Manufacturing method of metal film system wide-spectrum attenuation sheet
By plating the metal alloy film system with a 'Cr+Ag+Cr' sandwich structure on an optical glass substrate, the existing dielectric film system has solved the problem of narrow bandwidth and large deviation of the bandwidth of the wide spectrum attenuation sheet, and achieved a wavelength of 0.4 μm to 2.5 μm The uniform attenuation effect in the area reduces color cast distortion and noise interference, and improves the performance of the photoelectric system.
Patent Information
- Application Number
- CN202410972664.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-22
AI Technical Summary
In practical applications, existing dielectric film-based wide spectrum attenuation sheets have problems of color distortion and noise interference in the photoelectric system due to narrow bandwidth and large deviations.
By using vacuum coating method on optical glass substrates, metal alloy film systems with different thicknesses of 'Cr+Ag+Cr' sandwich structures are prepared, so that uniform attenuation effect in wavelength regions of 0.4μm to 2.5μm can be achieved, and the attenuation transmittance can be from 0% to 10% variable, with a deviation of less than ±1.0%.
It realizes uniform attenuation effect in a wide spectrum area, reduces color cast distortion and noise interference, and improves the performance and environmental adaptability of the photoelectric system.
Smart Images

Figure CN118993569A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical film preparation, and in particular relates to a method for preparing a metal film wide spectrum attenuation film. Background Art
[0002] In recent years, with the rapid progress of optical materials, photoelectric detection devices, and computer software, optoelectronic systems are increasingly developing towards light weight, multi-functionality, miniaturization, and integration. Such an optoelectronic system must contain many optical paths and detection devices, and a wide spectral region will be used. The wide spectrum needs to be separated, selected, and attenuated to achieve effective use of the wide spectrum and the application of different spectra for different optical paths and detection devices. Therefore, attenuation devices are widely used in such military and civilian optoelectronic systems, such as CCD cameras, short-wave infrared imaging, laser imaging, security monitoring, etc. The spectral attenuation area of the attenuation sheet, the uniformity of the attenuation area, and the attenuation transmittance are the key core components that determine the attenuation performance of the attenuation device.
[0003] However, in practical applications, the existing dielectric film wide spectrum attenuation film has problems such as color cast distortion and noise interference in the optoelectronic system due to its narrow bandwidth and large deviation. Therefore, the field urgently needs to develop a new method for manufacturing a metal film wide spectrum attenuation film. Summary of the invention
[0004] The purpose of the present invention is to solve the above-mentioned technical problems and to propose a method for manufacturing a metal film wide spectrum attenuation film to solve the problems of color cast distortion, noise interference, etc. in the optoelectronic system caused by the narrow bandwidth and large deviation of the existing dielectric film wide spectrum attenuation film in practical applications.
[0005] The technical solution proposed in the present application is: a method for producing a metal film-based wide-spectrum attenuation film, by preparing a metal alloy film system with a "Cr+Ag+Cr" sandwich structure of different thicknesses on the surface of an optical glass substrate by a vacuum coating method, to obtain a metal film-based wide-spectrum attenuation film with a variable attenuation transmittance from 0% to 10% and a uniform attenuation effect with a deviation of less than ±1.0% in the wavelength region of 0.4μm to 2.5μm, wherein the purity of Cr and Ag is both above 99.99%.
[0006] Preferably, a method for manufacturing a metal film wide spectrum attenuation sheet of the present application specifically comprises the following steps:
[0007] S1. K9 crown optical glass is selected as the optical glass substrate; this optical glass has strong mechanical properties, high chemical stability, good environmental adaptability, and is not easy to produce a metamorphic layer in the atmospheric environment.
[0008] S2. Select metal materials Ag and Cr as optical thin film materials, and use the "Cr+Ag+Cr" sandwich structure as a metal alloy film system; the metal alloy film system uses the Cr film with strong mechanical properties and high chemical stability to protect the Ag film with weak mechanical properties and poor chemical stability, thereby preventing the Ag film from being mechanically damaged, chemically deteriorating and falling off; the Cr film with strong bonding strength connects the optical glass substrate and the Ag film, thereby preventing the Ag film from falling off due to the weak bonding strength between the Ag film and the optical glass.
[0009] S3. Calculate the physical thickness of each film layer in the metal alloy film system and the corresponding quarter-center wavelength optical thickness coefficient when achieving an attenuation transmittance of 0% to 10% in the spectral wavelength region of 0.4 μm to 2.5 μm based on the metal spectral characteristic parameters of Ag and Cr;
[0010] S4. According to the physical thickness of the film layer determined in step S3, a Cr film is plated using an ion source assisted coating machine in an ion source assisted manner. This is because the chemical activity of Cr is weak, and ion source assistance can improve the density and firmness of the Cr film. A dense and firm film layer is beneficial to preventing the film layer from falling off the optical glass substrate, and is beneficial to protecting the Ag film, preventing the atmosphere from corroding the Ag film, and improving the environmental adaptability of the product. The Ag film is plated in a non-ion source assisted manner. This is because the chemical activity of Ag is strong, which prevents the Ag film from reacting with weak impurities in the ion source assisted ion beam, causing the spectral characteristic parameters of the Ag film to deviate.
[0011] S5. Use a spectrometer to measure the spectral characteristics of the metal film wide spectrum attenuation film to obtain a qualified metal film wide spectrum attenuation film. The spectrometer is an Agilent Cary 7000 UV-VIS-NIR fully automatic spectrometer from the United States or a Shimadzu FTIR-8400S Fourier transform infrared spectrometer from Japan.
[0012] Preferably, step S3 includes the following steps:
[0013] Step S31, calculate or select the complex refractive index or refractive index of the corresponding film layer according to the following formula:
[0014] Ag complex refractive index: η2 = n Ag -ik Ag ;
[0015] Complex refractive index of Cr: η1=η3=n Cr -ik Cr ;
[0016] Refractive index of optical glass substrate: η g =n glass ;
[0017] Refractive index of air: η a =nAir ;
[0018] Step S32, calculating the phase thickness of the corresponding film layer at the corresponding thickness according to the following formula:
[0019] Assuming that the physical thickness of the first Cr film is d1, the corresponding phase thickness is:
[0020]
[0021] Assuming that the physical thickness of the second Ag film is d2, the corresponding phase thickness is:
[0022]
[0023] Assuming that the physical thickness of the third Cr film is d3, its corresponding phase thickness is:
[0024]
[0025] Step S33, respectively obtain the characteristic matrix of each film layer and the entire metal alloy film system:
[0026] Among them, the characteristic matrix of the first layer of Cr film is:
[0027]
[0028] The characteristic matrix of the second Ag film is:
[0029]
[0030] The characteristic matrix of the third Cr film is:
[0031]
[0032] The characteristic matrix of the entire metal alloy film system is listed as follows:
[0033]
[0034] get:
[0035]
[0036] Step S34, substituting the corresponding spectral wavelength data and attenuation transmittance data into the characteristic matrix of step S33, and calculating the phase thickness of each film layer;
[0037] Step S35, substituting the phase thickness of each film layer into the corresponding formula in step S32 to calculate the physical thickness of each film layer;
[0038] Step S36, calculating the quarter central wavelength optical thickness coefficient α, the calculation formula is as follows:
[0039] Thickness = αλ4n,
[0040] Thickness is the physical thickness of each film layer, λ is the spectral wavelength, and n is the refractive index of the film material at the spectral wavelength.
[0041] Preferably, according to step S36, when the spectrum wavelength λ is 0.55 μm, it is calculated that 0.005≤a≤0.012; and then the film structure of the metal film wide spectrum attenuation plate is determined as:
[0042] Sub / (36a)L(a)H(36a)L / Air;
[0043] Wherein, Sub is the optical glass substrate, Air is air, H is Ag, L is Cr, and α is the optical thickness coefficient of one quarter of the central wavelength.
[0044] Preferably, step S4 includes the following steps:
[0045] S41. Maintain the vacuum coating room environment: temperature: 22℃~26℃, humidity: 40%~60%, cleanliness: Class 10,000;
[0046] S42. Use absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume to clean the optical glass substrate, and use the breath method to check the cleanliness of the parts. If the surface of the parts is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are marks, it should be wiped further. After cleaning, load it into the ion source assisted coating machine and evacuate it;
[0047] S43, when the vacuum degree is higher than 6×10 -2 When the temperature is Pa, the optical glass substrate is baked at 120°C and kept at a constant temperature for 30min to 40min, which can improve the surface activity of the substrate and help improve the firmness of the film.
[0048] S44, continue to evacuate, when the vacuum degree is higher than 2×10 -3 When the pressure is 0.0457 W / m, two argon gases are introduced into the ion source auxiliary coating machine. The gas flow rate of the first argon gas is 4 sccm, which is used to generate ions. The gas flow rate of the second argon gas is 8 sccm, which is used to protect the entire gas space of the ion source and prevent external gas from rushing into the discharge space of the ion source, playing the role of an air curtain. The APS ion source is turned on to clean the optical glass substrate under the process parameters of a discharge current of 50 A, a deflection voltage of 120 V and a temperature of 120 ° C. The cleaning time is 10 min to remove dust and water vapor on the surface of the optical glass substrate and reduce the occurrence of metal film defects.
[0049] S45 , according to the physical thickness of the film layer determined in step S3 , and according to the set APS ion source assisted film coating process parameters, a first layer of Cr film, a second layer of Ag film and a third layer of Cr film are sequentially plated.
[0050] Preferably, in step S45, when the first and third Cr films are plated, the APS ion source is turned on, and the APS ion source-assisted film-plating process parameters are set as follows:
[0051] The gas flow rate of the first argon gas is 2 sccm, the gas flow rate of the second argon gas is 16 sccm, the discharge current is 50A, the deflection voltage is 120V and the temperature is 120°C;
[0052] Preferably, in step S45, when the second layer of Ag film is plated, the APS ion source is turned off, and the plating is performed at a rate of 0.2 nm / s at a temperature of 120°C.
[0053] Preferably, the ion source assisted coating machine adopts the German SYRUSpro1100 coating machine.
[0054] The present invention also includes other steps or devices that can enable the normal use of a method for manufacturing a metal film wide spectrum attenuation plate, which are conventional means in the field. In addition, steps or devices not limited in the present invention all adopt the existing technology in the field.
[0055] The working principle of the present invention is as follows: (1) the present invention can obtain different attenuation characteristics by plating different metal film thicknesses, and the attenuation transmittance can be adjusted from 0% to 10% to meet the needs of attenuation devices with different requirements; (2) the attenuation characteristics of metal Cr and metal Ag are opposite in the 0.4μm to 2.5μm spectral region, and the attenuation characteristics of the two metal materials compensate and inhibit each other, and the wide spectrum uniformity is better, and a uniformity deviation of less than ±1.0% can be obtained; (3) Metal Ag has poor bonding strength with optical glass, poor mechanical properties, and is easily damaged and detached. However, by utilizing the strong bonding strength of metal Cr with optical glass and metal Ag, and strong mechanical properties, metal Cr is placed in a sandwich structure of the bottom connecting layer and the top protective layer, and the environmental adaptability is better.
[0056] Compared with the prior art, the invention has the following beneficial effects: the product has a simple structure and is easy to prepare; the metal film has the advantages of being resistant to sand and dust friction, atmospheric erosion, and strong environmental adaptability, and is easy to promote. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 This is the attenuation spectrum characteristic of 20nm thick silver (Ag) (the horizontal axis represents wavelength and the vertical axis represents transmittance).
[0058] Figure 2This is the attenuation spectrum characteristic of 20nm thick silver (Cr) (the horizontal axis represents wavelength and the vertical axis represents transmittance).
[0059] Figure 3 Spectral characteristic curve of the metal film wide spectrum attenuation plate in the embodiment.
[0060] Figure 4 Schematic diagram of the film layer structure of the metal film wide spectrum attenuation film in the embodiment.
[0061] Figure 5 It is the measured spectral characteristic curve of the metal film wide spectrum attenuation plate specifically used in the embodiment. DETAILED DESCRIPTION
[0062] The technology of the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0063] Example
[0064] like Figures 1 to 4 As shown, this embodiment proposes a method for manufacturing a metal film wide spectrum attenuation sheet, comprising the following steps:
[0065] S1. K9 crown optical glass produced by Chengdu Guangming Optoelectronics Co., Ltd. was selected as the optical glass substrate. This optical glass has strong mechanical properties, high chemical stability, good environmental adaptability, and is not easy to produce a metamorphic layer in the atmospheric environment.
[0066] S2. Select metal materials Ag and Cr as optical thin film materials, wherein the purity of Cr and Ag is above 99.99%. And use the "Cr+Ag+Cr" sandwich structure as a metal alloy film system; the metal alloy film system uses the Cr film with strong mechanical properties and high chemical stability to protect the Ag film with weak mechanical properties and poor chemical stability, preventing the Ag film from being mechanically damaged, chemically deteriorated and falling off; the Cr film with strong bonding strength connects the optical glass substrate and the Ag film, preventing the Ag film from falling off due to the weak bonding strength between the Ag film and the optical glass.
[0067] S3. According to the metal spectral characteristic parameters of Ag and Cr (as shown in Table 1 below), the physical thickness of each film layer in the metal alloy film system and the corresponding quarter center wavelength optical thickness coefficient are calculated when an attenuation transmittance of 0% to 10% is achieved in the spectral wavelength region of 0.4 μm to 2.5 μm;
[0068] Table 1 Spectral characteristic parameters of metal materials
[0069]
[0070] S4. According to the physical thickness of the film layer determined in step S3, a Cr film is plated using a German SYRUSpro1100 coating machine under ion source assistance. This is because the chemical activity of Cr is weak, and ion source assistance can improve the density and firmness of the Cr film. A dense and firm film layer is beneficial to preventing the film layer from falling off the optical glass substrate, and is beneficial to protecting the Ag film, preventing the atmosphere from corroding the Ag film, and improving the environmental adaptability of the product; the Ag film is plated without the assistance of an ion source. This is because the chemical activity of Ag is strong, which prevents the Ag film from reacting with weak impurities in the ion beam assisted by the ion source, causing the spectral characteristic parameters of the Ag film to deviate.
[0071] S5. Use a spectrometer to measure the spectral characteristics of the metal film wide spectrum attenuation film to obtain a qualified metal film wide spectrum attenuation film. The spectrometer is an American Agilent Cary 7000 UV-VIS-NIR fully automatic spectrometer or a Japanese Shimadzu FTIR-8400S Fourier transform infrared spectrometer. Figure 3 As shown, after measurement, the spectral characteristics of the metal film wide spectrum attenuation plate prepared according to the present invention meet the manufacturing requirements (the horizontal axis in the figure represents the wavelength, and the vertical axis represents the transmittance), the average transmittance in the wavelength region of 0.4μm to 2.5μm is ≤10%, and the uniformity is ≤±1.0%.
[0072] Specifically, step S3 includes the following steps:
[0073] Step S31, calculate or select the complex refractive index or refractive index of the corresponding film layer according to the following formula:
[0074] Ag complex refractive index: η2 = n Ag -ik Ag ;
[0075] Complex refractive index of Cr: η1=η3=n Cr -ik Cr ;
[0076] Refractive index of optical glass substrate: η g =n glass ;
[0077] Refractive index of air: η a =n Air ;
[0078] Step S32, calculating the phase thickness of the corresponding film layer at the corresponding thickness according to the following formula:
[0079] Assuming that the physical thickness of the first Cr film is d1, the corresponding phase thickness is:
[0080]
[0081] Assuming that the physical thickness of the second Ag film is d2, the corresponding phase thickness is:
[0082]
[0083] Assuming that the physical thickness of the third Cr film is d3, its corresponding phase thickness is:
[0084]
[0085] Step S33, respectively obtain the characteristic matrix of each film layer and the entire metal alloy film system:
[0086] Among them, the characteristic matrix of the first layer of Cr film is:
[0087]
[0088] The characteristic matrix of the second Ag film is:
[0089]
[0090] The characteristic matrix of the third Cr film is:
[0091]
[0092] The characteristic matrix of the entire metal alloy film system is listed as follows:
[0093]
[0094] get:
[0095]
[0096] Step S34, substituting the corresponding spectral wavelength data and attenuation transmittance data into the characteristic matrix of step S33, and calculating the phase thickness of each film layer;
[0097] Step S35, substituting the phase thickness of each film layer into the corresponding formula in step S32 to calculate the physical thickness of each film layer;
[0098] Step S36, calculate the quarter center wavelength optical thickness coefficient α (as shown in Table 2 below), the calculation formula is as follows:
[0099] Thickness = αλ4n,
[0100] Thickness is the physical thickness of each film layer, λ is the spectral wavelength, where λ is 0.55μm, and n is the refractive index of the film material at the spectral wavelength.
[0101] Table 2 Attenuation characteristics of different metal film thicknesses
[0102] Alpha value Attenuation Transmittance 0.005 10% 0.006 7.00% 0.007 5.00% 0.008 3.30% 0.009 2.20% 0.01 1.60% 0.011 1.20% 0.012 0.80%
[0103] According to step S36, when the spectrum wavelength λ is 0.55 μm, it is calculated that 0.005≤a≤0.012; and then the film structure of the metal film wide spectrum attenuation plate is determined as:
[0104] Sub / (36a)L(a)H(36a)L / Air;
[0105] Wherein, Sub is the optical glass substrate, Air is air, H is Ag, L is Cr, and α is the optical thickness coefficient of one quarter of the central wavelength.
[0106] In this embodiment, step S4 includes the following steps:
[0107] S41. Maintain the vacuum coating room environment: temperature: 22℃~26℃, humidity: 40%~60%, cleanliness: Class 10,000;
[0108] S42. Use absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume to clean the optical glass substrate, and use the breath method to check the cleanliness of the parts. If the surface of the parts is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are marks, it should be wiped further. After cleaning, load it into the ion source assisted coating machine and evacuate it;
[0109] S43, when the vacuum degree is higher than 6×10 -2 When the temperature is Pa, the optical glass substrate is baked at 120°C and kept at a constant temperature for 30min to 40min, which can improve the surface activity of the substrate and help improve the firmness of the film.
[0110] S44, continue to evacuate, when the vacuum degree is higher than 2×10 -3 When the pressure is 0.0457 W / m, two argon gases are introduced into the ion source auxiliary coating machine. The gas flow rate of the first argon gas is 4 sccm, which is used to generate ions. The gas flow rate of the second argon gas is 8 sccm, which is used to protect the entire gas space of the ion source and prevent external gas from rushing into the discharge space of the ion source, playing the role of an air curtain. The APS ion source is turned on to clean the optical glass substrate under the process parameters of a discharge current of 50 A, a deflection voltage of 120 V and a temperature of 120 ° C. The cleaning time is 10 min to remove dust and water vapor on the surface of the optical glass substrate and reduce the occurrence of metal film defects.
[0111] S45 , according to the physical thickness of the film layer determined in step S3 , and according to the set APS ion source assisted film coating process parameters, a first layer of Cr film, a second layer of Ag film and a third layer of Cr film are sequentially plated.
[0112] Preferably, in step S45, when the first and third Cr films are plated, the APS ion source is turned on, and the APS ion source-assisted film-plating process parameters are set as follows:
[0113] The gas flow rate of the first argon gas is 2 sccm, the gas flow rate of the second argon gas is 16 sccm, the discharge current is 50A, the deflection voltage is 120V and the temperature is 120°C;
[0114] In the step S45, when the second layer of Ag film is plated, the APS ion source is turned off, and the plating is performed at a rate of 0.2 nm / s at a temperature of 120°C.
[0115] The present application uses a vacuum coating method to prepare a metal alloy film system of a "Cr+Ag+Cr" sandwich structure of different thicknesses on the surface of an optical glass substrate, thereby obtaining a metal film system wide spectrum attenuation sheet with a variable attenuation transmittance from 0% to 10% and a uniform attenuation effect with a deviation of less than ±1.0% in the wavelength region of 0.4μm to 2.5μm. The working principle of the metal film system wide spectrum attenuation sheet is as follows: (1) The present application can obtain different attenuation characteristics by coating different metal film thicknesses, and the attenuation transmittance can be adjusted from 0% to 10% to meet the attenuation requirements of different needs. (1) Reduce the demand for devices; (2) The attenuation characteristics of metal Cr and metal Ag are opposite in the 0.4μm to 2.5μm spectral region. The attenuation characteristics of the two metal materials compensate and inhibit each other, and the wide spectrum uniformity is better, and a uniformity deviation of less than ±1.0% can be obtained; (3) Metal Ag has poor bonding with optical glass and poor mechanical properties, and is easily damaged and detached. However, by utilizing the strong bonding between metal Cr and optical glass and metal Ag, and the strong mechanical properties, metal Cr is placed in a sandwich structure between the bottom connection layer and the top protective layer, which has better environmental adaptability.
[0116] It should be noted that, in this embodiment, the alcohol-ether mixture meets the requirements of GB / T 678, including ethanol (anhydrous ethanol) and ether (meeting the requirements of GB / T 12591). In addition, the present application uses TFC optical thin film software for optical thin film analysis.
[0117] Specific applications:
[0118] Prepare optical parts with a diameter of 50mm and a thickness of 3mm. The optical material is K9 (for surface quality inspection of optical parts, there is no deterioration layer, cracks and paths on the surface, which meets the requirements of 3×0.1 in GB / T 1185-2006). The attenuation requirements are as follows:
[0119] Tave≈2.2%, uniformity≤±1.0%, and the rest refer to the following industry standards: JB / T8226.8-1999.
[0120] According to the above technical indicators, the α value is taken as 0.009. The spectral characteristic parameters of metal materials are consulted. The material refractive index n of metal chromium (Cr) at a spectral wavelength of 0.55μm is 3.16. The thickness of each chromium film is calculated to be 14.1nm. The spectral characteristic parameters of metal materials are consulted. The material refractive index n of metal silver (Ag) at a spectral wavelength of 0.55μm is 0.055. The thickness of each silver film is calculated to be 22.5nm.
[0121] The first layer of 14.1 nm chromium film, the second layer of 22.5 nm silver film and the third layer of 14.1 nm chromium film were sequentially prepared on the substrate by the above-mentioned vacuum coating method to obtain a metal film-based wide spectrum attenuation plate.
[0122] like Figure 5 As shown, the spectral characteristics are measured by a spectrometer. The average transmittance of the product in the spectral wavelength region of 0.4μm to 2.5μm is Tave≈2.2%, and the uniformity is ≤±1.0%; the film characteristics meet the JB / T8226.8-1999 standard.
[0123] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for manufacturing a metal film wide spectrum attenuation sheet, characterized in that: By using a vacuum coating method to prepare a metal alloy film system with a "Cr+Ag+Cr" sandwich structure of different thicknesses on the surface of an optical glass substrate, a metal film system wide spectrum attenuation sheet with a variable attenuation transmittance from 0% to 10% and a uniform attenuation effect with a deviation of less than ±1.0% in the spectral wavelength region of 0.4μm to 2.5μm is obtained.
2. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 1, characterized in that: The steps include: S1. Select K9 crown optical glass as the optical glass substrate; S2, selecting metal materials Ag and Cr as optical thin film materials, and using a "Cr+Ag+Cr" sandwich structure as a metal alloy film system; S3. Calculate the physical thickness of each film layer in the metal alloy film system and the corresponding quarter-center wavelength optical thickness coefficient when achieving an attenuation transmittance of 0% to 10% in the spectral wavelength region of 0.4 μm to 2.5 μm based on the metal spectral characteristic parameters of Ag and Cr; S4, according to the physical thickness of the film layer determined in step S3, using an ion source assisted coating machine to plate a Cr film in an ion source assisted manner, and to plate an Ag film in a non-ion source assisted manner; S5. Use a spectrometer to measure the spectral characteristics of the metal film wide spectrum attenuation sheet to obtain a qualified metal film wide spectrum attenuation sheet.
3. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 2, characterized in that: Step S3 includes the following steps: Step S31, calculate or select the complex refractive index or refractive index of the corresponding film layer according to the following formula: Ag complex refractive index: η2 = n Ag -ik Ag ; Complex refractive index of Cr: η1=η3=n Cr -ik Cr ; Refractive index of optical glass substrate: η g =n glass ; Refractive index of air: η a =n Air ; Step S32, calculating the phase thickness of the corresponding film layer at the corresponding thickness according to the following formula: Assuming that the physical thickness of the first Cr film is d1, the corresponding phase thickness is: Assuming that the physical thickness of the second Ag film is d2, the corresponding phase thickness is: Assuming that the physical thickness of the third Cr film is d3, its corresponding phase thickness is: Step S33, respectively obtain the characteristic matrix of each film layer and the entire metal alloy film system: Among them, the characteristic matrix of the first layer of Cr film is: The characteristic matrix of the second Ag film is: The characteristic matrix of the third Cr film is: The characteristic matrix of the entire metal alloy film system is listed as follows: get: Step S34, substituting the corresponding spectral wavelength data and attenuation transmittance data into the characteristic matrix of step S33, and calculating the phase thickness of each film layer; Step S35, substituting the phase thickness of each film layer into the corresponding formula in step S32 to calculate the physical thickness of each film layer; Step S36, calculating the quarter central wavelength optical thickness coefficient α, the calculation formula is as follows: Thickness = αλ4n, Thickness is the physical thickness of each film layer, λ is the spectral wavelength, and n is the refractive index of the film material at the spectral wavelength.
4. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 3, characterized in that: According to step S36, when the spectrum wavelength λ is 0.55 μm, it is calculated that 0.005≤a≤0.012; and then the film structure of the metal film wide spectrum attenuation plate is determined as: Sub / (36a)L(a)H(36a)L / Air; Wherein, Sub is the optical glass substrate, Air is air, H is Ag, L is Cr, and α is the optical thickness coefficient of one quarter of the central wavelength.
5. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 2, characterized in that: The step S4 includes the following steps: S41. Maintain the vacuum coating room environment: temperature: 22℃~26℃, humidity: 40%~60%, cleanliness: Class 10,000; S42. Use absorbent gauze dipped in a 1:1 alcohol-ether mixture by volume to clean the optical glass substrate, and use the breath method to check the cleanliness of the parts. If the surface of the parts is evenly covered with air after the breath, it is clean. If the surface is unevenly covered with air or there are marks, it should be wiped further. After cleaning, load it into the ion source assisted coating machine and evacuate it; S43, when the vacuum degree is higher than 6×10 -2 Pa, the optical glass substrate is baked at 120°C and kept at a constant temperature for 30min to 40min to improve the firmness of the film; S44, continue to evacuate, when the vacuum degree is higher than 2×10 -3 When the pressure drops to 1.5 Pa, two argon gases are introduced into the ion source auxiliary coating machine, wherein the gas flow rate of the first argon gas is 4 sccm, which is used to generate ions, and the gas flow rate of the second argon gas is 8 sccm, which is used to protect the entire gas space of the ion source and prevent external gas from rushing into the discharge space of the ion source, acting as an air curtain. The APS ion source is turned on to clean the optical glass substrate under the process parameters of a discharge current of 50 A, a deflection voltage of 120 V and a temperature of 120 ° C. The cleaning time is 10 min to remove dust and water vapor on the surface of the optical glass substrate. S45 , according to the physical thickness of the film layer determined in step S3 , and according to the set APS ion source assisted film coating process parameters, a first layer of Cr film, a second layer of Ag film and a third layer of Cr film are sequentially plated.
6. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 5, characterized in that: In step S45, when the first and third layers of Cr films are plated, the APS ion source is turned on, and the APS ion source-assisted film-plating process parameters are set as follows: The gas flow rate of the first argon gas is 2 sccm, the gas flow rate of the second argon gas is 16 sccm, the discharge current is 50 A, the deflection voltage is 120 V and the temperature is 120° C.
7. The method for manufacturing a metal film wide spectrum attenuation sheet according to claim 6, characterized in that: In the step S45, when the second layer of Ag film is plated, the APS ion source is turned off, and the plating is performed at a rate of 0.2 nm / s at a temperature of 120°C.
8. A method for manufacturing a metal film wide spectrum attenuation sheet according to any one of claims 2 to 7, characterized in that: The ion source assisted coating machine adopts the German SYRUSpro1100 coating machine.
Citation Information
Patent Citations
Third surface metallic film for automobile semi-reflecting semi-transparent type electrochromic inner rearview mirror
CN106802437A
Silver-based film structure capable of efficiently reflecting ultraviolet light, visible light and infrared light and film coating method
CN110488402A
Ultra-wide passband short-wave pass filter film and preparation method thereof
CN111766655A
Preparation method of ultra-wide passband short-wave pass filter film
CN114415281A
Ultraviolet induced transmission band-pass optical filter and preparation method thereof