygen tetrahedral framework, and its cation coordination rarely changes, so some properties of its oxide can be considered constant. 2 O 3 It helps to provide a base glass with a low melting temperature. In addition, adding B 2 O 3 , and can also improve the damage resistance of glass ceramics. 2 O 3 The mass fraction is 0 to 4 wt%, for example, SnO 2 The mass fraction is 0wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt% and any one of the ranges formed by any two of the above values, preferably 2-4wt%.

[0069] In some embodiments, when the base glass is melted, some clarifiers need to be added to facilitate homogenization of the glass components and eliminate internal bubbles. The clarifiers include NaCl, Sb 2 O 3 、As 2 O 3 , nitrate, sulfate. The mass of the clarifier is 0.1-1wt% of the total mass of all raw materials, for example, the mass fraction of the clarifier is 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt% and any one of the ranges formed by any two of the above values.

[0070] In some embodiments, the temperature of the base glass melt molding is 1400-1650°C, for example, the temperature of the melt molding is 1400°C, 1450°C, 1500°C, 1550°C, 1600°C or 1650°C.

[0071] In some embodiments, the temperature of the annealing treatment in S1 is greater than (T g -120)℃, less than (T g -60)℃. If the annealing temperature exceeds (T g -60)℃, it may cause the glass to burst during processing. If the annealing temperature is lower than (T g -60)℃ will lead to incomplete annealing of the glass and unstable internal structure. Preferably, the annealing temperature is greater than (T g -100)℃, less than (T g-80)°C. The annealing time is 6 to 168 hours. For example, the annealing time is 6 hours, 12 hours, 24 hours, 48 ​​hours, 72 hours, 96 hours, 120 hours, 148 hours or 168 hours. Preferably, the annealing time is 6 to 96 hours.

[0072] In some embodiments, the temperature of the nucleation treatment in S2 is (T g ±30)℃. If the temperature of the nucleation treatment exceeds (T g +30)℃, which will cause the glass to crystallize during the nucleation process. g -30)~(T g +30)℃, which can ensure that almost only nucleation reaction occurs inside the glass. Preferably, the temperature of the nucleation treatment is (T g The time of the nucleation treatment is 60 to 600 min, for example, the time of the nucleation treatment is 60 min, 80 min, 120 min, 180 min, 240 min, 360 min, 480 min or 600 min. The heating rate of the nucleation treatment is 3 to 20 ° C / min, for example, the heating rate of the nucleation treatment is 5 ° C / min, 10 ° C / min, 15 ° C / min or 20 ° C / min. Preferably, the heating rate of the nucleation treatment is 10 ° C / min.

[0073] In some embodiments, the temperature of the crystallization treatment in S2 is (T p ±45)°C. Preferably, the temperature of the crystallization treatment is (T p ±40)°C, more preferably, the crystallization temperature is (T p ±35)°C. The time of the crystallization treatment is 10 to 360 min, for example, the time of the crystallization treatment is 10 min, 20 min, 50 min, 100 min, 150 min, 200 min, 250 min, 300 min, 350 min or 360 min. Preferably, the time of the crystallization treatment is 20 to 240 min, more preferably, the time of the crystallization treatment is 30 to 120 min. The heating rate of the crystallization treatment is 3 to 20°C / min, for example, the heating rate of the crystallization treatment is 5°C / min, 10°C / min, 15°C / min or 20°C / min. Preferably, the heating rate of the crystallization treatment is 10°C / min.

[0074] In some embodiments, before S3, step S21 is further included, wherein the glass ceramic obtained in S2 is subjected to deep cold processing such as cutting, grinding, and polishing to obtain a transparent glass ceramic precursor. Impurities attached to the surface of the glass ceramic precursor can be removed by polishing or grinding, so that the glass ceramic precursor becomes transparent. Cutting, polishing, and grinding can be performed using conventional equipment or methods, which are not limited here.

[0075] In some embodiments, the chemical strengthening treatment in S3 includes the step of placing the glass ceramic precursor in a molten salt for 1 to 36 hours. For example, the time of placing in the molten salt (chemical strengthening treatment) can be 1 hour, 2 hours, 4 hours, 8 hours, 16 hours, 20 hours, 24 hours or 36 hours, etc. Preferably, the time of placing in the molten salt is 2 to 24 hours, and more preferably, the time of placing in the molten salt is 3 to 18 hours. The molten salt includes at least one of sodium ions, lithium ions, and potassium ions. In the chemical strengthening treatment, the temperature of the molten salt is 380 to 560°C, for example, the temperature of the molten salt is 380°C, 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C or 560°C, etc.

[0076] In some embodiments, in terms of ion concentration, the concentration of lithium ions in the molten salt for chemically strengthening the glass-ceramic precursor is 0 to 100 ppm, the concentration of sodium ions is ≥ 250,000 ppm, and the concentration of potassium ions is 1 to 25,000 ppm.

[0077] In some embodiments, the glass ceramic precursor is chemically strengthened with Na in the molten salt. + Provided by at least one of sodium nitrate, sodium sulfate and sodium carbonate, K + Provided by at least one of potassium nitrate, potassium sulfate, and potassium carbonate, Li + Provided by at least one of lithium nitrate, lithium sulfate and lithium carbonate.

[0078] On the one hand, chemical strengthening treatment improves the mechanical properties of glass ceramics such as tensile stress, stress layer depth, and compressive stress at a depth of 50μm from the surface of glass ceramics, making them more resistant to drop. At the same time, it can effectively inhibit crack propagation and make them strong and durable.

[0079] On the other hand, the chemical strengthening treatment makes the chemically strengthened glass-ceramics have a compressive stress layer on the surface formed by ion exchange chemical strengthening and a tensile stress layer inside. Since the tensile stress layer has not undergone ion exchange, its composition is the same as that of the transparent glass-ceramics before strengthening, thereby ensuring its optical properties to meet the current 3C consumer electronics products and vehicle-mounted display devices for optical properties.

[0080] In some embodiments, the number of chemical strengthening treatments in S3 is 1 to 3. By performing chemical strengthening treatments multiple times, the ion exchange in the chemically strengthened glass-ceramics can be more complete, ensuring the effect of chemical strengthening, thereby effectively improving the mechanical properties and optical properties of the chemically strengthened glass-ceramics.

[0081] In some embodiments, the method for preparing the chemically strengthened glass-ceramic comprises the steps of:

[0082] S101. Preparation of basic glass: according to the formula, the compound ingredients containing the corresponding oxides are uniformly mixed and melted in a platinum crucible at 1500-1600°C for 4 hours, then poured into a molding mold for molding, cooled to 900°C, placed in an annealing furnace at 450-600°C for annealing for 6-240 hours, and then cooled to room temperature with the furnace to obtain the basic glass.

[0083] In some embodiments, a certain amount of clarifier may be added during the melting and forming process of the base glass. The clarifier includes NaCl, Sb 2 O 3 、As 2 O 3 , nitrate, sulfate. The mass of the clarifier is 0.1-1wt% of the total mass of all raw materials. For example, the mass of the clarifier is 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt% of the total mass of all raw materials.

[0084] S102. Preparation of glass ceramics: The basic glass prepared in S101 is subjected to nucleation treatment and crystallization treatment in sequence to obtain a glass ceramic precursor.

[0085] The crystallization furnace is heated to 500-700° C. at a rate of 3-20° C. / min and kept at this temperature for 5-1440 min. Then, the crystallization furnace is heated to 640-750° C. at a rate of 3-20° C. / min and kept at this temperature for 5-1440 min.

[0086] S103, cold-processing the glass ceramic precursor obtained in S102. Specifically, the glass ceramic precursor is first shaped and sliced, and after the slicing, it can be processed by numerical control (CNC), grinding, polishing, or after the slicing, at least one of CNC, grinding, and polishing is selected to be modified to obtain a glass ceramic sample of a desired size. For example, after the cold processing, a polished sheet with a length, width, and thickness of 50 mm×50 mm×0.7 mm, 158.8 mm×72.8 mm×0.7 mm, etc. is obtained.

[0087] S104, chemically strengthening the polishing sheet in S103 in a molten salt at 380-550°C for 1-24 hours. The molten salt includes at least one of sodium ions, lithium ions, and potassium ions. + Provided by at least one of sodium nitrate, sodium sulfate and sodium carbonate, K + Provided by at least one of potassium nitrate, potassium sulfate, and potassium carbonate, Li + Provided by at least one of lithium nitrate, lithium sulfate and lithium carbonate.

[0088] In some embodiments, the molten salt includes 0.1 to 100 wt % NaNO 3 , 0~99wt% KNO 3 and 0-10wt% LiNO 3 .

[0089] According to a second aspect of the embodiments of the present application, there is provided a chemically strengthened glass-ceramic prepared by the preparation method of the chemically strengthened glass-ceramic.

[0090] Among them, the main crystalline phases of chemically strengthened glass-ceramics include triclinic nepheline, sodium nepheline (NaAlSiO 4 ), sodium silicate (Na 4 SiO 4 ). The total content of the main crystalline phase accounts for more than 50wt% of the glass ceramic; preferably, the total content of the main crystalline phase accounts for more than 55wt% of the glass ceramic; more preferably, the total content of the main crystalline phase accounts for more than 60wt% of the chemically strengthened glass ceramic. At the same time, the chemically strengthened glass ceramic may also contain impurity phases, such as zirconium oxide.

[0091] Sodium nepheline (NaAlSiO 4 ) is a hexagonal crystal system, triclinic nepheline is a metastable state, and the crystal structure of nepheline is SiO 2 Hexagonal, the channel has vacancies, in order to maintain charge balance, half of the network Si 4+ Al located on these vacancies 3+ 、Na + Replacement, at the same time due to Na + The ion radius is large, the electric load field is strong, and at high temperature, the high content of Na + Priority over Li + With Al 3+ , Si 4+ and O 2+ Formation of sodium nepheline (NaAlSiO 4 ) crystal, so Li + It is left in sodium nepheline (NaAlSiO 4 ) in the glass phase of chemically strengthened glass-ceramics, which can remove the Na + Replace Li in glass ceramics + , further enhancing the mechanical properties of glass ceramics.

[0092] In some embodiments, the content of the main crystalline phase of the chemically strengthened glass-ceramic is 50-85wt% of the mass of the chemically strengthened glass-ceramic. For example, the content of the main crystalline phase of the chemically strengthened glass-ceramic is 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt% or 85wt% of the mass of the chemically strengthened glass-ceramic, and any value in the range consisting of any two of the above values.

[0093] In some embodiments, the average grain size of the main crystalline phase in the chemically strengthened glass-ceramic is less than 100 nm, for example, the average grain size of the main crystalline phase in the chemically strengthened glass-ceramic is 10 nm, 15 nm, 20 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm or 100 nm, etc. Preferably, the average grain size of the main crystalline phase in the chemically strengthened glass-ceramic is 10 to 80 nm. More preferably, the average grain size of the main crystalline phase in the chemically strengthened glass-ceramic is 10 to 40 nm.

[0094] In some embodiments, when the thickness of the chemically strengthened glass-ceramic is 0.70 mm-1.0 mm, the chemically strengthened glass-ceramic has the following stress characteristics at 0.7 mm: surface CS: 200-680 MPa; CS_50: 100-400 MPa; |CT_CV|: 85-210 MPa; |CT_AV|: 95-200 MPa; CT_LD: 48000-80000 MPa / mm.

[0095] In some embodiments, the chemically strengthened glass ceramics also have excellent anti-drop performance / anti-fall performance. When the thickness of the chemically strengthened glass ceramics is between 0.5 and 1 mm, at least 10 samples of the same thickness are taken under a 120-mesh sandpaper environment and subjected to a 200g mass load for a sandpaper drop test. The average sandpaper drop height of the chemically strengthened glass ceramics is greater than 150 cm, and the average impact energy that can be sustained is greater than 0.30 joules; at a thickness of 0.65 mm, at least 10 chemically strengthened glass ceramic samples are taken and subjected to a 120-mesh sandpaper load of 200g mass for a sandpaper drop test, and the average sandpaper drop height is 1.5 to 2 m; at a thickness of 0.65 mm, at least 10 chemically strengthened glass ceramic samples are taken and subjected to a 180-mesh sandpaper load of 200g mass for a sandpaper drop test, and the average sandpaper drop height is 2.5 m.

[0096] In some embodiments, the impact energy test of chemically strengthened glass ceramics is performed according to the following steps: when the thickness of the chemically strengthened glass ceramics is between 0.50 and 1.0 mm, at least 10 samples of the same thickness of chemically strengthened glass ceramic polishing sheets are taken, the lower surface of the sample is supported on all sides, and the middle is hollowed out. A steel ball with a weight of 32.65 g corresponding to an impact energy of 0.2 J is used. At a test height of 62.5 cm, the steel ball is freely dropped at the corresponding height to hit two points around the sample, a total of 8 points, plus the center position of the intersection of the sample diagonals, a total of 9 points, and each point is impacted once. If the 0.2 J sample does not break, the test height can be increased until the sample is broken, and the corresponding average value of the maximum energy that at least 10 samples can withstand is recorded.

[0097] In some embodiments, the chemically strengthened glass ceramic also has excellent optical properties. When the thickness is 0.30 to 1 mm, for light with a wavelength of 400 to 800 nm, the chemically strengthened glass ceramic has a transmittance of ≥89%, a haze of ≤0.15, and a color index LAB value of |B| ≤1.2. At a thickness of 0.65 mm, for light with a wavelength of 550 nm, the chemically strengthened glass ceramic is transparent and has a transmittance of not less than 90%.

[0098] The base glass is subjected to a nucleation and crystallization heat treatment to prepare a crystalline glass ceramic precursor, which is then placed in a certain concentration of pure sodium salt or Li + 、Na + , K + Ion exchange chemical strengthening is carried out in one and / or two and / or three mixed molten salts to obtain chemically strengthened glass-ceramics, so that the above-mentioned stress requirements are met after strengthening, and better anti-fall performance is obtained, thereby improving the mechanical properties of the chemically strengthened glass-ceramics of the present application.

[0099] In a third aspect of the embodiments of the present application, there is provided an application of the chemically strengthened glass-ceramic material described above in the preparation of a protective cover plate for a consumer electronic product and / or a vehicle-mounted display device screen. The consumer electronic products include mobile phones, notebooks, tablet computers, POS terminals, etc. The vehicle-mounted display device screen can be installed on a car dashboard, a center console, behind the front seats, a rear console, a car ceiling, etc.

[0100] The following is further described by means of specific examples.

[0101] Examples 1 to 6

[0102] (1) According to the composition and percentage of the corresponding compound raw materials containing the oxides shown in Table 1, weigh a total of 1000 g of various raw material powders, add 5 g of NaCl (clarifier), mix with a mixer for 30 min, and melt in a platinum crucible at 1650°C for 5 h. Then pour into a molding mold for molding. After cooling to 900°C, put it into a 480°C annealing furnace for annealing for 12 h, and then cool it to room temperature at a rate of 5°C / min to obtain a basic glass brick.

[0103] (2) The base glass is placed in an annealing furnace for nucleation / crystallization heat treatment. The temperature setting of the nucleation / crystallization heat treatment is shown in Table 1. The base glass is then cooled to room temperature in the furnace to obtain a glass ceramic sample brick (precursor).

[0104] (3) After shaping, slicing, CNC, flat grinding and polishing, the glass ceramic sample bricks were polished to obtain 50 mm × 50 mm × 0.7 mm polished pieces. Three molten salts (NaNO 3 、KNO 3 、LiNO 3 ), with a total weight of 1000 g, were mixed and placed in a crucible, and heated to 480° C. to obtain a molten salt for chemical strengthening. The polished sheet was placed in the molten salt and subjected to a chemical strengthening treatment at 480° C. for 7 h to obtain a chemically strengthened glass ceramic.

[0105] Table 1. Raw material composition and heat treatment parameters of Examples 1 to 6

[0106]

[0107]

[0108] It can be seen from Table 1 that the amount of nucleating agent added in Example 4 and Example 5 is less than that in other examples. Therefore, the corresponding T in Table 2 is g With T p The temperature is relatively high, that is, a higher temperature is required to induce nucleation. In addition, the crystallization temperature of Example 6 is low, resulting in a low degree of glass crystallization, a small proportion of the main crystal phase, and a small crystal size.

[0109] Test Example 1

[0110] The mechanical properties of the prepared chemically strengthened glass-ceramics were tested.

[0111] (1) Use Luceo (Orihara, Japan) model SLP-2000 stress meter to test the stress of chemically strengthened glass ceramics. The light source wavelength is 518nm, SOC = 25.5 (nm / cm) / MPa, refractive index = 1.56, exposure time: 300μs. When testing the surfaces CS, CS_50, CS_100, |CT_AV|, |CT_CV|, DOL_0, it is necessary to drop a special refractive liquid on the stress meter, then wipe the chemically strengthened glass ceramic product clean, place it on the test path, and test its value. The refractive index of the refractive liquid used by SLP2000 is 1.51.

[0112] CT_LD is related to the thickness, strengthening depth and average tensile stress of chemically strengthened glass-ceramics, and can be used to evaluate the drop resistance of chemically strengthened glass-ceramics. CT_LD satisfies the following formula:

[0113]

[0114] Wherein t represents the thickness of the chemically strengthened glass ceramic (the thickness of the chemically strengthened glass ceramic prepared in the embodiment is 0.7 mm), the unit is mm, DOL_0 represents the depth of the compressive stress layer, the unit is μm; |CT_AV| represents the internal average tensile stress, and its absolute value is taken in the calculation, the unit is MPa.

[0115] Table 2 Mechanical test table of chemically strengthened glass-ceramics in Examples 1 to 6

[0116]

[0117]

[0118] The mechanical test results of the chemically strengthened glass ceramics in Examples 1 to 6 are shown in Table 2. As can be seen from Table 2, the CS of the chemically strengthened ceramic glass in Examples 1 to 6 is 200 to 680 MPa; CS_50: 100 to 400 MPa; |CT_CV|: 85 to 210 MPa; |CT_AV|: 95 to 200 MPa; CT_LD: 48000 to 80000 MPa / mm. This shows that the chemically strengthened glass ceramics in this application have excellent mechanical properties. In addition, the Al in Examples 1 and 6 2 O 3 The small amount of addition makes it difficult for crystals to form and the crystallinity is low, resulting in the prepared microcrystalline glass having a low surface compressive stress although the transmittance can meet the requirements. 2 The amount of O added is small, resulting in poor chemical strengthening performance in the later stage.

[0119] (2) The chemically strengthened glass-ceramics prepared in Examples 1 to 6 were subjected to a 120-grit sandpaper drop test. The specific steps include:

[0120] Stick the chemically strengthened glass-ceramic to be tested on the front of a 200g model machine; place the model machine on a drop machine so that the chemically strengthened glass-ceramic to be tested faces the sandpaper, and drop it at a certain drop height (0.4m), impacting the sandpaper located below the model machine to simulate the normal drop posture of a mobile phone. If the chemically strengthened glass-ceramic to be tested does not break, the drop height of the model machine increases according to a certain rule (increases by 0.1m each time), and then a drop impact is performed until the chemically strengthened glass-ceramic to be tested is broken. The last drop height when the chemically strengthened glass-ceramic to be tested is broken is recorded as the anti-sandpaper drop high speed. For example, when the chemically strengthened glass-ceramic to be tested breaks at a drop height of 0.5m, its anti-sandpaper drop height is 0.4m. Take at least 10 pieces of chemically strengthened glass-ceramic to be tested in each batch of the same thickness for testing, and take the average value.

[0121] The results of the sandpaper drop test of the chemically strengthened glass-ceramics are shown in Table 3. At least 10 samples of the same thickness are taken to take the average value. It can be seen from Table 3 that the height of the 120-mesh sandpaper drop test of the chemically strengthened glass-ceramics prepared in the present application exceeds 150 cm on average, and the average impact energy that the sample can withstand is greater than 0.30 joules, which further indicates that the chemically strengthened glass-ceramics prepared in the present application have excellent drop resistance. Combined with its excellent mechanical properties, it can effectively inhibit crack propagation while resisting drop, and is strong and durable.

[0122] Table 3. Height table of the drop test of the chemically strengthened glass-ceramics prepared in Examples 1 to 6 using 120-mesh sandpaper.

[0123]

[0124] (3) The chemically strengthened glass-ceramics prepared in Example 1 were subjected to differential scanning calorimetry (DSC) testing. The specific steps include: grinding the sample to be tested and passing it through a 200-mesh sieve; the testing conditions are: room temperature to 1000°C, a heating rate of 10°C / min; the testing instrument is a German NETZSCH STA 449F3 thermogravimetric and synchronous thermal analyzer. The test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the nucleation temperature of the base glass prepared in Example 1 is between 530 and 550°C, and the crystallization temperature is between 670 and 700°C.

[0125] (4) The transmittance of the chemically strengthened glass-ceramic prepared in Example 1 at a wavelength of 200 to 1000 nm was tested using a Shimadzu UV-2600 ultraviolet-visible spectrophotometer. The results are as follows: Figure 2 As shown. Figure 2It can be seen from the figure that in the visible light wavelength, the chemically strengthened glass ceramic of the present application has a high transmittance and good transparency. At the same time, the chemically strengthened glass ceramic prepared in Example 1 was subjected to X-ray diffraction analysis, and the results are as follows: Figure 3 As shown. Figure 3 It can be seen that the chemically strengthened glass-ceramics of the present application mainly contain sodium nepheline and triclinic nepheline crystal phases.

[0126] In summary, the chemically strengthened glass-ceramics in this application adopts a specific proportion of raw materials, and is melted, annealed, nucleated, and crystallized to control the nanocrystalline crystal form, size, and proportion of the entire chemically strengthened glass-ceramics, so that its main crystal phase has at least one of sodium nepheline, triclinic nepheline, and sodium silicate. Through chemical strengthening treatment, the tensile stress, stress layer depth, and mechanical properties such as compressive stress at a depth of 50 μm from the surface of the chemically strengthened glass-ceramics are improved, so that it has better anti-fall performance, and can effectively inhibit crack propagation, and is durable. By controlling the nanocrystalline crystal form, size, and chemical strengthening treatment of chemically strengthened glass-ceramics, the chemically strengthened glass-ceramics has a compressive stress layer formed by chemical strengthening through ion exchange on the surface and a tensile stress layer inside, and the tensile stress layer is not ion exchanged, so its composition is the same as that of the transparent glass-ceramics before strengthening, which ensures the optical properties of the chemically strengthened glass-ceramics, and can fully meet the current 3C consumer electronics and vehicle-mounted display devices. The demand for optical properties. The raw materials used in the preparation method of the present application have a low content of lithium oxide, which reduces the preparation cost of chemically strengthened glass-ceramics and saves resources.

[0127] It should be understood that the application of the present application is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to this application.

Claims

1. A method for preparing a chemically strengthened glass-ceramic, characterized in that: Includes steps: The corresponding compound raw materials containing oxides are uniformly mixed, melted and formed, and annealed to obtain the basic glass; The base glass is subjected to nucleation treatment and crystallization treatment to obtain a glass ceramic precursor; The glass ceramic precursor is subjected to chemical strengthening treatment to obtain the chemically strengthened glass ceramic; Wherein, the oxides in the raw materials are calculated by mass percentage and include: SiO2: 40~55%, Al2O3: 4~28%, Na2O: 10~25%, ZrO2: 1~7.5%, TiO2: 1~2%, P2O5: 1~7%, CaO: 0~2%, Li2O: 1~8%, K2O: 0~3%, SnO2: 0.2~2%, B2O3: 0~4%; The chemically strengthened glass-ceramic satisfies: 0.255t≥DOL_0≥0.155t, 400Mpa≥CS_50≥100Mpa, 200Mpa≥|CT_AV|≥95Mpa, 210Mpa≥|CT_CV|≥85Mpa, 80000Mpa / mm≥CT_LD≥48000Mpa / mm, t is the thickness of the chemically strengthened glass-ceramic, in mm; When the thickness of the chemically strengthened glass ceramic glass is between 0.5 and 1.0 mm, at least 10 glass ceramic samples of the same thickness are selected and fixedly dropped under 120-mesh sandpaper, with an average maximum drop height H ≥ 150 cm and an average impact energy E ≥ 0.3 joules. When the thickness of the chemically strengthened glass ceramic is between 0.3 and 1.0 mm, for light with a wavelength of 400 to 800 nm, the transmittance of the chemically strengthened glass ceramic is ≥89%, the haze is ≤0.15, and the color index LAB value |B| is ≤1.

2.

2. The preparation method according to claim 1, characterized in that: The oxides in the raw materials are calculated by mass percentage and include: SiO2: 42~55%, Al2O3: 5~28%, Na2O: 12~25%, ZrO2: 1~7.5%, TiO2: 1.2~2%, P2O5: 2~7%, CaO: 0.1~2%, Li2O: 3~8%, K2O: 0.1~3%, SnO2: 0.5~2%, B2O3: 1~4%.

3. The preparation method according to claim 1, characterized in that: The oxides in the raw materials are calculated by mass percentage and include: SiO2: 42~52%, Al2O3: 6~28%, Na2O: 14~25%, ZrO2: 1.5~7.5%, TiO2: 1.4~2%, P2O5: 3~7%, CaO: 0.2~2%, Li2O: 4~8%, K2O: 0.2~3%, SnO2: 1~2%, B2O3: 2~4%.

4. The preparation method according to claim 1, characterized in that: A clarifier is added during the melt forming process, wherein the clarifier includes at least one of NaCl, Sb2O3, As2O3, nitrate, and sulfate; The mass of the clarifier is 0.1-1% of the total mass of the raw materials.

5. The preparation method according to claim 1, characterized in that: The temperature T of the annealing treatment satisfies the relationship: (T g -120)℃≤T≤(T g -60)℃, where T g is the transition temperature of the base glass; and the annealing treatment time is 6 to 168 hours.

6. The preparation method according to claim 1, characterized in that: The basic glass is processed and formed by one of the following methods: float method, overflow down-draw method, roller pressing method and casting method.

7. The preparation method according to claim 1, wherein the temperature of the nucleation treatment is (T g ±30)℃, where T g is the transition temperature of the base glass; the time of the nucleation treatment is 60 to 600 minutes, and the heating rate of the nucleation treatment is 3 to 20°C / min; The temperature of the crystallization treatment is (T p ±45)℃, where T p The temperature is the temperature at which the difference between the thermal analysis DSC curve of the base glass and the quasi-baseline is the largest; the time of the crystallization treatment is 10 to 360 minutes, and the heating rate of the crystallization treatment is 3 to 20° C. / min.

8. The preparation method according to claim 1, characterized in that: The chemical strengthening treatment comprises the steps of: placing the glass ceramic precursor in a molten salt for 1 to 36 hours; The molten salt includes at least one of sodium ions, lithium ions and potassium ions, and the temperature of the molten salt is 380 to 560°C.

9. The preparation method according to claim 8, characterized in that: In terms of ion concentration, the concentration of lithium ions in the molten salt is 0 to 100 ppm, the concentration of sodium ions in the molten salt is ≥ 250000 ppm, and the concentration of potassium ions in the molten salt is 10 to 25000 ppm.

10. A chemically strengthened glass-ceramic prepared by the method for preparing a chemically strengthened glass-ceramic according to any one of claims 1 to 9.

11. The chemically strengthened glass-ceramic according to claim 10, characterized in that: The main crystalline phase of the chemically strengthened glass-ceramic includes at least one of triclinic nepheline, sodium nepheline and sodium silicate; The content of the main crystalline phase is ≥50wt%, and the average grain size of the main crystalline phase is ≤100nm.

12. Use of the chemically strengthened glass ceramics prepared by the method for preparing the chemically strengthened glass ceramics according to any one of claims 1 to 9 in protective cover plates for screens of consumer electronic products and / or automotive display devices.

Citation Information

Patent Citations

  • Microcrystalline glass and substrate thereof

    CN107963815A

  • Glass ceramic, glass ceramic product and manufacturing method thereof

    CN116023034A

  • Method for regulating crystallization of microcrystalline glass and product thereof

    CN116444140A

  • Antimicrobial alkali-silicate glass ceramic and the use thereof

    US20050009682A1

Cited By

  • Chemically strengthened microcrystalline glass and preparation thereof

    CN121672942A