Preparation method of high-viscosity anti-seepage inorganic anchoring agent
By using high viscosity and anti-seepage inorganic anchoring agent preparation method of silicate cement, micro-expanding agent, water reducing agent, PBO fiber and other materials in anchoring agent, the poor stability of anchoring agent in high temperature and high humidity and freeze-thaw environment is solved. Problem, achieving higher strength and durability, suitable for mining engineering.
Patent Information
- Application Number
- CN202411230163.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
AI Technical Summary
Existing anchoring agents are difficult to maintain stability in high temperature and high humidity and freeze-thaw environments, especially in underground mining projects, where anchoring performance degradation problems occur.
The preparation method of high viscosity anti-seepage inorganic anchoring agent including silicate cement, micro-expanding agent, water reducing agent, PBO fiber, polymer auxiliary agent, slag powder, premature strength agent and hydrophobic agent is adopted, and the preparation method of high viscosity anti-seepage inorganic anchoring agent including silicate cement, micro-expanding agent, water reducing agent, PBO fiber, polymer auxiliary agent, slag powder, premature strength agent and hydrophobic agent is adopted, through dry mixing and uniformity of aqueous solution. Stir to form an anchoring agent with high strength and durability.
It significantly improves the durability of anchoring agent in high temperature and high humidity and freeze-thaw environments, is suitable for mining engineering, and enhances the pulling strength and stability.
Smart Images

Figure BDA0005025870520000091 
Figure BDA0005025870520000101 
Figure BDA0005025870520000102
Abstract
Description
Technical Field
[0001] The invention relates to the field of anchoring agents, and in particular to a method for preparing a high-viscosity anti-seepage inorganic anchoring agent. Background Art
[0002] Anchoring agent is a commonly used engineering material, generally used in construction and mining projects to anchor specific areas or components. Anchoring stability is an important indicator for evaluating anchoring agents, especially for underground mining projects, which have specific requirements. For example, higher pull-out strength, and maintaining stable anchoring performance under high temperature, high humidity and freeze-thaw environments in mines. To this end, the present application provides an anchoring agent material suitable for special working conditions. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-viscosity anti-seepage inorganic anchoring agent.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] The first aspect of the present invention relates to an anchoring agent, characterized in that it comprises the following raw materials in parts by weight:
[0006] Portland cement, 255-300 parts
[0007] Micro-expanding agent, 10-20 parts
[0008] Water reducing agent, 2-5 parts
[0009] PBO fiber, 3-5 parts
[0010] Polymer auxiliary agent, 1 to 3 parts.
[0011] Optionally, any one or more of the following raw materials in parts by weight are also included:
[0012] Slag powder, 30-50 parts;
[0013] Early strength agent, 5-10 parts;
[0014] Hydrophobic agent, 2 to 5 parts.
[0015] Optionally, the micro-expansion agent is calcium sulphoaluminate.
[0016] Optionally, the water reducing agent is a polycarboxylic acid-based water reducing agent.
[0017] Optionally, the polymer adjuvant is hydroxypropyl methylcellulose or methylcellulose.
[0018] Optionally, the hydrophobic agent is hexadecyltrichlorosilane or polytetrafluoroethylene.
[0019] Optionally, the early strength agent is calcium chloride and / or sodium sulphoaluminate.
[0020] The second aspect of the present invention relates to a method for preparing an anchoring agent, characterized in that it comprises the following steps:
[0021] 255-300 parts by weight of silicate cement, 10-20 parts by weight of micro-expansion agent, 30-50 parts by weight of slag powder, 5-10 parts by weight of early strength agent, 3-5 parts by weight of PBO fiber and 1-3 parts by weight of polymer auxiliary agent are weighed and put into a stirrer for dry mixing to obtain a dry mixed material.
[0022] 2 to 5 parts by weight of a water reducer is added to water and stirred until completely dissolved, and then the dry mixed material is added and stirred to obtain the anchoring agent.
[0023] Beneficial effects of the present invention:
[0024] Compared with the prior art, the anchor material of the present application adopts PBO fiber to obtain higher strength. On this basis, the durability in high temperature, high humidity and freeze-thaw environment is further improved by using specific hydrophobic agents and polymers, making it suitable for use in mining projects. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In the following examples, all parts are by weight unless otherwise specified.
[0027] Unless otherwise specified, the specific information of each raw material in the following examples and comparative examples is as follows:
[0028] Portland cement, Conch P·ll52.5R is used in the following examples and comparative examples;
[0029] The water reducing agent adopts Subot, PCA-HP polycarboxylic acid highly adaptable water reducing agent;
[0030] The polymer auxiliary agent is polythiophene.
[0031] Example 1
[0032] In some embodiments of the present invention, a method for preparing an inorganic anchoring agent is disclosed, comprising the following steps:
[0033] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of PBO fiber, 5 parts of hexadecyltrichlorosilane and 2 parts of polymer adjuvant.
[0034] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0035] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0036] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0037] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0038] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0039] Example 2
[0040] In some embodiments of the present invention, a method for preparing an inorganic anchoring agent is disclosed, comprising the following steps:
[0041] Weigh 280 parts of Portland cement, 15 parts of calcium sulfoaluminate, 40 parts of slag powder, 7 parts of calcium chloride, 4 parts of PBO fiber, 3 parts of hexadecyltrichlorosilane and 2 parts of polymer adjuvant.
[0042] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0043] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0044] Add 3 parts of polycarboxylic acid water reducer into water and stir until completely dissolved.
[0045] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0046] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0047] Example 3
[0048] In some embodiments of the present invention, a method for preparing an inorganic anchoring agent is disclosed, comprising the following steps:
[0049] Weigh 300 parts of Portland cement, 10 parts of calcium sulfoaluminate, 30 parts of slag powder, 5 parts of calcium chloride, 3 parts of PBO fiber, 2 parts of hexadecyltrichlorosilane and 2 parts of polymer adjuvant.
[0050] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0051] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0052] Add 2 parts of polycarboxylic acid water reducer into water and stir until completely dissolved.
[0053] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0054] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0055] Example 4
[0056] In some embodiments of the present invention, a method for preparing an inorganic anchoring agent is disclosed, comprising the following steps:
[0057] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of PBO fiber, 5 parts of polytetrafluoroethylene and 2 parts of polymer auxiliary agent.
[0058] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0059] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0060] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0061] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0062] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0063] Comparative Example 1
[0064] A method for preparing an inorganic anchoring agent comprises the following steps:
[0065] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of glass fiber, 5 parts of hexadecyltrichlorosilane and 2 parts of polymer adjuvant.
[0066] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0067] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0068] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0069] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0070] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0071] Comparative Example 2
[0072] A method for preparing an inorganic anchoring agent comprises the following steps:
[0073] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of PBO fiber and 2 parts of polymer auxiliary agent.
[0074] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0075] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0076] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0077] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0078] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0079] Comparative Example 3
[0080] A method for preparing an inorganic anchoring agent comprises the following steps:
[0081] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of PBO fiber and 5 parts of hexadecyltrichlorosilane.
[0082] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0083] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0084] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0085] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0086] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0087] Comparative Example 4
[0088] A method for preparing an inorganic anchoring agent comprises the following steps:
[0089] Weigh 255 parts of Portland cement, 20 parts of calcium sulfoaluminate, 50 parts of slag powder, 10 parts of calcium chloride, 5 parts of glass fiber, 5 parts of polytetrafluoroethylene and 2 parts of polymer auxiliary agent.
[0090] The silicate cement and slag powder are ultra-finely ground and screened to make the particle size reach 10-15 microns to ensure the various properties of the finished product. The surface area of the silicate cement is ≥400m 2 / kg.
[0091] The weighed silicate cement, calcium sulfoaluminate, slag powder, early strength agent, PBO fiber and polymer adjuvant were placed in a mixer for dry mixing for 5 minutes to ensure that all materials were evenly mixed to obtain a dry mixed material.
[0092] Add 5 parts of polycarboxylate water reducer into water and stir until completely dissolved.
[0093] Use a magnetic stirrer to stir and ensure that the water reducer is evenly dispersed in the water.
[0094] When the mixer is running at a low speed, the water solution containing the water reducing agent is gradually added to the dry mixed material. When all the water solution is added, the mixer speed is increased to a medium speed, and stirring is continued until the mixture is uniform and there is no agglomeration, thereby obtaining the anchoring agent.
[0095] Impermeability test
[0096] Preparation of anchoring agent specimens for experiments:
[0097] The anchoring agents (in slurry state) of the above-mentioned embodiments and comparative examples were placed on a vibration table and vibrated for 5 minutes to remove bubbles in the slurry.
[0098] Slowly pour the degassed slurry into the mold to avoid secondary introduction of bubbles.
[0099] After pouring, vibrate the mold on the vibration table again to ensure that the slurry fills the mold and the surface is flat.
[0100] After the anchoring agent in the mold has initially solidified, it is placed in a curing box for standard curing.
[0101] After curing for 24 hours, remove the mold from the curing box and demould.
[0102] The anchor agent samples after demoulding continued to be cured in the curing box for 7 days, and finally the test pieces were obtained.
[0103] Place the test piece into the permeameter and continue to use an electric hair dryer to accelerate the drying of the sealing material. Start the pressure test after about 1 hour, starting from 0.2MPa pressure, and increase the pressure by 0.1MPa every hour. Continue to pressurize the test until the pressure reaches 1.5MPa. Keep the pressure constant for 1 hour to observe whether the test piece has water seepage.
[0104] Pull-out test (normal indoor environment)
[0105] The concrete, steel bar and anchoring agent assembly for the pull-out test are prepared by the following method: a test hole is opened on the concrete (cylindrical, 200 mm in diameter, 400 mm in height), the steel bar is inserted into the hole, the anchoring agent implemented in the above comparative example and embodiment is added, and after complete solidification, the pull-out strength is tested by a pull-out tester. The material of the concrete slab used is C30 grade concrete, the hole diameter is 20 mm, and the hole depth is 170 mm. The steel bar used is HRB400 grade threaded steel bar with a diameter of 16 mm.
[0106] The sensors of the pulling equipment record the maximum tensile force value (i.e. the force value when the steel bar is pulled out of the concrete block) and the corresponding displacement value.
[0107] The calculation formula of pull-out strength (τ) is:
[0108]
[0109] τ is the pull-out strength, D is the steel bar diameter, H is the insertion depth, P max is the maximum pulling force value.
[0110] Freeze-thaw durability test
[0111] Take the anchoring agents of various embodiments and comparative examples, and make test pieces according to the pull-out test method.
[0112] Place the specimen in a freeze-thaw test chamber, set the temperature cycle (e.g., -18°C to 5°C), and perform 100 freeze-thaw cycles;
[0113] The pull-out strength was tested according to the above pull-out test method.
[0114] Wet heat durability test
[0115] Take the anchoring agents of various embodiments and comparative examples, and make test pieces according to the pull-out test method.
[0116] The test piece was placed in a wet heat test box, and the temperature was set at 60° C. and the humidity was set at 95%.
[0117] The pull-out strength was tested according to the above pull-out test method.
[0118] The relevant data of the above test are shown in Tables 1 and 2:
[0119] Table 1
[0120]
[0121] Table 2
[0122]
[0123] It can be seen from the results of Example 1 and Comparative Example 1 that, compared with conventional fiber materials, the use of PBO fibers can improve the comprehensive performance of the anchor material.
[0124] The reinforcing agent is hexadecyltrichlorosilane and polytetrafluoroethylene.
[0125] Hexadecyltrichlorosilane can bring a certain degree of hydrophobicity and also improve the durability and bonding strength of the anchor material, which may be due to the good bonding effect between hexadecyltrichlorosilane and the surface of PBO fibers.
[0126] It can be seen from Example 4 and Comparative Example 2 that polytetrafluoroethylene can also bring about a certain hydrophobic effect. It can be seen from Example 4 compared with Comparative Example 1, Comparative Example 2 and Comparative Example 4 that the absence of PBO fiber and polytetrafluoroethylene has a certain impact on the durability of the anchor material, and the durability of polytetrafluoroethylene alone in extreme environments is also limited. It can be seen that polytetrafluoroethylene has a good bonding force with some polar groups on the surface of PBO, which makes the anchor material have better chemical stability on a macro scale, and has more stable performance in a high humidity and high temperature environment, and the retention rate of the pull-out strength can reach (93%-94%).
[0127] By comparing Example 3 with Example 1, it can be seen that one of the functions of the polymer is to provide an antistatic effect, making the anchor material more suitable for special working conditions with extremely high safety requirements such as underground. In addition, it can be seen from the comparative example that polythiophene also affects the durability of the anchor in high temperature and high humidity and freeze-thaw environments. This may be because the conjugated double bond system of polythiophene forms a relatively stable network structure with the PBO fiber, thereby improving the stability of the anchor material, reducing its performance attenuation, and may also improve the crack resistance of the anchor material, etc.
[0128] The above embodiments and comparative examples have illustrated the technical solution of the present application and its application effects. However, in order to further clearly explain the selection of each component or operating method of the present application and its technical effects, the embodiments and their raw materials and preparation methods are further analyzed below.
[0129] The present application improves the mechanical and corrosion resistance of the anchoring agent by adding fiber materials. In order to better combine with other raw materials, the present application uses PBO fiber, which can relatively provide higher strength. However, it should be understood by those skilled in the art that the PBO fiber of the present application can be replaced by other known fiber materials, including but not limited to basalt fiber, glass fiber, polypropylene fiber material, etc., and relatively excellent technical effects can also be achieved.
[0130] The present application can improve durability such as sulfate resistance and alkali aggregate reaction resistance by introducing slag powder, especially when used in combination with PBO fiber material, it can increase the service life of the anchor under harsh working conditions. At the same time, it can also appropriately improve the toughness of the anchor, so that the anchor can withstand large deformation without cracking / breaking.
[0131] The role of hydroxypropyl methylcellulose in the present application at least includes reducing dust caused by split materials and cement raw materials and optimizing the production environment. In addition, in combination with a polycarboxylic acid-based water reducer, it can also synergistically enhance the fluidity of the overall material of the anchoring agent. In addition, those skilled in the art should also know that the hydroxypropyl methylcellulose of the present application can also be replaced by other cellulose materials, for example, methylcellulose.
[0132] In each embodiment of the present application, a polycarboxylic acid-based water reducer is used. Similarly, those skilled in the art can select other water reducers according to the requirements for the performance of the anchoring agent, including but not limited to phosphate-based water reducers, aliphatic water reducers, etc. The advantage of phosphate-based water reducers is that they improve the mechanical properties of the anchoring agent, while the advantage of aliphatic water reducers is that they improve the dispersion of other materials in the cement raw materials.
[0133] It should also be noted that some of the specific implementation schemes given in the above embodiments of the present application are only used as examples. Those skilled in the art can make routine adjustments according to the knowledge recorded in the prior art to obtain other embodiments if the expected results can be obtained. For example, although the subject matter of the present application is limited to inorganic, it is because the raw material that accounts for the main component is cement material, which is different from other anchoring agents with organic fillers as the main raw materials, but it does not mean that the raw materials of the present application cannot include any organic materials. Organic components that can be used in cement-based anchoring agent materials known in the art can also be used in the present application.
[0134] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0135] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. An anchoring agent, characterized in that: It includes the following raw materials in parts by weight: Portland cement, 255-300 parts; Micro-expanding agent, 10-20 parts; Water reducing agent, 2 to 5 parts; PBO fiber, 3-5 parts; Polymer auxiliary agent, 1 to 3 parts.
2. The anchoring agent according to claim 1, characterized in that It also includes any one or more of the following raw materials by weight: Slag powder, 30-50 parts; Early strength agent, 5-10 parts; Hydrophobic agent, 2 to 5 parts.
3. The anchoring agent according to claim 1, characterized in that: The micro-expanding agent is calcium sulphoaluminate.
4. The anchoring agent according to claim 1, characterized in that The water reducing agent is a polycarboxylic acid water reducing agent.
5. The anchoring agent according to claim 1, characterized in that The polymer auxiliary agent is polythiophene.
6. The anchoring agent according to claim 2, characterized in that: The hydrophobic agent is hexadecyltrichlorosilane or polytetrafluoroethylene.
7. The anchoring agent according to claim 2, characterized in that: The early strength agent is calcium chloride and / or sodium sulphoaluminate.
8. A method for preparing an anchoring agent, characterized in that: The following steps are involved: 255-300 parts by weight of silicate cement, 10-20 parts by weight of micro-expansion agent, 30-50 parts by weight of slag powder, 5-10 parts by weight of early strength agent, 3-5 parts by weight of PBO fiber and 1-3 parts by weight of polymer auxiliary agent are weighed and put into a stirrer for dry mixing to obtain a dry mixed material. 2 to 5 parts by weight of a water reducer is added to water and stirred until completely dissolved, and then the dry mixed material is added and stirred to obtain the anchoring agent.
9. The method for preparing an anchoring agent according to claim 8, characterized in that: Using silicate cement and slag powder, grinding is carried out.