Manufacturing method of tunnel sprayed concrete
By optimizing the formulation of jet concrete, combining ZP-1 catalyst and modified nanozeolite powder, the problem of high rebound rate of jet concrete in tunnel construction is solved, and the effect of low rebound rate, high strength and high efficiency construction is achieved.
Patent Information
- Application Number
- CN202411114756.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
In tunnel construction, the rebound rate of sprayed concrete is high, resulting in serious over-consuming concrete. It is difficult for the existing technology to maintain the early strength and solidification speed of concrete while reducing the rebound rate. There are balance problems with the use of existing catalysts.
Using specific ratios of cement, active additives, fine aggregates, coarse aggregates, catalysts and quick-setting agents, including the use of ZP-1 catalysts and modified nanozeolite powders, through the combination of fly ash and composite dispersants , optimize the formulation of sprayed concrete, reduce rebound rate and improve the strength and compactness of concrete.
It significantly reduces the rebound amount of sprayed concrete, improves the compressive strength of concrete for one day and 28 days, shortens the initial settling time, reduces the amount of cement and quick-setting agent, and improves the construction efficiency and the comprehensive performance of materials.
Smart Images

Figure BDA0004993315600000071 
Figure BDA0004993315600000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of shotcrete, in particular to a method for preparing tunnel shotcrete. Background Art
[0002] In tunnel construction, shotcrete is often used in tunnels with complex geological conditions and weak tunnel walls. It has the advantages of fast construction speed and high efficiency: the concrete mixture is sprayed directly onto the tunnel rock layer or the surface of the initial support part using a sprayer, eliminating the process of template construction and disassembly, and significantly improving the construction speed; shotcrete can fit tightly to the tunnel rock layer, effectively fill the gaps between rocks, improve the integrity and stability of the surrounding rock, and prevent rock shedding and water seepage; at the same time, the sprayed concrete can form a relatively uniform concrete layer, improving the overall quality of the tunnel.
[0003] However, in actual tunnel construction, over-consumption of shotcrete is quite common. Generally, concrete consumption is reduced by controlling the smooth blasting effect of the tunnel, strengthening on-site management, and reducing over-excavation. However, the rebound of shotcrete accounts for a large proportion of the over-consumption of concrete. In order to reduce the rebound rate, the existing technology generally adopts the addition of external catalysts to reduce the rebound of shotcrete, but it may reduce the early strength and solidification speed of concrete. The use of external catalysts and the comprehensive strength of concrete cannot reach a balance point.
[0004] Therefore, it is of great significance to find a method for producing tunnel shotcrete with low rebound rate, high strength and high comprehensive performance. Summary of the invention
[0005] The object of the present invention is to provide a method for producing tunnel shotcrete to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A tunnel shotcrete comprises the following raw materials in parts by weight: 310-330 parts of cement, 145-155 parts of active additives, 910-930 parts of fine aggregate, 775-790 parts of coarse aggregate, 175-185 parts of water, 3.5-4 parts of water reducer, 4.5-5 parts of catalyst, and 23-24 parts of accelerator.
[0008] More preferably, the cement is P.O42.5 silicate cement.
[0009] Preferably, the fine aggregate is medium sand with a fineness modulus Mx of 2.8 to 3.0; the coarse aggregate is crushed stone with a particle size of 5 to 10 mm; the catalyst is a ZP-1 type catalyst; and the water reducer is a slow-setting water reducer.
[0010] Among them, the ZP-1 type catalyst, similar to an accelerator, can make the shotcrete quickly hydrate, release heat, solidify, and strengthen early, reduce the falling blocks and rebound rate of concrete, and can also correct the state of concrete to prevent the concrete from clogging the pipe. Moreover, this catalyst will not have an accelerated setting effect when an accelerator is not added, so it can be added to the concrete alone in advance.
[0011] More preferably, the active additive includes fly ash; the fly ash is Class F Grade II fly ash; and the accelerator includes YTF-1 alkali-free accelerator.
[0012] Fly ash has volcanic ash activity. After adding water, it can react with the cement of concrete to form a water-insoluble calcium silicate gel, thereby reducing the possibility of dissolution, filling the internal pores of concrete, improving the strength and impermeability of concrete, and also reducing the water demand, reducing early drying shrinkage, and improving the compactness of concrete. The spherical glass particles of fly ash have a smooth surface, fine particle size, and compact texture, which can reduce the friction resistance of concrete to the pump pipe of the spraying machine and improve the performance of sprayed concrete.
[0013] Preferably, the active additive further comprises modified nano zeolite powder; the active additive comprises the following raw materials in parts by weight: 105-110 parts of fly ash and 40-45 parts of modified nano zeolite powder.
[0014] Preferably, the accelerator further comprises a composite dispersant; the accelerator comprises the following raw materials in parts by weight: 14 to 16 parts of YTF-1 alkali-free accelerator and 7 to 10 parts of composite dispersant.
[0015] Preferably, the modified nano zeolite powder comprises the following raw materials in parts by mass: 5 to 8 parts of nano zeolite powder, 70 to 80 parts of deionized water, 6 to 10 parts of γ-aminopropyltriethoxysilane, 15 to 20 parts of acrylic anhydride, 140 to 170 parts of N-methylpyrrolidone, 8 to 10 parts of hydroxy-polyethylene glycol-thiol, and 1 to 2 parts of azobisisobutyronitrile.
[0016] Preferably, the molecular weight of hydroxy-polyethylene glycol-thiol is 2000-3000.
[0017] Preferably, the preparation of the modified nano zeolite powder includes the following method: (1) adding nano zeolite powder to deionized water for ultrasonic dispersion, then adding γ-aminopropyltriethoxysilane, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder A; (2) ultrasonically dispersing modified nano zeolite powder A and acrylic anhydride in N-methylpyrrolidone, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder B; (3) ultrasonically dispersing modified nano zeolite powder B, hydroxy-polyethylene glycol-thiol, and azobisisobutyronitrile in N-methylpyrrolidone, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder.
[0018] In a further scheme, modified nano zeolite powder is used to partially replace fly ash to further improve the comprehensive performance of shotcrete. Among them, nano zeolite powder has extremely small particle size and high specific surface area, can well fill the tiny gaps of concrete, and can act on the products after cement hydration to form a more compact structure, improve the density and strength of concrete. At the same time, nano zeolite powder, as a mineral admixture, can also reduce the amount of cement and reduce energy consumption. At the same time, in order to further improve the comprehensive performance of concrete, the surface of nano zeolite powder is also modified, and organic functional groups such as amino, carboxyl, ether, and hydroxyl are introduced to enhance the surface activity of nano zeolite powder. When added to concrete, the interaction force between the nano zeolite powder and the concrete substrate can be enhanced, and the carboxylic acid and amino groups can form a chemical bond with the calcium ions in the concrete hydration products, thereby improving the interfacial bonding force. Ether, hydroxyl, and thiol improve the dispersibility of modified nano zeolite powder in concrete, and also improve the overall fluidity and water retention of concrete, further improving the comprehensive strength and performance of concrete.
[0019] Preferably, in process (1), the ultrasonic dispersion temperature is 30-40°C, the ultrasonic power is 200-250W, and the ultrasonic time is 20-30min; the heating temperature is 85-95°C, the electric stirring speed is 2000-3000r / min, and the time is 3-4h.
[0020] Preferably, in process (2), the heating temperature is 73-89° C., the electric stirring speed is 2000-3000 r / min, and the time is 3-4 h.
[0021] Preferably, in process (3), the heating temperature is 75-85°C, the electric stirring speed is 2000-3000 r / min, and the time is 3-4 h.
[0022] Preferably, the composite dispersant comprises the following substances in parts by mass: 10 to 15 parts of polyacrylic acid, 15 to 17 parts of ethanolamine, 3 to 5 parts of phosphoric acid, and 2 to 3 parts of p-toluenesulfonic acid.
[0023] More preferably, the molecular weight of the polyacrylic acid is 2000-5000.
[0024] Preferably, the preparation method of the composite dispersant comprises the following method: dispersing polyacrylic acid in deionized water, adding ethanolamine, phosphoric acid and p-toluenesulfonic acid respectively, and heating and electromagnetic stirring to obtain the composite dispersant.
[0025] More preferably, during the heating and stirring process, the heating temperature is 80-90° C., the electromagnetic stirring speed is 2000-3000 r / min, and the electromagnetic stirring time is 0.5-1 h.
[0026] In a further solution, a composite dispersant is introduced to further improve the comprehensive performance of shotcrete. Among them, polyacrylic acid is a highly efficient anionic dispersant that prevents particle agglomeration through electrostatic repulsion and steric hindrance effect, thereby improving the dispersion and uniformity of the accelerator in concrete. Ethanolamine can improve the wettability of the accelerator to concrete particles and promote the penetration and distribution of the accelerator in concrete. At the same time, a part of the polyacrylic acid and ethanolamine produce an interfacial effect, further improving the steric hindrance effect, promoting the dispersion of the accelerator in concrete, and can also form a thin film on the surface of the concrete, thereby improving the comprehensive strength and performance of the concrete.
[0027] Preferably, a method for making tunnel shotcrete comprises the following steps:
[0028] S1: Add coarse aggregate, part of fine aggregate and cement into a mixer in sequence and mix them evenly; then, during the mixing process, gradually add the remaining fine aggregate, active additives, water and water reducing agent in batches and mix them evenly to obtain a rough shotcrete mixture;
[0029] S2: adding a catalyst and an accelerating agent to the above-mentioned rough shotcrete mixture, stirring for 2 to 3 minutes to obtain a shotcrete mixture;
[0030] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0031] Compared with the prior art, the beneficial effects achieved by the present invention are: (1) By increasing the fly ash content in the concrete mix, the friction resistance of concrete to the pump pipe of the spraying machine is reduced, thereby improving the performance of the sprayed concrete. (2) The water-cement ratio of the sprayed concrete is reduced, and the 1-day and 28-day compressive strengths are increased. (3) Under the action of the catalyst, the initial setting time of the sprayed concrete can be significantly shortened, and the rebound of the sprayed concrete at the construction site can be reduced. (4) Under the condition of meeting the concrete strength, the externally added catalyst can significantly increase the fly ash content and reduce the cement and accelerator content, thereby saving costs and achieving the effect of reducing costs and increasing efficiency. (5) The use of modified nano zeolite to partially replace fly ash and further introduce a composite dispersant into the accelerator can further improve the comprehensive performance of the sprayed concrete. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In this embodiment, it should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions and exemplarily include: cement, P.O42.5, provided by Guizhou Ziyun Southwest Cement Co., Ltd.; fly ash, Class F II, provided by Xuanwei Power Generation Fly Ash Development Co., Ltd.; medium sand, Mx=2.9, provided by Puding County Huaqiang Building Materials Co., Ltd.; crushed stone, 5-10 mm, provided by Puding County Huaqiang Building Materials Co., Ltd.; water, drinking water, provided by Machang Town; water reducer, YTJ-1 high-performance water reducer (slow-setting type), provided by Yunnan Zhongtie New Materials Technology Co., Ltd.; accelerator, YTF-1 alkali-free accelerator (liquid), provided by Yunnan Zhongtie New Materials Technology Co., Ltd.; catalyst , ZP-1, provided by Chongqing Anorthite Building Materials Co., Ltd.; zeolite powder, purity 99%, provided by Wuhan Jiyesheng Chemical Co., Ltd.; γ-aminopropyltriethoxysilane, purity 99%, provided by Jinan Yongyue Chemical Co., Ltd.; acrylic anhydride, purity 99%, provided by Tianmen Hengchang Chemical Co., Ltd.; hydroxy-polyethylene glycol-mercapto, purity 99%, provided by Shanghai Zhenzhun Biotechnology Co., Ltd.; azobisisobutyronitrile, purity 99%, provided by Zouping Mingxing Chemical Co., Ltd.; polyacrylic acid, purity 99%, provided by Hubei Fangde New Materials Co., Ltd.; ethanolamine, purity 99.8%, provided by Changzhou Guxu Chemical Co., Ltd.; p-toluenesulfonic acid, purity 99%, provided by Nanjing Datang Chemical Co., Ltd.
[0034] In each embodiment, the preparation method of modified nano zeolite powder includes the following steps: (1) adding 7 parts of nano zeolite powder to 75 parts of deionized water, ultrasonically dispersing at 35°C with a power of 200 W for 25 minutes, adding 8 parts of silane coupling agent KH550 (γ-aminopropyltriethoxysilane), electromagnetically stirring at 2500 r / min for 3 hours at 90°C, filtering, washing and drying to obtain modified nano zeolite powder A; (2) adding 11 parts of modified nano zeolite powder A and 17 parts of Acrylic anhydride was added to 100 parts of N-methylpyrrolidone and ultrasonically dispersed, and then electromagnetically stirred at 2500 r / min for 5 hours at 85°C, filtered, washed and dried to obtain modified nano zeolite powder B; (3) 13 parts of modified nano zeolite powder B, 9 parts of hydroxy-polyethylene glycol-mercapto and 1 part of azobisisobutyronitrile were added to 55 parts of N-methylpyrrolidone and ultrasonically dispersed, and electromagnetically stirred at 2500 r / min for 3.5 hours at 80°C to obtain modified nano zeolite powder.
[0035] The preparation method of the composite dispersant comprises the following steps: adding 13 parts of polyacrylic acid to deionized water for ultrasonic dispersion, then adding 16 parts of ethanolamine, 4 parts of phosphoric acid and 2.5 parts of p-toluenesulfonic acid, and electromagnetically stirring at 2500 r / min for 0.5 h at 85° C. to obtain the composite dispersant.
[0036] Embodiment 1:
[0037] S1: 782 parts of crushed stone, 300 parts of sand and 320 parts of cement were added to a mixer in sequence and stirred, and then 619 parts of sand, 150 parts of fly ash, 179 parts of water and 3.76 parts of water reducing agent were gradually added in batches during the stirring process, and stirred evenly to obtain a rough shotcrete mixture;
[0038] S2: Add 4.7 parts of catalyst and 23.5 parts of YTF-1 alkali-free accelerating agent to the above-mentioned rough shotcrete, stir for 2 minutes, and obtain a shotcrete mixture;
[0039] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0040] Embodiment 2:
[0041] S1: 782 parts of crushed stone, 300 parts of sand and 320 parts of cement were added to a mixer in sequence and stirred evenly; then during the stirring process, 619 parts of sand, 107 parts of fly ash, 43 parts of modified nano zeolite powder, 179 parts of water and 3.76 parts of water reducing agent were gradually added in batches and stirred evenly to obtain a rough shotcrete mixture;
[0042] S2: Add 4.7 parts of catalyst, 15 parts of YTF-1 alkali-free quick-setting agent, and 8.5 parts of composite dispersant to the above-mentioned rough shotcrete mixture, and stir for 2 minutes to obtain a shotcrete mixture;
[0043] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0044] Embodiment 3:
[0045] S1: 775 parts of crushed stone, 300 parts of sand and 310-330 parts of cement are added to a mixer in sequence and stirred evenly; then, during the stirring process, 610 parts of sand, 105 parts of fly ash, 40 parts of modified nano zeolite powder, 175 parts of water and 3.5 parts of water reducing agent are gradually added in batches and stirred evenly to obtain a rough shotcrete mixture;
[0046] S2: Add 4.5 parts of catalyst, 14 parts of YTF-1 alkali-free quick-setting agent and 7 parts of composite dispersant to the above-mentioned rough shotcrete mixture, stir for 2 minutes to obtain a shotcrete mixture;
[0047] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0048] Embodiment 4:
[0049] S1: 790 parts of crushed stone, 310 parts of sand and 330 parts of cement were added to a mixer in sequence and stirred evenly; then during the stirring process, 620 parts of sand, 110 parts of fly ash, 45 parts of modified nano zeolite powder, 185 parts of water and 4 parts of water reducing agent were gradually added in batches and stirred evenly to obtain a rough shotcrete mixture;
[0050] S2: Add 5 parts of catalyst, 16 parts of YTF-1 alkali-free accelerating agent and 10 parts of composite dispersant to the above-mentioned rough shotcrete mixture, stir for 3 minutes to obtain a shotcrete mixture;
[0051] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0052] Comparative Example 1: Taking Example 1 as a control, Comparative Example 1 is the mix ratio of ordinary shotcrete, and the other processes remain unchanged.
[0053] S1: 801 parts of crushed stone, 320 parts of sand and 420 parts of cement were added to the mixer in sequence and mixed evenly, and then during the mixing process, 620 parts of sand, 189 parts of water and 4.2 parts of water reducing agent were gradually added in batches and mixed evenly to obtain a rough shotcrete mixture;
[0054] S2: adding 33.6 parts of YTF-1 alkali-free quick-setting agent to the above-mentioned rough shotcrete mixture and stirring for 2 minutes to obtain a shotcrete mixture;
[0055] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0056] Comparative Example 2: Using Example 2 as a control, Comparative Example 2 uses unmodified nano zeolite powder, and the rest of the process remains unchanged.
[0057] S1: 782 parts of crushed stone, 300 parts of sand and 320 parts of cement were added to a mixer in sequence and stirred evenly; then during the stirring process, 619 parts of sand, 107 parts of fly ash, 43 parts of nano zeolite powder, 179 parts of water and 3.76 parts of water reducing agent were gradually added in batches and stirred evenly to obtain a rough shotcrete mixture;
[0058] S2: Add 4.7 parts of catalyst, 15 parts of YTF-1 alkali-free quick-setting agent, and 8.5 parts of composite dispersant to the above-mentioned rough shotcrete mixture, and stir for 2 minutes to obtain a shotcrete mixture;
[0059] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0060] Comparative Example 3: Taking Example 2 as a control, no composite dispersant was added to Comparative Example 3, and the other processes remained unchanged.
[0061] S1: 782 parts of crushed stone, 300 parts of sand and 320 parts of cement were added to a mixer in sequence and stirred evenly; then during the stirring process, 619 parts of sand, 107 parts of fly ash, 43 parts of modified nano zeolite powder, 179 parts of water and 3.76 parts of water reducing agent were gradually added in batches and stirred evenly to obtain a rough shotcrete mixture;
[0062] S2: adding 4.7 parts of catalyst and 23.5 parts of YTF-1 alkali-free quick-setting agent to the above-mentioned rough shotcrete mixture, stirring for 2 minutes to obtain a shotcrete mixture;
[0063] S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.
[0064] Detection experiment 1:
[0065] The concrete working performance test was carried out on the shotcrete of Example 1 and the ordinary shotcrete of Comparative Example 1. The test results are shown in Table 1.
[0066]
[0067] Table 1
[0068] The water-binder ratio of shotcrete in Example 1 is smaller than that of ordinary shotcrete, which is more conducive to the quality assurance of shotcrete construction; the apparent density of shotcrete in Example 1 is 50kg / m smaller than that of ordinary shotcrete 3 , it is calculated that 2.1% of materials can be saved per cubic meter of concrete; the ratio of fly ash and cement in Example 1 shotcrete II is 8:17. Under the same construction equipment, environment and other conditions, compared with ordinary shotcrete, the pumping performance is improved, the pumping pressure is smaller, and the work efficiency per unit time is improved.
[0069] Test experiment 2: The rebound amount of the shotcrete of Example 1 and the ordinary shotcrete of Comparative Example 1 was measured and compared at the construction site. The test results are shown in Table 2.
[0070]
[0071] Table 2
[0072] For ordinary shotcrete, the average rebound of the arch is 16.6% after three measurements, and the average rebound of the arch waist is 7.4% after three measurements. For shotcrete of Example 1, the average rebound of the arch is 6.4% after three measurements, and the average rebound of the arch waist is 3.7% after three measurements. Compared with ordinary shotcrete, the shotcrete of Example 1 can reduce the rebound of shotcrete by 10.2% in the initial support construction of the arch, and can reduce the rebound of shotcrete by 3.7% in the initial support construction of the arch waist.
[0073] Test experiment 3: According to GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the concrete strength tests were carried out on each embodiment and comparative example at 1 day (1d) and 28 days (28d). The test results are shown in Table 3.
[0074] Concrete Type 1d strength / MPa 28d strength / MPa Example 1 Shotcrete 13.2 50.1 Example 2 Shotcrete 13.5 53.4 Example 3 Shotcrete 13.3 52.9 Example 4 Shotcrete 13.4 53.1 Comparative Example 1 Shotcrete 12.5 46.5 Comparative Example 2 Shotcrete 13.0 49.5 Comparative Example 3 Shotcrete 12.9 48.7
[0075] Table 3
[0076] Comparative Example 1: Taking Example 1 as a control, Comparative Example 1 is the mix ratio of ordinary shotcrete, and the other processes remain unchanged: Compared with Example 1, no external catalyst and fly ash are added. Due to the longer initial setting time, the early strength of ordinary concrete is not as good as that of Example 1; without adding fly ash, the later strength is also reduced.
[0077] Comparative Example 2: Using Example 2 as a control, Comparative Example 2 uses unmodified nano zeolite powder, and the rest of the process remains unchanged: the nano zeolite powder is not modified, has no active functional groups, has poor dispersibility in concrete, and the strength before and after is also reduced.
[0078] Comparative Example 3: Taking Example 2 as a control, no composite dispersant is added to Comparative Example 3, and the other processes remain unchanged: due to the lack of dispersant, the accelerator cannot be well dispersed in the concrete, and the fluidity will also be reduced, so that the strength of the concrete in the early and late stages is reduced.
[0079] Conclusion: By optimizing and changing the mix ratio of shotcrete, introducing active additives containing fly ash and modified nano-zeolite powder, accelerating setting agent containing YTF-1 alkali-free accelerating setting agent and composite dispersant, and introducing external catalyst, the early and late strengths of concrete are improved, while the rebound of shotcrete is reduced, thereby improving the comprehensive performance of shotcrete.
[0080] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for producing tunnel shotcrete, Features: The tunnel shotcrete comprises the following raw materials in parts by weight: 310-330 parts of cement, 145-155 parts of active additives, 910-930 parts of fine aggregate, 775-790 parts of coarse aggregate, 175-185 parts of water, 3.5-4 parts of water reducer, 4.5-5 parts of catalyst, and 23-24 parts of accelerator.
2. A method for producing tunnel shotcrete according to claim 1, Features: The cement is P.O42.5 silicate cement.
3. A method for producing tunnel shotcrete according to claim 1, Features: The fine aggregate is medium sand with a fineness modulus Mx of 2.8 to 3.0; the coarse aggregate is crushed stone with a particle size of 5 to 10 mm; the catalyst is a ZP-1 type catalyst; and the water reducer is a slow-setting water reducer.
4. A method for producing tunnel shotcrete according to claim 1, Features: The active additive includes fly ash; the fly ash is Class F Grade II fly ash; and the accelerating setting agent includes YTF-1 alkali-free accelerating setting agent.
5. A method for producing tunnel shotcrete according to claim 4, Features: The active additive further comprises modified nano zeolite powder; the active additive comprises the following raw materials in parts by weight: 105 to 110 parts of fly ash and 40 to 45 parts of modified nano zeolite powder.
6. A method for producing tunnel shotcrete according to claim 4, Features: The accelerator also includes a composite dispersant; the accelerator includes the following raw materials in parts by weight: 14 to 16 parts of YTF-1 alkali-free accelerator and 7 to 10 parts of composite dispersant.
7. A method for producing tunnel shotcrete according to claim 5, Features: The modified nano zeolite powder comprises the following raw materials in parts by weight: 5 to 8 parts of nano zeolite powder, 6 to 10 parts of gamma-aminopropyltriethoxysilane, 15 to 20 parts of acrylic anhydride, 8 to 10 parts of hydroxyl-polyethylene glycol-mercapto, and 1 to 2 parts of azobisisobutyronitrile.
8. A method for producing tunnel shotcrete according to claim 7, Features: The preparation method of the modified nano zeolite powder includes the following steps: (1) adding nano zeolite powder to deionized water for ultrasonic dispersion, then adding γ-aminopropyltriethoxysilane, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder A; (2) ultrasonically dispersing the modified nano zeolite powder A and acrylic anhydride in N-methylpyrrolidone, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder B; (3) ultrasonically dispersing the modified nano zeolite powder B, hydroxy-polyethylene glycol-mercapto group, and azobisisobutyronitrile in N-methylpyrrolidone, heating and stirring, filtering, washing, and drying to obtain modified nano zeolite powder.
9. A method for producing tunnel shotcrete according to claim 6, Features: The composite dispersant comprises the following substances in parts by mass: 10 to 15 parts of polyacrylic acid, 15 to 17 parts of ethanolamine, 3 to 5 parts of phosphoric acid, and 2 to 3 parts of p-toluenesulfonic acid.
10. A method for producing tunnel shotcrete according to any one of claims 1 to 9, Features: The following steps are involved: S1: Add coarse aggregate, part of fine aggregate and cement into a mixer in sequence and mix them evenly; then, during the mixing process, gradually add the remaining fine aggregate, active additives, water and water reducing agent in batches and mix them evenly to obtain a rough shotcrete mixture; S2: adding a catalyst and an accelerating agent to the above-mentioned rough shotcrete mixture, stirring for 2 to 3 minutes to obtain a shotcrete mixture; S3: Spray the shotcrete mixture on the tunnel rock surface and solidify to obtain tunnel shotcrete.