Low-alkali regenerated vegetation concrete as well as preparation method and alkali reduction method thereof

Through the use of low-alkaline cement compounding and ultrafine fly ash, combined with water glass and silane treatment, the balance between planted concrete between performance and ecology is solved, and the efficient use of recycled aggregates and ecological restoration is achieved, which has improved the The ecological and environmental protection properties of concrete.

CN118993666APending Publication Date: 2024-11-22NO 1 ENG CO LTD OF FHEC OF CCCC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411128258.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing plant-grown concrete is difficult to balance between plant growth and concrete performance, and traditional treatment methods lead to waste of resources and environmental pollution, and the inability to effectively utilize recycled aggregates, limiting its widespread application.

Method used

Low-alkalisulfanoaluminate cement and ordinary silicate cement are combined, combined with ultrafine fly ash and reinforced regenerated aggregate, and the low-alkali regenerated phytogenetic concrete is prepared by immersion of water glass solution and vacuum impregnation, and the low-alkali regenerated phytogenetic concrete is optimized. Physical performance and ecological properties.

Benefits of technology

The efficient use of recycled aggregates is achieved, the dependence on natural aggregates is reduced, the workingability and durability of concrete is improved, the growth of plant roots is promoted, and the ecological restoration is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997095360000061
    Figure BDA0004997095360000061
  • Figure BDA0004997095360000062
    Figure BDA0004997095360000062
  • Figure BDA0004997095360000071
    Figure BDA0004997095360000071
Patent Text Reader

Abstract

The invention discloses low-alkali regenerated vegetation concrete as well as a preparation method and an alkali reduction method thereof. The vegetation concrete is prepared from the following raw materials in parts by weight: 1421 to 1460 parts of recycled aggregate, 184 to 224 parts of cement, 40 to 56 parts of fly ash, 13 to 28 parts of silica fume, 1 to 3 parts of a water reducing agent, 1 to 1.4 parts of a retarder and 78 to 84 parts of water, the recycled aggregate is reinforced recycled aggregate obtained by soaking and modifying in a water glass solution; the fly ash is superfine fly ash. According to the invention, building solid waste or industrial solid waste is taken as a main raw material, natural aggregate is completely replaced, and meanwhile, part of cement is replaced, so that secondary utilization of solid waste resources is realized; the superfine fly ash is introduced as an admixture, the superfine fly ash is more excellent in performance than common fly ash, particles of the superfine fly ash are extremely fine, a ball effect can be generated when the superfine fly ash is applied to the concrete, the coating uniformity of the slurry on the aggregate is improved, and the micro-aggregate characteristic and the volcanic ash activity are beneficial to the development of the strength of the concrete and the reduction of the alkalinity. And double optimization of efficient ecological restoration and building performance is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ecological concrete, and in particular to a low-alkali regeneration vegetation concrete and a preparation method and an alkali reduction method thereof. Background Art

[0002] With the acceleration of urbanization, traditional concrete building materials, while meeting construction needs, have also brought about a series of environmental problems, such as the heat island effect, urban waterlogging, and rainwater runoff pollution. Vegetative concrete is a new type of building material introduced to build a "sponge city" that takes into account both plant compatibility and engineering functionality. It is a concrete material with a certain strength and suitable for plant growth, with porous concrete as the skeleton and pores filled with plant substrates. However, the cementitious materials used in the preparation of existing vegetative concrete are mostly silicate cement, which produces a large amount of hydration products Ca(OH) after hydration. 2 The alkalinity in the pores of the prepared vegetative concrete is high and cannot meet the requirements for plant root growth. Existing products often find it difficult to strike a balance between plant growth and concrete performance, limiting their widespread application.

[0003] At the same time, the output of construction waste has increased year by year. Traditional treatment methods not only lead to resource waste, but also aggravate environmental pollution. If recycled aggregates are used in bio-concrete, it can not only reduce construction waste pollution, but also reduce the mining of natural sand and gravel aggregates, and realize the complementary advantages of bio-concrete and recycled aggregates. Therefore, the development of a concrete material that can efficiently utilize recycled aggregates and has excellent ecological performance is of great significance to achieve sustainable development of the building materials industry. Summary of the invention

[0004] Based on this, it is necessary to provide a low-alkali regenerated vegetation concrete and its preparation method and alkali reduction method to address the above-mentioned technical problems.

[0005] The present invention is achieved through the following technical solutions:

[0006] In a first aspect, a low-alkali recycled vegetation concrete, the raw materials of the vegetation concrete include the following components in parts by weight: 1421-1460 parts of recycled aggregate, 184-224 parts of cement, 40-56 parts of fly ash, 13-28 parts of silica fume, 1-3 parts of water reducer, 1-1.4 parts of retarder, and 78-84 parts of water;

[0007] The recycled aggregate is a reinforced recycled aggregate obtained by being modified by soaking in a water glass solution; and the fly ash is ultrafine fly ash.

[0008] Furthermore, the particle size of the ultrafine fly ash is less than 10 μm.

[0009] Furthermore, the cement is compounded by low alkalinity sulphoaluminate cement and ordinary Portland cement in a weight ratio of 3 to 4:1. Furthermore, the low alkalinity sulphoaluminate cement is L·SAC42.5 grade low alkalinity sulphoaluminate cement; the ordinary Portland cement is P·O 42.5 grade ordinary Portland cement. Sulphoaluminate cement has low alkalinity, high early strength, and strong corrosion resistance, but its later strength is unstable and its price is relatively high. Portland cement has the advantages of high later strength and stable performance. Compounding the two cements can achieve the effect of complementary advantages and improve the performance of a single cement.

[0010] Furthermore, the particle size of the recycled aggregate is 10-20 mm.

[0011] In a second aspect, a method for preparing low-alkali regenerated vegetation concrete comprises the following steps:

[0012] (1) crushing the discarded concrete test blocks in the laboratory with a jaw crusher to obtain recycled coarse aggregate with a particle size of 10-20 mm, cleaning and removing impurities for standby use;

[0013] (2) Pour the recycled coarse aggregate into the water glass solution and soak it, take it out and drain it, then spread it out and place it in a ventilated and cool place, turn it over regularly to prevent it from sticking, and let it dry naturally to obtain reinforced recycled aggregate; water glass can penetrate into the internal structure of the recycled aggregate, and when it hardens, silica gel can precipitate to bond and fill micro cracks and holes. At the same time, water glass can react with the hydration products of the old mortar layer to generate hydrated calcium silicate and calcium aluminate, which can further repair pores and cracks and improve the strength and durability of the aggregate.

[0014] (3) Prepare raw materials according to the following weight parts: 1421-1460 parts of recycled aggregate, 184-224 parts of cement, 40-56 parts of fly ash, 13-28 parts of silica fume, 1-3 parts of water reducer, 1-1.4 parts of retarder, and 78-84 parts of water;

[0015] Put cement, fly ash and silica fume into a mixer, stir and mix them evenly, add part of water and part of admixture, continue stirring to make the cementitious material and water evenly mixed, add the reinforced recycled aggregate into the mixer, add the remaining water and admixture, continue stirring to obtain a concrete mixture;

[0016] (4) Pour the prepared concrete mixture into a mold and use a vibration molding process to produce low-alkali regenerated biomass concrete.

[0017] Furthermore, the aggregate surface of the concrete mixture is glossy.

[0018] Furthermore, step (4) is specifically as follows: the prepared concrete mixture is loaded into the mold in multiple layers, each layer is vibrated 25 times, and after being filled, the side of the test mold is gently tapped with a rubber hammer, and the molding surface is smoothed with a spatula, and the mold is removed after sealing and curing on the molding surface.

[0019] In a third aspect, a method for reducing alkali in low-alkali regenerated vegetation concrete is provided, wherein the cured vegetation concrete is immersed in a silane impregnating agent for vacuum impregnation treatment.

[0020] Furthermore, the alkali reduction method includes the following steps: placing the cured vegetation concrete in an oven until the surface of the specimen is dry; placing the dry vegetation concrete specimen in a vacuum device, adding a silane impregnating agent to cover all the specimens, keeping the vacuum degree in the container below -0.1MPa, and maintaining it for more than 40 minutes; taking out the sample, wiping the surface liquid and letting it dry naturally.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention uses construction solid waste or industrial solid waste as the main raw material, completely replaces natural aggregates and replaces part of cement, realizing the secondary utilization of solid waste resources. By strengthening the treatment of recycled aggregates, the performance of recycled aggregates is optimized, the utilization rate of recycled aggregates in concrete is greatly improved, and the dependence on natural aggregate resources is effectively reduced. The resource utilization of construction waste is realized, and it has good ecological benefits; at the same time, the present invention creatively introduces ultrafine fly ash as an admixture. Ultrafine fly ash has better performance than ordinary fly ash, and its particles are extremely fine. When applied to concrete, it will produce a ball effect, which is conducive to improving the uniformity of the slurry wrapping the aggregates, and the micro-aggregate characteristics and volcanic ash activity contribute to the development of concrete strength. It not only improves the workability and durability of the vegetation concrete, but also further enhances its ecological and environmental protection attributes. It realizes the dual optimization of efficient ecological restoration and building performance.

[0023] The present invention compounds low-alkali sulphoaluminate cement and silicate cement to achieve complementary advantages and improve the performance of single cement. The prepared vegetation concrete not only has good physical properties, but also can effectively promote the growth of plant roots inside the concrete, thereby achieving ecological restoration.

[0024] The present invention also proposes a new and effective alkali reduction method, which adopts a vacuum impregnation method to promote the impregnating agent to penetrate deeper into the concrete and improve the silane impregnation efficiency. After the prepared vegetation concrete is treated with silane vacuum impregnation to reduce alkali, the pH is <9, the 28d strength is >10MPa, and the porosity is 27.8-28.3%. It not only has good physical properties, but also can effectively promote the growth of plant roots inside the concrete to achieve ecological restoration.

[0025] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. DETAILED DESCRIPTION

[0026] Hereinafter, examples will be given to illustrate the embodiments of the present disclosure, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values ​​and materials are sometimes exemplified, but other numerical values ​​and materials may also be used as long as the effects of the present disclosure can be obtained. In this specification, a description such as "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be replaced by "numerical value A or more and numerical value B or less". In the following description, when a lower limit and an upper limit are exemplified with respect to numerical values ​​such as specific physical properties and conditions, any one of the exemplified lower limits and any one of the exemplified upper limits can be arbitrarily combined as long as the lower limit does not become above the upper limit. When multiple materials are exemplified, one of them can be selected and used alone, or two or more can be used in combination.

[0027] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features and technical solutions in the embodiments may be combined with each other.

[0029] Embodiment 1:

[0030] This embodiment shows a method for preparing low-alkali regeneration vegetation concrete, which includes the following steps:

[0031] (1) The discarded laboratory fly ash concrete test blocks with a strength grade of C30 and a large amount of fly ash were crushed by a jaw crusher and manually sieved to obtain recycled coarse aggregate with a particle size of 10-20 mm. The recycled aggregate was washed with clean water to remove impurities such as dust and soil on the surface, and then dried naturally for later use;

[0032] (2) Pour the recycled coarse aggregate into a water glass solution with a concentration of 8% and soak it for 12 hours. Take it out and drain it. Then spread it out and place it in a ventilated and cool place. Turn it over from time to time within 1 hour to prevent sticking. Let it dry naturally to obtain reinforced recycled aggregate with a particle size of 10-20 mm and an apparent density of 2490 kg / m 3 , compact packing density is 1450kg / m 3 , the crushing value is 16.4%;

[0033] (3) 3.36 parts of low-alkali sulphoaluminate cement, 1.12 parts of ordinary Portland cement, 1.12 parts of fly ash and 0.56 parts of silica fume were added into a mixer and stirred for 30 seconds to mix the cementitious materials evenly. Then, 0.84 parts of water, 0.03 parts of water reducer and 0.014 parts of retarder were added and stirred for 60 seconds to mix the cementitious materials and water evenly. Finally, 29.2 parts of reinforced recycled aggregate were added into the mixer, and then 0.84 parts of water, 0.03 parts of water reducer and 0.014 parts of retarder were added and stirred for 120 seconds to mix the components evenly until the cementitious material slurry evenly covered the aggregate surface and the aggregate surface was glossy.

[0034] (4) The mixed concrete was placed in a cubic mold with a size of 100 mm × 100 mm × 100 mm in three layers by manual vibration. Each layer was vibrated 25 times. The molding surface was smoothed with a spatula. The molding surface was covered with a plastic film and sealed for 24 hours before demolding. After demolding, the concrete was cured in a standard curing room with a temperature of 20°C and a relative humidity of 95% until the specified age, and low-alkali regeneration vegetation concrete was obtained.

[0035] The alkali reduction method of low-alkali regenerated vegetation concrete specifically includes the following steps: take out the vegetation concrete specimen that has been cured for 28 days, remove the dust and debris on the surface, and put it into a 60° oven until the surface of the specimen is dry. Place the dried vegetation concrete specimen in a vacuum device, add silane impregnating agent to cover all the specimens, seal it, and use a vacuum pump to evacuate the container to maintain the vacuum degree at -0.1MPa for 40 minutes. Turn off the vacuum pump and all switches, take out the sample, wipe the surface liquid and place it in the laboratory to dry naturally, and perform performance testing after drying.

[0036] Embodiment 2:

[0037] This embodiment shows a method for preparing low-alkali regeneration vegetation concrete, which includes the following steps:

[0038] (1) The discarded laboratory fly ash concrete test blocks with a strength grade of C30 and a large amount of fly ash were crushed by a jaw crusher and manually sieved to obtain recycled coarse aggregate with a particle size of 10-20 mm. The recycled aggregate was washed with clean water to remove impurities such as dust and soil on the surface, and then dried naturally for later use;

[0039] (2) Pour the recycled coarse aggregate into a water glass solution with a concentration of 8% and soak it for 12 hours, take it out and drain it, then spread it out and place it in a ventilated and cool place. Take it out and turn it from time to time within 1 hour to prevent it from sticking, and let it dry naturally to obtain reinforced recycled aggregate;

[0040] (3) 2.76 parts of low-alkali sulphoaluminate cement, 0.92 parts of ordinary Portland cement, 0.80 parts of fly ash and 0.26 parts of silica fume were added into a mixer and stirred for 30 seconds to mix the cementitious materials evenly. Then, 0.78 parts of water, 0.01 parts of water reducer and 0.01 parts of retarder were added and stirred for 60 seconds to mix the cementitious materials and water evenly. Finally, 28.42 parts of reinforced recycled aggregate were added into the mixer, and then 0.78 parts of water, 0.01 parts of water reducer and 0.021 parts of retarder were added and stirred for 120 seconds to mix the various components evenly until the cementitious material slurry evenly covered the surface of the aggregate and the surface of the aggregate was shiny.

[0041] (4) The mixed concrete was placed in a cubic mold with a size of 100 mm × 100 mm × 100 mm in three layers by manual vibration. Each layer was vibrated 25 times. The molding surface was smoothed with a spatula. The molding surface was covered with a plastic film and sealed for 24 hours before demolding. After demolding, the concrete was cured in a standard curing room with a temperature of 20°C and a relative humidity of 95% until the specified age, and low-alkali regeneration vegetation concrete was obtained.

[0042] The alkali reduction method of low-alkali regenerated vegetation concrete specifically includes the following steps: take out the vegetation concrete specimen that has been cured for 28 days, remove the dust and debris on the surface, and put it in a 60°C oven until the surface of the specimen is dry. Place the dried vegetation concrete specimen in a vacuum device, add silane impregnating agent to cover all the specimens, seal it, and use a vacuum pump to evacuate the container to maintain the vacuum degree at -0.1MPa for 40 minutes. Turn off the vacuum pump and all switches, take out the sample, wipe the surface liquid and place it in the laboratory to dry naturally, and perform performance testing after drying.

[0043] Embodiment 3:

[0044] This embodiment shows a method for preparing low-alkali regeneration vegetation concrete, which includes the following steps:

[0045] (1) The discarded laboratory fly ash concrete test blocks with a strength grade of C30 and a large amount of fly ash were crushed by a jaw crusher and manually sieved to obtain recycled coarse aggregate with a particle size of 10-20 mm. The recycled aggregate was washed with clean water to remove impurities such as dust and soil on the surface, and then dried naturally for later use;

[0046] (2) Pour the recycled coarse aggregate into a water glass solution with a concentration of 8% and soak it for 12 hours, take it out and drain it, then spread it out and place it in a ventilated and cool place. Take it out and turn it from time to time within 1 hour to prevent it from sticking, and let it dry naturally to obtain reinforced recycled aggregate;

[0047] (3) 3.06 parts of low-alkali sulphoaluminate cement, 1.02 parts of ordinary Portland cement, 0.96 parts of fly ash and 0.41 parts of silica fume were added into a mixer and stirred for 30 seconds to mix the cementitious materials evenly. Then, 0.81 parts of water, 0.02 parts of water reducer and 0.012 parts of retarder were added and stirred for 60 seconds to mix the cementitious materials and water evenly. Finally, 28.81 parts of reinforced recycled aggregate were added into the mixer, and then 0.81 parts of water, 0.02 parts of water reducer and 0.012 parts of retarder were added and stirred for 120 seconds to mix the various components evenly until the cementitious material slurry evenly covered the surface of the aggregate and the surface of the aggregate was shiny.

[0048] (4) The mixed concrete was placed in a cubic mold with a size of 100 mm × 100 mm × 100 mm in three layers by manual vibration. Each layer was vibrated 25 times. The molding surface was smoothed with a spatula. The molding surface was covered with a plastic film and sealed for 24 hours before demolding. After demolding, the concrete was cured in a standard curing room with a temperature of 20°C and a relative humidity of 95% until the specified age, and low-alkali regeneration vegetation concrete was obtained.

[0049] The alkali reduction method of low-alkali regenerated vegetation concrete specifically includes the following steps: take out the vegetation concrete specimen that has been cured for 28 days, remove the dust and debris on the surface, and put it into a 60° oven until the surface of the specimen is dry. Place the dried vegetation concrete specimen in a vacuum device, add silane impregnating agent to cover all the specimens, seal it, and use a vacuum pump to evacuate the container to maintain the vacuum degree at -0.1MPa for 40 minutes. Turn off the vacuum pump and all switches, take out the sample, wipe the surface liquid and place it in the laboratory to dry naturally, and perform performance testing after drying.

[0050] Comparative Example 1: It is basically the same as Example 1, except that ordinary Portland cement is used as cement.

[0051] Comparative Example 2: It is basically the same as Example 1, except that the recycled aggregate used is not strengthened by soaking in water glass solution.

[0052] Comparative Example 3: It is basically the same as Example 1, except that the prepared vegetation concrete is not subjected to silane soaking and vacuum treatment.

[0053] Comparative Example 4: It is basically the same as Example 1, except that the prepared vegetation concrete is treated by silane immersion.

[0054] Comparative Example 5: It is basically the same as Example 1, except that the fly ash used is Grade II fly ash, and the residue on a 45 μm square sieve is 3.2%.

[0055] Comparative Example 6: The method is basically the same as Example 1, except that in step (3), water, water reducing agent and retarder are not added in batches.

[0056] Comparative Example 7 is substantially the same as Example 1, except that the vacuuming is maintained for 20 minutes.

[0057] Comparative Example 8 is substantially the same as Example 1, except that the vacuuming is maintained for 60 minutes.

[0058]

Performance test

[0059] (1) Porosity

[0060] The drainage method was used to test the porosity of the vegetation concrete. The length a, width b, and height h of the vegetation concrete test block were measured with a vernier caliper, and the average value was taken for three measurements to calculate the apparent volume V of the test block; the test block was immersed in water until it was saturated with water, and its mass M in water was weighed with a water balance. 1 ; Dry the test piece in an oven to constant weight and weigh its mass M 2 ; Calculate the porosity P according to the following formula:

[0061]

[0062] Where: P ~ measured porosity, %;

[0063] M 1 ~~The mass of the test piece in water, g;

[0064] M 2 ~~The mass of the test piece in dry state, g;

[0065] ρ~~density of water, g / cm3;

[0066] V~~apparent volume of test block, cm3.

[0067] (2) pH value

[0068] The porous matrix immersion method of planted concrete is used to reflect the alkalinity change of the pores inside the porous concrete matrix through the change of the pH value of the pore contact water. The specific operation method is as follows: place a planted concrete test block with a size of 100mm×100mm×100mm in a plastic container, inject clean water into the container until it covers the upper surface of the test block by at least 5cm, and seal it. After 24 hours, extract the upper, middle and lower three layers of immersion water solution in the plastic container, and use an acidometer to measure the pH value of the upper, middle and lower three layers of water solution respectively. Take the average pH value to reduce the error, re-inject an equal amount of clean water and repeat the test according to this method until the pH test value of the water solution tends to be stable.

[0069] (3) Compressive strength

[0070] A cubic specimen with a size of 100mm×100mm×100mm was used, and the test method was carried out in accordance with the current national standard GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".

[0071] The test results of all embodiments and comparative examples are shown in Table 1.

[0072] Table 1 Test results of vegetation concrete performance

[0073]

[0074]

[0075] From the data of Comparative Examples 1 and 3, it can be seen that the pH of the vegetation concrete prepared with silicate cement and the vegetation concrete without alkali reduction treatment is high and is not suitable for plant growth. The present invention significantly reduces the pH value of the pore environment of the vegetation concrete by adding low-alkali cement and using a silane impregnating agent to reduce the alkali of the vegetation concrete. The prepared vegetation concrete not only has good physical properties, but also can effectively promote the growth of plant roots inside the concrete to achieve ecological restoration.

[0076] It can be seen from the data of comparative example 2 that the strength of the vegetation concrete prepared from the recycled coarse aggregate without strengthening treatment is low, because the surface of the recycled aggregate is not only attached with many weak mortars, but also contains a lot of holes and gaps, and its physical and mechanical properties are relatively poor. Soaking the recycled aggregate in a water glass solution can improve the performance of the recycled aggregate. The water glass can penetrate into the internal structure of the recycled aggregate, and when hardened, silica gel can be precipitated to bond and fill micro cracks and holes. At the same time, the water glass can react with the hydration products of the old mortar layer to generate hydrated calcium silicate and calcium aluminate, further repairing the pores and cracks, and improving the strength and durability of the aggregate. The present invention optimizes the performance of the recycled aggregate by strengthening the treatment of the recycled aggregate, so that the recycled coarse aggregate can be more used in the vegetation concrete, thereby recycling resources and reducing the damage of concrete waste to the environment.

[0077] It can be seen from the data of Comparative Example 4 that the alkalinity of the regenerated vegetation concrete soaked in silane has increased to a certain extent compared with the alkalinity of the regenerated vegetation concrete soaked in silane and vacuum treated. This shows that the silane soaking and vacuum treatment method is more effective in reducing the alkalinity of the regenerated vegetation concrete.

[0078] It can be seen from the data of Comparative Example 5 that the compressive strength and alkalinity of the regenerated vegetation concrete added with Grade II fly ash do not change much, and the alkalinity of the regenerated vegetation concrete is reduced to a certain extent, which shows that ultrafine fly ash has a certain promoting effect on increasing the compressive strength and reducing the alkalinity of the regenerated vegetation concrete.

[0079] It can be seen from the data of Comparative Example 6 that the addition of water, water reducing agent and retarder in batches has little effect on the compressive strength of the regenerated vegetation concrete, and has almost no effect on the alkalinity of the regenerated vegetation concrete.

[0080] It can be seen from the data of Comparative Examples 7 and 8 that as the vacuum treatment time of silane immersion increases, the alkalinity of the regenerated vegetation concrete will gradually decrease. After 40 minutes of silane immersion, the effect of reducing the alkalinity of the regenerated vegetation concrete is not obvious. This is because under a certain vacuum degree, increasing the vacuum time will not increase the depth of silane immersion into the concrete, and the hydrophobic effect of silane has basically reached saturation.

[0081] Obviously, the embodiments described above are only some embodiments of the present invention, rather than all embodiments, but do not limit the patent scope of the present invention. The present invention can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. Although the present invention has been described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacements for some of the technical features therein. Any equivalent structure made using the contents of the present invention specification, directly or indirectly used in other related technical fields, is also within the scope of patent protection of the present invention.

Claims

1. A low-alkali regenerated vegetation concrete, It is characterized in that The raw materials of the bio-concrete include the following components in parts by weight: 1421-1460 parts of recycled aggregate, 184-224 parts of cement, 40-56 parts of fly ash, 13-28 parts of silica fume, 1-3 parts of water reducer, 1-1.4 parts of retarder, and 78-84 parts of water; The recycled aggregate is a reinforced recycled aggregate obtained by being modified by soaking in a water glass solution; and the fly ash is ultrafine fly ash.

2. The low-alkali regeneration vegetation concrete according to claim 1, It is characterized in that The particle size of the ultrafine fly ash is less than 10 μm.

3. The low-alkali regeneration vegetation concrete according to claim 1, It is characterized in that The cement is prepared by compounding low-alkalinity sulphoaluminate cement and ordinary silicate cement in a weight ratio of 3 to 4:

1.

4. The low-alkali regeneration vegetation concrete according to claim 3, It is characterized in that The low-alkalinity sulphoaluminate cement is L·SAC42.5 grade low-alkalinity sulphoaluminate cement; and the ordinary Portland cement is P·O 42.5 grade ordinary Portland cement.

5. The low-alkali regeneration vegetation concrete according to claim 1, It is characterized in that The particle size of the recycled aggregate is 10-20 mm.

6. A method for preparing low-alkali regenerated vegetation concrete, It is characterized in that It includes the following steps: (1) The discarded concrete test blocks in the laboratory are crushed by a jaw crusher to obtain recycled coarse aggregate with a particle size of 10-20 mm, which is then cleaned and removed for later use; (2) Pour the recycled coarse aggregate into a water glass solution and soak it, take it out and drain it, then spread it out and place it in a ventilated and cool place, turn it over regularly to prevent it from sticking, and let it dry naturally to obtain reinforced recycled aggregate; (3) Prepare raw materials according to the following weight parts: 1421-1460 parts of recycled aggregate, 184-224 parts of cement, 40-56 parts of fly ash, 13-28 parts of silica fume, 1-3 parts of water reducer, 1-1.4 parts of retarder, and 78-84 parts of water; Put cement, fly ash and silica fume into a mixer, stir and mix them evenly, add part of water and part of admixture, continue stirring to make the cementitious material and water evenly mixed, add the reinforced recycled aggregate into the mixer, add the remaining water and admixture, continue stirring to obtain a concrete mixture; (4) Pour the prepared concrete mixture into a mold and use a vibration molding process to produce low-alkali regenerated biomass concrete.

7. The method for preparing low-alkali regeneration vegetation concrete according to claim 6, It is characterized in that The aggregate surface of the concrete mixture is glossy.

8. The method for preparing low-alkali regeneration vegetation concrete according to claim 6, It is characterized in that Step (4) is specifically as follows: the prepared concrete mixture is loaded into the mold in multiple layers, each layer is vibrated 25 times, and after being filled, the side of the test mold is gently tapped with a rubber hammer, and the molding surface is smoothed with a spatula, and the mold is removed after sealing and curing on the molding surface.

9. A method for reducing alkali in low-alkali regenerated vegetation concrete. It is characterized in that The cured vegetation concrete is immersed in a silane impregnating agent for vacuum impregnation treatment.

10. The alkali reduction method according to claim 9, It is characterized in that It includes the following steps: Place the cured green concrete in an oven until the surface of the specimen is dry; place the dry green concrete specimen in a vacuum device, add silane impregnating agent to cover the entire specimen, keep the vacuum degree in the container below -0.1MPa, and maintain it for more than 40 minutes; take out the specimen, wipe the surface liquid and let it air dry naturally.

Citation Information

Patent Citations

  • Recycled aggregate plant-growing type concrete and preparing method thereof

    CN105272063A

  • Preparation method of strengthened recycled aggregate and strengthened recycled aggregate concrete

    CN106477929A

  • Preparation method for precast concrete with resistance to water penetration and freezing-thawing

    CN109265095A

  • Alkalinity reduction treatment method for ecological concrete

    CN109400208A

  • Waterproof sealing of deep cracks in concrete - by impregnating the cleaned crack with a silane compsn. and applying a pourable sealing compsn. contg. an organo-silane

    DE2818445A1