Method for regulating and controlling shear stress and viscosity of sulphoaluminate cement-based material by using urea

By adding urea to sulfaaluminate cement to regulate its shear stress and viscosity, the problem of insufficient fluidity and plasticity of sulfuraaluminate cement-based materials is solved, and the fluidity of sulfuraaluminate cement-based materials is optimized and Plasticity improves its application range and compressive strength in porous phytogenetic concrete, helping to achieve the carbon reduction goal of the engineering industry.

CN118993660APending Publication Date: 2024-11-22NORTHWEST A & F UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411068048.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The application of sulfur aluminate cement-based materials in porous vegetative concrete is due to the lack of fluidity and plasticity caused by its early strength and fast setting characteristics. The existing technology is difficult to effectively regulate its rheological behavior, which affects its engineering. application.

Method used

By incorporating urea into sulfaaluminate cement, it regulates its shear stress and viscosity, optimizes fluidity and plasticity, and tests the mix ratio of sulfaaluminate cement-based materials through rheometer to reduce water consumption and prevent Isolate and improve the adaptability of planted concrete.

Benefits of technology

The fluidity and plasticity of sulfaluminate cement-based materials have been optimized, which reduces shear stress and viscosity, extends the initial settling time, improves the workingability and compressive strength of concrete, and enhances its in porous vegetated concrete. The scope of application helps the engineering industry achieve carbon reduction goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a method for regulating and controlling shear stress and viscosity of a sulphoaluminate cement-based material by using urea, which comprises the following steps: 1) weighing sulphoaluminate cement, urea and water in proportion for later use; 2) adding sulphoaluminate cement and urea into a stirrer, stirring for 20-40 seconds, then adding water, and stirring for 50-70 seconds; (3) putting the sulphoaluminate cement paste obtained in the step (2) into a rheometer for testing; and 4) collecting the shear stress and viscosity of the sample obtained in the step 3) through a rheometer. According to the method, the shear stress and the viscosity of the sulphoaluminate cement are regulated and controlled by utilizing the inhibition effect of urea on early hydration of the sulphoaluminate cement, the flowability, the cohesiveness and the water-retaining property of the sulphoaluminate cement are improved, the initial setting time is prolonged, and the uniform and dense sulphoaluminate cement-based material with excellent comprehensive performance is obtained. Furthermore, the low-alkali sulphoaluminate cement is used for the plant-growing concrete without fine aggregate, so that the problems of early setting and poor fluidity of the sulphoaluminate cement-based plant-growing concrete are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and relates to a method for controlling the rheological behavior of cement-based materials, and specifically to a method for regulating the shear stress and viscosity of sulphoaluminate cement-based materials by using urea. Background Art

[0002] In recent years, sulphoaluminate cement has been used as a cementitious material for green concrete due to its advantages such as low alkali and low carbon. However, its early strength and rapid setting characteristics lead to poor workability of the paste, which restricts its application in porous green concrete. Therefore, under the premise of meeting certain cohesiveness and water retention, the good fluidity and plasticity of sulphoaluminate cement-based materials are important issues that need to be solved in their application in porous green concrete.

[0003] The so-called fluidity is the ability of cement-based materials to overcome the deformation caused by the interaction between internal particles. Therefore, the interaction force between particles will affect its fluidity. From the perspective of rheology, the fluidity of the slurry can be characterized by the limiting shear stress. Increasing the water-cement ratio, expanding the distance between particles in the slurry, and weakening the interaction force between particles can increase fluidity. However, too much water will cause cement-based composite materials to segregate, bleed, and have poor cohesion and water retention. The plasticity of cement-based materials is the ability of the slurry to produce plastic deformation without breaking after overcoming the limiting shear stress. From the perspective of rheology, the smaller the plastic viscosity, the better the plasticity.

[0004] Therefore, it is necessary to adopt various technological means to adjust and control the rheological behavior of sulphoaluminate cement-based materials in order to determine reasonable rheological parameters, thereby accurately controlling the workability of sulphoaluminate cement concrete and guiding engineering applications.

[0005] Patent application CN117800680A discloses a vegetation concrete based on nitrogen-phosphorus modified biochar, a preparation method and an application. The method uses cement, aggregate, silica fume, water, a reinforcing agent and nitrogen-phosphorus modified biochar as raw materials. The nitrogen-phosphorus modified biochar is obtained by pyrolysis of straw immersed in a urea solution, and then modified with potassium dihydrogen phosphate, ground and screened to improve the vegetation performance of the vegetation concrete. However, the study used silicate cement, which has a high alkalinity, and silicate cement has a higher carbon emission than sulphoaluminate cement. The vegetation effect is difficult to guarantee, the environmental friendliness is poor, and the urea in silicate cement does not play a role in regulating rheological behavior.

[0006] Huang Qingliang studied the effect of adding urea and diammonium hydrogen phosphate on the fluidity of sulphoaluminate cement paste in the paper "Preparation and Performance Research of Fertilizer-Efficient Slow-Release Porous Ecological Concrete" ([D]. Jinan: Jinan University). He used the fluidity index and found that the fluidity of the paste increased significantly with the increase of urea content. Gong et al. determined the effect of urea on the fluidity of sulphoaluminate cement in the paper "Effects of carbamide on fluidity and setting time of sulphoaluminate cement and properties of planting concrete from sulphoaluminate cement". The fluidity was determined by measuring the diameter of the cement paste using a cone (60 mm high, 36 mm top diameter, and 60 mm bottom diameter). The water-cement ratio (w / c) of the prepared sample was 0.45. The maximum diameter of the extended specimen and its corresponding vertical diameter were measured, and the average of these two values ​​was defined as the fluidity. However, the above studies all used simple fluidity measurement, namely the conventional slump spread method test. This method is difficult to systematically evaluate the rheological behavior of the paste, cannot fully reflect the effect of urea on the shear stress and viscosity of sulfoaluminate cement, and cannot provide a reference for the fine design of concrete. Summary of the invention

[0007] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a method for regulating the shear stress and viscosity of sulphoaluminate cement-based materials using urea, which method can not only optimize the fluidity of sulphoaluminate cement paste, but also reduce water consumption, prevent concrete segregation, and optimize the mix ratio of sulphoaluminate-based concrete. At the same time, due to its low alkalinity and slow-release fertilizer properties, the application scope of sulphoaluminate cement can be improved, helping the engineering industry to achieve carbon reduction goals and realize the ecological sustainable development of the construction industry.

[0008] In order to achieve the above-mentioned object of the present invention, the technical scheme adopted is as follows: A method for regulating the shear stress and viscosity of sulphoaluminate cement-based materials using urea comprises the following steps: 1) Weigh 65-75 parts of sulphoaluminate cement, 1-3 parts of urea, and 25-29 parts of water and set aside; 2) Add sulphoaluminate cement and urea into a mixer and mix for 30 seconds, then add water and mix for 60 seconds; 3) putting the sulphoaluminate cement paste obtained in step 2) into a rheometer for testing; 4) The shear stress and viscosity of the sample obtained in step 3) are collected by rheometer.

[0009] Furthermore, according to the above scheme, the sulphoaluminate cement described in step 1) is low-alkali sulphoaluminate cement (LAC, 42.5 R grade).

[0010] Furthermore, according to the above scheme, the standard consistency water consumption of the sulphoaluminate cement in step 1) is 24.4%.

[0011] Furthermore, according to the above scheme, the initial setting time of the sulphoaluminate cement experimentally measured in step 1) is 11 minutes, and the final setting time is 43 minutes.

[0012] Furthermore, according to the above scheme, the main components of the sulphoaluminate cement in step 1) are anhydrous calcium sulphoaluminate, gypsum, calcium carbonate and a small amount of monosulfide hydrated calcium sulphoaluminate.

[0013] Furthermore, according to the above scheme, the urea described in step 1) is produced by Shaanxi Weihe Heavy Chemical Industry Co., Ltd., and the production standard is GB / T2440-2017.

[0014] Furthermore, according to the above scheme, the urea particle size d1.18-3.35 mm in step 1) has a total nitrogen content of 46.3%.

[0015] Furthermore, according to the above scheme, the water-cement ratio in step 1) is 0.34.

[0016] Further, according to the above solution, the rheometer model described in step 2) is Anton Paar MCR102, with a maximum torque of 200 mNm and a maximum angular velocity of 314 rad / s.

[0017] Further, according to the above scheme, in step 3), the shear rate increases in a logarithmic mode, and the shear stress and viscosity of the fresh cement paste are collected.

[0018] The second object of the present invention is to provide application of the above method in sulphoaluminate-based recycled brick aggregate green concrete.

[0019] The urea-doped sulphoaluminate-based recycled brick aggregate bio-concrete of the present invention is composed of sulphoaluminate cement, urea, basalt fiber, recycled brick aggregate, natural crushed stone aggregate and water. The mass ratio of the sulphoaluminate cement, urea, basalt fiber, recycled brick aggregate, natural crushed stone aggregate and water is 3:0-0.024:0.0015:9:50:1.

[0020] Furthermore, in the above solution, the basalt fiber has a diameter of 16 μm, a length of 12 mm, and a breaking strength of 1910 MPa.

[0021] Furthermore, in the above scheme, the recycled brick aggregate is construction waste that is screened into a particle size of 15 to 20 mm.

[0022] Furthermore, in the above scheme, the single particle size aggregate is crushed stone with a particle size of 15 to 20 mm.

[0023] The third object of the present invention is to provide a method for preparing the above-mentioned urea-doped sulphoaluminate-based recycled brick aggregate bio-concrete.

[0024] Furthermore, the above technical solution, the above urea sulphoaluminate-based recycled brick aggregate planted concrete, comprises the following steps: 1) Weigh sulphoaluminate cement, urea, basalt fiber, water, single-grain recycled brick aggregate, and natural crushed stone aggregate according to the formula ratio and set aside; 2) Add single-size recycled brick aggregate, natural crushed stone aggregate, sulphoaluminate cement and 20% to 30% basalt fiber into a mixer and stir for 30 seconds, then add 30% basalt fiber and continue stirring for 30 seconds; then add the remaining basalt fiber and continue stirring for 30 seconds, and finally add water and stir for 60 seconds; 3) Fill the mold with the vegetation concrete obtained in step 2) to 1 / 2 of the volume, and vibrate it clockwise 14 times using a special vibrating tool. Then fill the mold with the vegetation concrete, and continue to vibrate it clockwise 15 times using a special vibrating tool;

[0025] 4) After molding, cover the mold surface with plastic film to keep it moist for 24 hours and then remove the mold; 5) After demoulding, maintain heat preservation and moisture retention for no less than 3 days, and the green concrete will be obtained after 28 days.

[0026] Furthermore, in the above scheme, the step 1) needs to soak the recycled brick aggregate for 24 hours to ensure that the recycled brick aggregate is saturated with water. After soaking, the recycled brick aggregate should be drained and the surface moisture of the aggregate should be wiped dry with a towel to ensure that it is in a saturated surface dry state.

[0027] Furthermore, in the above scheme, the contact surface size of the special vibrating tool used in step 3) is 50*50mm.

[0028] The reaction mechanism of the present invention and the role played by each raw material are as follows: The main components of low-alkali sulphoaluminate cement are anhydrous calcium sulphoaluminate, gypsum, calcium carbonate and a small amount of monosulfide hydrated calcium sulphoaluminate.

[0029] The molecular formula of urea is CO(NH2)2. After urea is added to low-alkali sulphoaluminate cement, urea affects the formation of hydration products such as calcium sulfaluminite, monosulfur calcium sulphoaluminate and aluminum hydroxide to a certain extent, and has an inhibitory effect on cement hydration. At the same time, during the hydration process of sulphoaluminate cement, as the amount of urea increases, the particle size of flocculated particles in the cement-based material changes, and the mutual attraction between particles weakens. In addition, the carbonate ions produced after urea is dissolved in water will react with the hydroxide ions in the sulphoaluminate cement, thereby slowing down the formation of hydration products of sulphoaluminate cement. This affects the shear stress and viscosity of the sulphoaluminate cement-based material.

[0030] Furthermore, adding urea to sulphoaluminate cement will optimize the workability of sulphoaluminate concrete on the basis of improving the fluidity of cement-based materials, and will prolong the initial setting time of sulphoaluminate cement, making it easier to mix and pour sulphoaluminate concrete. At the same time, adding urea to sulphoaluminate-based bio-concrete can slowly release the N element in urea during the long-term service of bio-concrete, which is beneficial to improving the adaptability of bio-concrete.

[0031] Compared with the prior art, the method of the present invention for regulating the shear stress and viscosity of sulphoaluminate cement-based materials by using urea has the following beneficial effects: 1. The present invention is based on the mixing and pouring processes of sulphoaluminate cement-based concrete, and uses urea to regulate the hydration process of sulphoaluminate cement and the effect of hydration products, thereby reducing the shear stress and viscosity of sulphoaluminate cement paste; 2. The addition of urea can not only regulate the rheological properties of sulphoaluminate cement-based vegetation concrete, but also provide necessary nutrients for plant growth, promote the engineering application of vegetation concrete, and improve the adaptability of vegetation concrete in long-term service environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 is the X-ray diffraction pattern of sulphoaluminate cement; Figure 2 The X-ray diffraction patterns of sulphoaluminate cement hydration products in different embodiments and comparative examples; Figure 3 is the shear stress of sulphoaluminate cement slurry of the embodiment and the comparative example; Figure 4is the viscosity of the sulphoaluminate cement slurry of the embodiment and the comparative example; Figure 5 The slump of sulphoaluminate cement-based vegetation concrete of different application examples and comparative examples; Figure 6 It is the compressive strength of sulphoaluminate cement-based vegetation concrete in different application examples and comparative examples. Specific implementation methods In order to better understand the present invention, the present invention is further described below in conjunction with examples. This implementation case is implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given to illustrate that the present invention is creative, but the protection scope of the present invention is not limited to the following implementation cases.

[0035] The sulphoaluminate cement used in the following embodiments of the present invention comes from Dengdian Group Cement Co., Ltd., and its X-ray diffraction pattern is shown in Figure 1 , Figure 1 It is the XRD spectrum of sulphoaluminate cement, Y: anhydrous calcium sulphoaluminate, O: calcium carbonate, ▽: gypsum, ◇: silicate disulfide, △: monosulfur calcium sulphoaluminate. Recycled brick aggregate is obtained by crushing brickwork, screening and washing.

[0036] The materials used in the embodiments and comparative examples are as follows: Example 1 The urea-doped sulphoaluminate cement slurry of this embodiment is prepared by the following method, and the steps are as follows: 1) Weigh 70 parts of hydrous sulphoaluminate cement, 27 parts of water and 1 part of urea according to the formula ratio and set aside; 2) adding sulphoaluminate cement, urea and water into a mixer and stirring for 60 seconds to form urea-sulphoaluminate cement slurry; 3) Loading the product obtained in step 2) into a rheometer for testing; 4) Measure the shear stress and viscosity of cement slurry using a rheometer.

[0037] Example 2 The urea-doped sulphoaluminate cement slurry of this embodiment is prepared by the following method, and the steps are as follows: 1) Weigh 72 parts of hydrous sulphoaluminate cement, 25 parts of water and 3 parts of urea according to the formula ratio and set aside; 2) The subsequent steps are the same as in Example 1.

[0038] Comparative Example 1 The urea-free sulphoaluminate cement slurry of this embodiment is prepared by the following method, and the steps are as follows: 1) Weigh 70 parts of hydrous sulphoaluminate cement, 26 parts of water and 0 parts of urea according to the formula ratio and set aside; 2) The subsequent steps are the same as in Example 1.

[0039] Application Example 1 The urea-doped sulphoaluminate cement-based vegetation concrete of this embodiment is prepared by the following method, and the steps are as follows: 1) According to the formula ratio, weigh 310 parts of sulphoaluminate cement, 12 parts of urea, 2 parts of basalt fiber, 105 parts of water, 455 parts of single-grain recycled brick aggregate, and 900 parts of natural crushed stone aggregate for use; 2) Add single-size recycled brick aggregate, natural crushed stone aggregate, sulphoaluminate cement and 20% to 30% basalt fiber into a mixer and stir for 30 seconds, then add 30% basalt fiber and continue stirring for 30 seconds; then add the remaining basalt fiber and continue stirring for 30 seconds, and finally add water and stir for 60 seconds; 3) Fill the mold with the vegetation concrete obtained in step 2) to 1 / 2 of the volume, and vibrate it clockwise 14 times using a special vibrating tool. Then fill the mold with the vegetation concrete, and continue to vibrate it clockwise 15 times using a special vibrating tool;

[0040] 4) After molding, cover the mold surface with plastic film to keep it moist for 24 hours and then remove the mold; 5) After demoulding, maintain heat preservation and moisture retention for no less than 3 days, and the green concrete will be obtained after 28 days.

[0041] Application Example 2 The urea-doped sulphoaluminate cement-based vegetation concrete of this embodiment is prepared by the following method, and the steps are as follows: 1) According to the formula ratio, weigh 310 parts of sulphoaluminate cement, 25 parts of urea, 2 parts of basalt fiber, 105 parts of water, 455 parts of single-grain recycled brick aggregate, and 900 parts of natural crushed stone aggregate, and set aside; 2) The subsequent steps are the same as those in Application Example 1.

[0042] Comparative Example 2 The urea-doped sulphoaluminate cement-based vegetation concrete of this embodiment is prepared by the following method, and the steps are as follows: 1) According to the formula ratio, weigh 310 parts of sulphoaluminate cement, 0 parts of urea, 2 parts of basalt fiber, 105 parts of water, 455 parts of single-grain recycled brick aggregate, and 900 parts of natural crushed stone aggregate for use; 2) The subsequent steps are the same as those in Application Example 1.

[0043] Test Example 1 The test objects are the shear stress and viscosity of the cement pastes prepared in Example 1, Example 2 and Comparative Example 1. The slump of the fresh concrete and the compressive strength after curing for 28 days using Example 1, Example 2 and Comparative Example 1 are tested.

[0044] 1) X-ray diffraction analysis. Figure 2 The X-ray diffraction patterns of the hydration products of sulphoaluminate cement in different embodiments and comparative examples are shown in FIG. 1 , wherein Y: anhydrous calcium sulphoaluminate, O: calcium carbonate, ▽: gypsum, ◇: dicalcium silicate, □: ettringite, △: monosulfurized calcium sulphoaluminate, K: aluminum hydroxide, and N: urea.

[0045] Depend on Figure 2 It can be seen that compared with Comparative Example 1, the types of hydration products of sulfoaluminate cement in Example 1 and Example 2 are basically the same, including calcium sulfaluminite, monosulfur calcium sulfoaluminate and aluminum hydroxide, and the calcium sulfaluminite content is the main factor affecting the hardening strength of sulfoaluminate cement. With the increase of urea dosage, the diffraction peaks of anhydrous calcium sulfoaluminate are basically the same, and the diffraction peaks of calcium sulfaluminite, monosulfur calcium sulfoaluminate and aluminum hydroxide are weakened, indicating that the addition of urea will reduce the hydration degree of anhydrous sulfoaluminate in sulfoaluminate cement. However, the diffraction peaks of dicalcium silicate are basically the same, indicating that urea does not significantly affect the hydration degree of dicalcium silicate. The research conclusions in the literature are similar. The addition of urea will prevent the formation of calcium sulfaluminite in low-alkali sulfoaluminate cement. The higher the dosage, the fewer hydration products. Studies have also found that the addition of urea will reduce the content of calcium sulfaluminite in the hydration products of sulfoaluminate cement, delay the hydration of sulfoaluminate cement, but accelerate the hydration of ordinary Portland cement;

[0046] 2) Shear stress. Figure 3 is the shear stress of sulphoaluminate cement slurry in Examples and Comparative Examples.

[0047] like Figure 3 As shown, as the shear rate increases, the shear stress shows a downward trend. It can be seen from the curves of Example 1 and Example 2 that when the shear rate increases from 0s-1 to 1s-1, the shear stress at 2% and 4% urea dosages decreases by about 63.8% and 57.25%, respectively. This indicates that urea will cause changes in the particle size of flocculated particles in the slurry, increase the distance between particles, reduce the internal friction between particles, thereby reducing the shear stress and increasing the fluidity of the sulphoaluminate cement paste;

[0048] 3) Viscosity. Figure 4 is the viscosity of sulphoaluminate cement slurry in Examples and Comparative Examples.

[0049] from Figure 4 The curves of Example 1 and Example 2 show that when the shear rate is 0 s -1 When the shear rate is around 0 s, the viscosity of Example 1 and Example 2 is significantly lower than that of Comparative Example 1, and the viscosity of Example 2 is lower than that of Example 1. As the shear rate increases, the viscosity of the sulphoaluminate cement paste decreases. -1 Increase to 1 s -1The viscosity of Example 1 and Example 2 both decreased by about 100%, and because the urea content of Example 2 was larger, the viscosity decreased at a slower rate. This indicates that urea can reduce the viscosity of sulphoaluminate cement paste, causing the bonding force between particles in the paste of fresh VC to weaken, and can more evenly wrap the coarse aggregate, which may be beneficial to the strength growth of the bioremediation concrete;

[0050] 4) Liquidity. Figure 5 It is the slump of sulphoaluminate cement-based vegetation concrete in different application examples and comparative examples.

[0051] According to Figure 5 The slump bar graphs of application examples 2 and 3 show that the slump of application example 1 increases by 223.2% due to the addition of urea compared with application comparison example 1, and the slump of application example 2 increases by 362.5% due to the addition of urea compared with application comparison example 1. Therefore, it is shown that the addition of urea to sulphoaluminate-based vegetation concrete can improve the workability of vegetation concrete and improve the problem of poor workability of vegetation concrete due to the absence of fine aggregate;

[0052] 5) Compressive strength. Figure 6 It is the compressive strength of sulphoaluminate cement-based vegetation concrete in different application examples and comparative examples.

[0053] From this column Figure 6 It can be seen that the compressive strength of Application Example 1 and Application Example 2 has been significantly improved compared to Application Comparative Example 1, increasing by 34.7% and 36.4% respectively. This may be because the addition of urea reduces the shear stress and viscosity of the sulphoaluminate cement paste, so that the sulphoaluminate cement can be better hydrated and the net paste strength is improved. At the same time, urea can bring better homogeneity to the cement paste, and can wrap the coarse aggregate well to ensure better contact between the contact surfaces of the coarse aggregate, which is beneficial to the improvement of the strength of the vegetation concrete. The results show that the sulfate cement-based vegetation concrete after the regulation of the present invention can better improve the compressive strength of the vegetation concrete after the concrete is formed.

Claims

1. A method for regulating the shear stress and viscosity of sulphoaluminate cement-based materials using urea, characterized in that: The following steps are involved: 1) Weigh 65-75 parts of sulphoaluminate cement, 1-3 parts of urea, and 25-29 parts of water and set aside; 2) Add sulphoaluminate cement and urea into a mixer and stir for 20 to 40 seconds, then add water and stir for 50 to 70 seconds; 3) putting the sulphoaluminate cement paste obtained in step 2) into a rheometer for testing; 4) The shear stress and viscosity of the sample obtained in step 3) are collected by rheometer.

2. The method for regulating shear stress and viscosity of sulphoaluminate cement-based materials using urea according to claim 1, characterized in that: The sulphoaluminate cement is low-alkali sulphoaluminate cement.

3. The method for regulating shear stress and viscosity of sulphoaluminate cement-based materials using urea according to claim 1, characterized in that: The standard consistency water consumption of the sulphoaluminate cement is 24.4%.

4. The method for regulating shear stress and viscosity of sulphoaluminate cement-based materials using urea according to claim 1, characterized in that: The initial setting time of the sulphoaluminate cement measured in the experiment is 11 minutes, and the final setting time is 43 minutes.

5. The method for regulating shear stress and viscosity of sulphoaluminate cement-based materials using urea according to claim 1, characterized in that: The main components of the sulphoaluminate cement are anhydrous calcium sulphoaluminate, gypsum, calcium carbonate and a small amount of monosulfide type hydrated calcium sulphoaluminate.

6. The method for regulating shear stress and viscosity of sulphoaluminate cement-based materials using urea according to claim 1, characterized in that: The urea particle size d1.18-3.35 mm, the total nitrogen content is 46.3%.

7. Application of the method for regulating shear stress and viscosity of sulphoaluminate cement-based materials by using urea as described in claim 1 in sulphoaluminate-based recycled brick aggregate bio-concrete.

8. A urea-doped sulphoaluminate-based recycled brick aggregate bio-concrete, characterized in that: The invention is composed of sulphoaluminate cement, urea, basalt fiber, recycled brick aggregate, natural crushed stone aggregate and water, wherein the mass ratio of the sulphoaluminate cement, urea, basalt fiber, recycled brick aggregate, natural crushed stone aggregate and water is 3:0-0.024:0.0015:9:50:

1.

9. The method for preparing the urea-doped sulphoaluminate-based recycled brick aggregate bio-concrete according to claim 8, characterized in that: The steps include: 1) Weigh sulphoaluminate cement, urea, basalt fiber, water, single-grain recycled brick aggregate, and natural crushed stone aggregate according to the formula ratio and set aside; 2) Add single-size recycled brick aggregate, natural crushed stone aggregate, sulphoaluminate cement and 20% to 30% basalt fiber into a mixer and stir for 30 seconds, then add 30% basalt fiber and continue stirring for 30 seconds; then add the remaining basalt fiber and continue stirring for 30 seconds, and finally add water and stir for 60 seconds; 3) Fill the mold with the green concrete obtained in step 2) to 1 / 2 of the volume, vibrate it clockwise 14 times using a special vibrating tool, then fill the mold with the green concrete, and continue to vibrate it clockwise 15 times using the special vibrating tool; 4) After molding, cover the mold surface with plastic film to keep it moist for 24 hours and then remove the mold; 5) After demoulding, maintain heat preservation and moisture retention for no less than 3 days, and the green concrete will be obtained after 28 days.