High-content ardealite gel material hardened body and preparation method thereof

Through the pressing molding process of the hardener of high-addition phosphogypsum gel material, combined with modified phosphogypsum, auxiliary active powder and alkalinity regulator, the low amount of phosphogypsum gel material and poor mechanical properties in concrete are solved. The problem has achieved the improvement of high strength and volume stability.

CN118993678AInactive Publication Date: 2024-11-22WUHAN UNIV OF TECH +1

Patent Information

Application Number
CN202411110863.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing phosphogypsum gelling materials are too low in the manufacturing of concrete products, cumbersome in the process, poor mechanical properties, and difficult to achieve high strength and volume stability.

Method used

Using high-dose phosphogypsum gel material hardener, through the combination of modified phosphogypsum, auxiliary active powder and alkalinity regulator, a compactly packed hydrated product is formed using the press molding process to regulate chemical reaction balance to improve the hardener density and mechanical properties.

Benefits of technology

The compressive strength of the hardened body of the phosphogypsum gelling material is improved to above 60MPa, reducing the risks of plastic shrinkage and dry shrinkage, ensuring volume stability, and enhancing the physical and mechanical properties of the hardened body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004992157520000081
    Figure BDA0004992157520000081
  • Figure BDA0004992157520000101
    Figure BDA0004992157520000101
  • Figure BDA0004992157520000121
    Figure BDA0004992157520000121
Patent Text Reader

Abstract

The invention provides a high-content ardealite gel material hardened body and a preparation method thereof, and belongs to the field of building materials, the high-content ardealite gel material hardened body comprises the following components according to the mass ratio: modified ardealite, auxiliary active powder and an alkalinity regulator, the components are uniformly mixed to form a mixture taking ardealite as a main body, and the mixture is mixed with the auxiliary active powder and the alkalinity regulator to form the high-content ardealite gel material hardened body. Pressing into a phosphogypsum cementing material hardened body through a compression molding process; the ardealite particles and the auxiliary active powder particles form a close packing and filling relationship due to differential matching between particle sizes, so that the porosity of a hardened body is reduced, and the compactness is improved; the alkalinity regulator is used for regulating the initial alkalinity of the cementing material, and the alkalinity is reduced along with the proceeding of the chemical reaction, so that the generation of chemical reaction products is slowed down. Under the condition of a certain material mixing ratio, the optimal forming pressure is determined by adopting a relation curve of the forming pressure and the apparent density, so that a blank of the mixture can reach relatively high compactness, and meanwhile, a certain space is reserved for generation of subsequent hydration products, so that the high-strength and high-performance hardened body of the high-content phosphogypsum cementing material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a hardened body of a high-dosage phosphogypsum gel material and a preparation method thereof. Background Art

[0002] Phosphogypsum is a solid precipitate of calcium sulfate discharged during the wet process of producing phosphoric acid. Every ton of phosphoric acid produced will produce 4 to 6 tons of phosphogypsum. The global stockpile of phosphogypsum is as high as 6 billion tons. Among them, my country, as a major producer of phosphogypsum, has a stockpile of about 800 million tons, and the new phosphogypsum production is about 78 million tons / year, but the comprehensive utilization rate is only about 40%. Stacking treatment is still the main method for disposing of excess phosphogypsum. There are many impurity elements inside phosphogypsum. Large-scale stockpiling not only occupies a large amount of land resources, but also pollutes the surrounding soil, water resources and atmosphere, seriously threatening human health and life safety. Therefore, how to deal with the excess phosphogypsum on a large scale and promote the resource utilization of phosphogypsum has become an urgent problem to be solved.

[0003] According to statistics, the utilization of phosphogypsum in the building materials industry accounts for 36%, which is the main industry in my country that consumes phosphogypsum. There are two major technical approaches to the comprehensive utilization of phosphogypsum. One is the air-hardening cementitious material approach, which can develop and produce gypsum products such as gypsum boards and gypsum blocks that are only suitable for air environments, while the other approach is to develop hydraulic cementitious materials and products that can be used in air and water environments. The development of hydraulic cementitious materials with phosphogypsum as the main component has gone through three stages: the first is super-sulfated cement (gypsum slag cement), in which the phosphogypsum content does not exceed 20%; the second is persulfated phosphogypsum slag cementitious materials, in which the phosphogypsum content is 40% to 50%; third, recently, an ultra-high-dosage hydraulic phosphogypsum cementitious material system has appeared on the basis of persulfated phosphogypsum slag cementitious materials. The phosphogypsum content in this cementitious material can reach 50% to 95%, which greatly improves the utilization rate of phosphogypsum.

[0004] However, in the existing concrete product manufacturing model, sand and gravel aggregates generally account for about 70%, while cementitious materials and water only account for about 30%. When concrete products are made with phosphogypsum-based cementitious materials, the amount of phosphogypsum in the cementitious materials will be "diluted" to a fairly low level. Chinese patent CN115872644A introduces a high-dosage phosphogypsum concrete, in which the amount of phosphogypsum reaches 80% to 95%, which is a major improvement in the comprehensive utilization of phosphogypsum. However, when preparing this concrete, most of the phosphogypsum cementitious materials need to be made into spherical aggregate particles in advance, and then bonded with the cementitious materials through a casting molding process to form a hardened body, in which the aggregate preparation process is an energy-consuming and time-consuming process. On the other hand, the compressive strength of the hardened body obtained by combining the phosphogypsum cementitious materials with the phosphogypsum aggregates in this case is not high, with a maximum of only 25.2MPa, which greatly limits its practicality.

[0005] The present invention attempts to solve the problem of low consumption of phosphogypsum in the current comprehensive utilization of phosphogypsum, or the problem of complicated process and poor mechanical properties despite high consumption of phosphogypsum. The key technology is to directly make a hardened body with phosphogypsum-based mixture and make it have the same performance as high-strength concrete. Summary of the invention

[0006] In view of this, the present invention proposes a hardened body of a high-dosage phosphogypsum gel material and a preparation method thereof, which are used to solve the problem that when a hardened body without sand and gravel is made from a high-dosage phosphogypsum gelling material to replace cement products, the product is difficult to achieve sufficient physical and mechanical properties and volume stability, thereby affecting the strength of concrete.

[0007] The technical solution of the present invention is achieved as follows: the present invention provides a high-dosage phosphogypsum gel material hardener, which includes the following components in terms of mass ratio: modified phosphogypsum, 70% to 90%; auxiliary active powder, 10% to 30%; alkalinity regulator, 0.01% to 1%; wherein, after the above components are evenly mixed to form a phosphogypsum cementitious material mixture, it is pressed into a phosphogypsum cementitious material hardener through a pressing molding process, and the optimal molding pressure of the hardener is 70 to 80% of the corresponding molding pressure value when the maximum apparent density is reached; the phosphogypsum particles and the auxiliary active powder particles react with each other to form hydration products and fill them between the phosphogypsum particles. At the same time, the close stacking and filling between the differentiated powder particles can improve the density of the hardener; the alkalinity regulator is used to adjust the initial alkalinity of the mixture system and adjust the process of chemical reaction and hydration product generation in the mixture. The main hydration products generated in the mixture are calcium sulfonate and C-(A)-SH gel.

[0008] The present invention aims to utilize phosphogypsum in large dosage and high efficiency, and solve the problem of volume stability of the hardened body of phosphogypsum cementitious material while improving the strength of the hardened body of phosphogypsum cementitious material to a practical level. Conventional concrete products have a large amount of sand and gravel aggregates as skeleton support, and the shrinkage produced by the cementitious material during the hydration and hardening process is largely offset by the sand and gravel. However, if the hardened body is prepared entirely by phosphogypsum cementitious material without sand and gravel, on the one hand, this hardened body is faced with the risk of large plastic shrinkage and drying shrinkage, and on the other hand, it is also faced with the risk of expansion and cracking caused by the large amount of calcium sulfonate generated. Therefore, the basic starting point of the present invention is to focus on grasping the physical particle accumulation balance and the chemical hydration product balance in the process of preparing this cementitious material hardened body.

[0009] The solution adopted by the present invention is that, firstly, the phosphogypsum cementitious material is pressed into a hardened body with a certain density through a compression molding process, and this density can also reserve a certain space for the subsequent production of hydration products, and the corresponding optimal molding pressure is determined according to the pressure-blank apparent density curve; secondly, the physical properties of the phosphogypsum particles and the auxiliary active powder particles are combined to achieve close packing of the particles to further reduce the hardened body voids and improve the density; finally, by regulating the ratio and amount of active silicon and aluminum in the system and the alkalinity of the system, an appropriate amount of hydration products is generated to wrap the phosphogypsum particles or further fill the remaining voids inside the hardened body, forming a more compact matrix structure to improve the mechanical properties of the hardened body of the phosphogypsum cementitious material. As the hydration reaction proceeds, the total deformation of the hardened body due to drying shrinkage and plastic shrinkage is quite small, and even a certain degree of micro-expansion is generated. In order to avoid expansion cracking caused by the large-scale generation of hydration products, especially calcium sulfonate, on the one hand, the material particles are closely contacted by controlling the molding pressure, and at the same time, a certain expansion space of the hydration products is reserved. On the other hand, with the decrease of alkalinity in the cementitious material, the generation rate of new hydration products will be greatly reduced.

[0010] In summary, in order to achieve higher mechanical properties for the hardened body, the present invention includes three mutually synergistic chemical reactions: first, a small amount of silicate cement and steel slag powder spontaneously react to provide a certain alkalinity, sulfate stimulates the chemical reaction of mineral powder, and alkali stimulates the chemical reaction of silica-alumina active components. The products of these reactions provide a "binder" for the bonding between particles; second, the present invention adjusts the molding pressure according to factors such as material composition, design strength, and material dryness and wetness, so that the material particles can be in close contact while reserving a certain gap to provide space for the subsequent generation of hydration products; third, the effect of alkalinity on chemical reactions is used to determine the initial alkalinity range, which is equivalent to setting a "brake button" for the chemical reaction. As the chemical reaction proceeds, the alkalinity of the system decreases and the chemical reaction tends to equilibrium, which provides a guarantee for the volume stability of the hardened body. It should be noted that the purpose of adding the alkalinity regulator in the present invention is to make the alkalinity of the gypsum system reach an optimal range. Therefore, the mass proportion of the alkalinity regulator in the present application is 0.01% to 1%, which is not a definite range value. It represents the means adopted by the present application to achieve the purpose of regulating the alkalinity of the gypsum system by adding the alkalinity regulator.

[0011] On the basis of the above technical solution, preferably, the pressure range when the mixture is pressurized by the compression molding process is 30 to 90 MPa.

[0012] On the basis of the above technical scheme, preferably, the modified phosphogypsum is obtained by adding water to a mixture of original phosphogypsum and calcareous material, mixing them wet and then aging them, the mass of the calcareous material is 2% to 4% of the mass of the original phosphogypsum, and the lime includes one or more of silicate cement, quicklime, mineral powder and carbide slag.

[0013] On the basis of the above technical solution, preferably, the auxiliary active powder material includes one or more of silicate cement, mineral powder, steel slag, metakaolin, silica fume, fly ash and yellow phosphorus slag.

[0014] On the basis of the above technical solution, preferably, the alkalinity regulator comprises one of water glass, sodium carbonate and sodium hydroxide. The alkalinity regulator is chemically pure.

[0015] On the other hand, the present invention also provides a method for preparing a high-dosage phosphogypsum gel material hardener, which is used to prepare the above-mentioned high-dosage phosphogypsum gel material hardener, comprising the following steps: step 1, according to the mix ratio design, respectively weigh the modified phosphogypsum and the auxiliary active powder, and dry mix them for 2 to 3 minutes in a high-speed stirring mode to make them evenly mixed; step 2, add water to the dry mixture and wet mix it for 2 to 3 minutes in a high-speed stirring mode to make it evenly mixed; step 3, adopt a pressing molding process, according to a predetermined molding pressure, fill the mixture into a pressing mold for pressing, demolding, molding and curing, and obtain a high-dosage phosphogypsum gel material hardener. Pressing molding refers to pressing the phosphogypsum gelling material into a hardener with a certain shape, size, density and strength by a press machine. The specific process includes uniform mixing of raw materials, weighing of raw materials, molding of the mixture, pressurization molding, pressure relief and demolding.

[0016] On the basis of the above technical scheme, preferably, in step one, before weighing each component separately according to the mix ratio design, the dry original phosphogypsum and the calcareous material are evenly mixed, the mass of the calcareous material is 2% to 4% of the mass of the original phosphogypsum, and water is added for wet mixing for 30 minutes and then aged for 24 hours to obtain the modified phosphogypsum, and the modified phosphogypsum is dried by oven or sun-drying.

[0017] Further preferably, when water is added to the mixture of dry original phosphogypsum and calcareous material for wet mixing in step one, the mass of the added water is 10% of the mass of the original phosphogypsum; and when water is added to the dry mixture for wet mixing in step two, the mass of the added water is 10% of the mass of the dry mixture.

[0018] On the basis of the above technical solution, preferably, when water is added to the dry mix for wet mixing in step 2, an alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to a range of 11.5 to 13.

[0019] On the basis of the above technical solution, preferably, the hardened body of the high-dosage phosphogypsum gel material finally obtained in step three has a 28d compressive strength of not less than 60 MPa and a softening coefficient of more than 0.8.

[0020] The high-dosage phosphogypsum gel material hardener and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:

[0021] (1) The present invention adopts a compression molding process to press the phosphogypsum cementitious material into a hardened body. The compression molding can make the phosphogypsum particles and the auxiliary active powder closely stacked and in close contact, and the degree of close contact is much greater than the degree of contact between particles in the conventional casting molding method. Relative to the hardened body formed by the conventional casting process, the porosity in the hardened body is greatly reduced and the density is greatly improved. At the same time, the close contact between the particle hydration products brings a strong bonding force, thereby giving the matrix a certain initial strength. With the large-scale generation, crystallization and expansion of hydration products, especially calcium sulfonate, the space originally supplied to the growth and development of hydration products is reduced, and there is a risk of matrix expansion and cracking. The present invention reserves a certain hydration product generation space and expansion space, and uses the law of gradually decreasing alkalinity to slow down and suppress the generation of chemical reaction products, thereby avoiding the risk of matrix cracking.

[0022] (2) The chemical reaction types in the present invention mainly include the autogenous hydration reaction of silicate cement and steel slag, the sulfate-induced reaction between phosphogypsum and mineral powder, the alkali-induced reaction between active silica-alumina and calcium hydroxide, and the dissolution and recrystallization of calcium sulfate; the hydration products formed are mainly ettringite and C-(A)-SH gel and recrystallized calcium sulfate crystals; from the perspective of chemical reactants, the main factors controlling the chemical balance of the hydration reaction are active silicon ions, active aluminum ions, OH - By adjusting the composition and proportion of the auxiliary active powder material, the equilibrium point of the hydration reaction can be adjusted, thereby adjusting the thickness of the hydration product layer on the surface of the phosphogypsum particles, and then the alkalinity regulator can be used to adjust the system OH - Concentration can accelerate the hydration reaction process or maintain the stability of the hydration product, thereby achieving the regulation of the physical and mechanical properties of the hardened body.

[0023] (3) The present invention uses calcareous materials to modify the original phosphogypsum. On the one hand, the alkaline substances (calcium oxide, calcium hydroxide) in the calcareous materials are used to neutralize the residual acidic substances in the original phosphogypsum. On the other hand, the calcareous materials are used to remove soluble phosphorus and fluorine impurities in the original phosphogypsum, thereby reducing the adverse effects of impurities on the performance of the phosphogypsum product. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] A high-dosage phosphogypsum gel material hardener of the present invention includes the following components by weight: 800 g of modified phosphogypsum; 200 g of auxiliary active powder; 0.01 g of alkalinity regulator or no alkalinity regulator. The modified phosphogypsum is obtained by modifying the original phosphogypsum with a calcareous material, the mass of the calcareous material is 2% of the mass of the original phosphogypsum, and the calcareous material is carbide slag. The auxiliary active powder material includes, by weight, 50 g of silicate cement, 30 g of steel slag, 100 g of mineral powder and 20 g of metakaolin. The alkalinity regulator is sodium hydroxide.

[0027] The invention discloses a method for preparing a high-dosage phosphogypsum gel material hardener, which is used for preparing the high-dosage phosphogypsum gel material hardener, and comprises the following steps: step 1, firstly, dry original phosphogypsum and calcareous material are mixed evenly, and water is added for wet mixing for 30 minutes and then aged for 24 hours to obtain modified phosphogypsum, wherein the mass of the added water is 10% of the mass of the original phosphogypsum, i.e. 80g, and the modified phosphogypsum is dried or sun-dried to be dry; then, the modified phosphogypsum and auxiliary active powder are weighed according to the mix ratio design, and dry mixing is performed for 3 minutes in a high-speed stirring mode to make the mixture evenly mixed, wherein the water-cement ratio is 0.07; step 2, water is added to the dry mixture and wet mixing is performed for 3 minutes in a high-speed stirring mode to make the mixture evenly mixed, wherein the mass of the added water is 10% of the mass of the dry mixture, i.e. 100g; step 3, a pressing molding process is adopted, and the mixture is filled into a pressing mold for pressing, demoulding, molding and curing to obtain a high-dosage phosphogypsum gel material hardener; and the pressure during pressurization is 30MPa.

[0028] Example 2

[0029] This embodiment adopts the same component proportions and preparation steps as those of Embodiment 1, except that in step three, the pressure when the mixture is pressurized by the compression molding process is 45 MPa.

[0030] Example 3

[0031] This embodiment adopts the same component proportions and preparation steps as those of Embodiment 1, except that in step three, the pressure when the mixture is pressurized by the compression molding process is 60 MPa.

[0032] Example 4

[0033] This embodiment adopts the same component ratio and preparation steps as those of Embodiment 1, except that in step three, the pressure when the mixture is pressurized by the compression molding process is 75 MPa.

[0034] Example 5

[0035] This embodiment adopts the same component ratio and preparation steps as those of Embodiment 1, except that in step three, the pressure when the mixture is pressurized by the compression molding process is 90 MPa.

[0036] The samples prepared in Examples 1 to 5 were tested by a compressive strength test. At the same time, a sample obtained by having the same composition ratio as that in Example 1 but without performing a pressing operation was used as a comparative example (serial number 0). The compressive strength of each sample at 3d, 7d and 28d was detected, and the softening coefficient and expansion rate of each sample at 28d were detected. The obtained data are recorded in the following Table 1.

[0037] Table 1

[0038]

[0039] By comparing the data of each embodiment and the comparative example in Table 1, it can be found that each embodiment in this experiment adopts a fixed component ratio, and prepares different phosphogypsum hardened bodies by changing the molding pressure. The results show that with the increase of molding pressure, the mechanical properties of the hardened body show an upward trend, and the compressive strength of the 28d hardened body can reach more than 60MPa; similarly, the expansion rate of the hardened body also shows an upward trend, but the overall expansion rate is maintained at about 1%. It shows that the mechanical properties of the cementitious material can be improved by changing the molding pressure to form a dense stack of particles, and the volume stability of the hardened body can be improved by reserving a certain growth space for hydration products. However, after the molding pressure exceeds 60MPa, the change trend of the compressive strength slows down, and the expansion rate also increases and exceeds the optimal expansion rate of 1%; therefore, when the molding pressure is preferably 60PMPa, both the molding pressure can be reduced and good physical and mechanical properties can be obtained.

[0040] Example 6

[0041] A high-dosage phosphogypsum gel material hardener of the present embodiment includes the following components by mass proportion: 800 g of modified phosphogypsum; 200 g of auxiliary active powder; 0.1 g of alkalinity regulator or no alkalinity regulator is added. Among them, the modified phosphogypsum is obtained by modifying the original phosphogypsum with a calcareous material, the mass of the calcareous material is 2% of the mass of the original phosphogypsum, and the calcareous material is carbide slag. The auxiliary active powder material includes, by mass proportion, 50 g of silicate cement, 50 g of mineral powder, 50 g of yellow phosphorus slag and 50 g of kaolin. The alkalinity regulator package is sodium hydroxide. The same preparation method as in Example 1 is adopted, except that the pressure when the mixture is pressurized by the compression molding process is 60 MPa.

[0042] Example 7

[0043] This embodiment adopts the same component ratio and preparation steps as Example 6, except that the auxiliary active powder material includes, by weight, 50 g of silicate cement, 50 g of mineral powder, 50 g of fly ash and 50 g of metakaolin.

[0044] Example 8

[0045] This embodiment adopts the same component ratio and preparation steps as Example 6, except that the auxiliary active powder material includes, by weight, 50 g of silicate cement, 100 g of mineral powder and 50 g of yellow phosphorus slag.

[0046] Example 9

[0047] This embodiment adopts the same component ratio and preparation steps as Embodiment 6, except that the auxiliary active powder material includes, by weight, 50 g of silicate cement, 100 g of mineral powder and 50 g of fly ash.

[0048] The samples prepared in Examples 6 to 9 were tested by compressive strength test and the compressive strength of each example sample at 3d, 7d and 28d was detected. The softening coefficient and expansion rate of each sample at 28d were also detected, and the obtained data were recorded in Table 2 below.

[0049] Table 2

[0050]

[0051] By comparing the data in Table 2, it can be found that in this experiment, better mechanical properties can be obtained by changing the type and proportion of auxiliary adhesives. The reason is that different types of auxiliary adhesives have certain differences in particle size and compatibility with modified phosphogypsum particle size. Taking Examples 8 and 9 as examples, when the mineral powder dosage is 10%, better mechanical properties can be obtained, and the compressive strength is above 60MPa; and through Examples 6 and 7, it can be found that replacing part of the mineral powder with yellow phosphorus slag or fly ash, although the mechanical properties have decreased, a higher softening coefficient can be obtained, and the durability of the hardened body is improved. It shows that by regulating the type and proportion of auxiliary active adhesives to regulate the hydration reaction balance of the system, the physical and mechanical properties and durability of the hardened body of high-dosage phosphogypsum cementitious materials can be regulated to obtain phosphogypsum products with the best performance.

[0052] Example 10

[0053] A high-dosage phosphogypsum gel material hardener of the present embodiment includes the following components in terms of mass ratio: 800 modified phosphogypsum; 200 auxiliary active powder; 0.1g alkalinity regulator or no alkalinity regulator. Among them, the modified phosphogypsum is obtained by modifying the original phosphogypsum with a calcareous material, the mass of the calcareous material is 2% of the mass of the original phosphogypsum, and the lime is carbide slag. The auxiliary active powder material includes, in terms of mass ratio, 50g of silicate cement, 30g of steel slag and 120g of mineral powder. The alkalinity regulator package is sodium hydroxide. The same preparation method as in Example 1 is adopted, except that the pressure when the mixture is pressurized by the pressing molding process is 60MPa. At the same time, the pH of the mixture system does not reach the range of 11.5 to 13.

[0054] Embodiment 11

[0055] This embodiment adopts the same component ratio and preparation steps as Example 10, except that the auxiliary active powder material includes, by weight, 50 g of silicate cement, 30 g of steel slag, 100 g of mineral powder and 20 g of metakaolin. The pH of the mixture system does not reach the range of 11.5 to 13.

[0056] Example 12

[0057] This embodiment adopts the same component proportions and preparation steps as those of Embodiment 10, except that the auxiliary active powder material includes, in terms of mass proportion, 50 g of silicate cement, 30 g of steel slag and 120 g of mineral powder; while adding water to the dry mixture for wet mixing, 10 g of alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to the range of 11.5 to 13.

[0058] Example 13

[0059] This embodiment adopts the same component ratio and preparation steps as Embodiment 10, except that the auxiliary active powder material includes, in terms of mass proportion, 50 g of silicate cement, 30 g of steel slag, 100 g of mineral powder and 20 g of metakaolin; while adding water to the dry mixture for wet mixing, 10 g of alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to the range of 11.5 to 13.

[0060] Embodiment 14

[0061] This embodiment adopts the same component ratio and preparation steps as those of Embodiment 10, except that the auxiliary active powder material includes, in terms of mass proportion, 50 g of silicate cement, 30 g of steel slag and 120 g of mineral powder; while adding water to the dry mixture for wet mixing, 20 g of alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to exceed the range of 11.5 to 13, so that the alkalinity of the system is too high.

[0062] Embodiment 15

[0063] This embodiment adopts the same component proportions and preparation steps as those of Embodiment 10, except that the auxiliary active powder material includes, in terms of weight percentage, 50 g of silicate cement, 30 g of steel slag, 100 g of mineral powder and 20 g of metakaolin; while adding water to the dry mixture for wet mixing, 20 g of alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to exceed the range of 11.5 to 13, so that the alkalinity of the system is too high.

[0064] The samples prepared in Examples 10 to 15 were tested by a compressive strength test and the compressive strength of each example sample at 3d, 7d and 28d was detected. The softening coefficient and expansion rate of each sample at 28d were also detected, and the obtained data were recorded in Table 3 below.

[0065] Table 3

[0066]

[0067] By comparing the data of Examples 10 and 12 and 11 and 13 in Table 3, it can be found that the amount of alkalinity regulator added in Examples 10 and 11 is very small, and it is difficult to meet the purpose of adjusting the alkalinity of the gypsum system of the corresponding samples to the range of 11.5 to 13. This experiment adjusts the pH value of the gypsum gel system by adjusting the alkalinity regulator. The results show that the 28d compressive strength and softening coefficient of the group incorporating a certain amount of alkalinity regulator are higher than those of the group not incorporating the alkalinity regulator; through the data of Examples 14 and 15, it can be found that when the alkalinity regulator is added in an amount exceeding 1%, the alkalinity of the gypsum system is too high, which may have an adverse effect on the compressive strength and softening coefficient of the sample. Therefore, it can be inferred that maintaining the alkalinity in the system within a reasonable range through the alkalinity regulator is conducive to improving the late strength development and durability of the hardened body.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-dosage phosphogypsum gel material hardener, characterized in that: The components include the following in terms of mass proportion: Modified phosphogypsum, 70% to 90%; Auxiliary active powder, 10% to 30%; Alkalinity regulator, 0.01% to 1%; Among them, after the above components are evenly mixed to form a phosphogypsum cementitious material mixture, it is pressed into a phosphogypsum cementitious material hardened body through a pressing molding process; the optimal molding pressure of the hardened body is 70-80% of the corresponding molding pressure value when the maximum apparent density is reached.

2. The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to claim 1, characterized in that: The pressure range of the mixed material when pressurized by the compression molding process is 30 to 90 MPa.

3. The high-dosage phosphogypsum gel material hardened body according to claim 1, characterized in that: The modified phosphogypsum is obtained by adding water to a mixture of original phosphogypsum and calcareous material, mixing them wet and then aging them. The mass of the calcareous material is 2% to 4% of the mass of the original phosphogypsum. The calcareous material includes one or more of silicate cement, quicklime, mineral powder and carbide slag.

4. The high-dosage phosphogypsum gel material hardened body according to claim 1, characterized in that: The auxiliary active powder material includes one or more of silicate cement, mineral powder, steel slag, metakaolin, silica fume, fly ash and yellow phosphorus slag.

5. The hardened body of high-dosage phosphogypsum gel material according to claim 1, characterized in that: The alkalinity regulator includes one of water glass, sodium carbonate and sodium hydroxide.

6. A method for preparing a hardened body of a high-dosage phosphogypsum gel material, characterized in that: The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to any one of claims 1 to 5 comprises the following steps: Step 1: According to the mix ratio design, the modified phosphogypsum and the auxiliary active powder are weighed and dry-mixed for 2 to 3 minutes in a high-speed stirring mode to make them uniformly mixed; Step 2, adding water to the dry mix and wet mixing for 2 to 3 minutes in a high-speed stirring mode to make the mixture uniform; Step three, using a compression molding process, according to a predetermined molding pressure, the mixture is filled into a compression mold for compression, demolding, molding and curing to obtain a hardened body of a high-doped phosphogypsum gel material.

7. The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to claim 6, characterized in that: In the step 1, before weighing each component according to the mix ratio design, the dry original phosphogypsum and the calcareous material are evenly mixed, the mass of the calcareous material is 2% to 4% of the mass of the original phosphogypsum, and water is added for wet mixing for 30 minutes and then aged for 24 hours to obtain the modified phosphogypsum, and the modified phosphogypsum is dried by oven or sun-drying.

8. The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to claim 7, characterized in that: In the step 1, when water is added to the mixture of dry original phosphogypsum and calcareous material for wet mixing, the mass of the added water is 10% of the mass of the original phosphogypsum; in the step 2, when water is added to the dry mixture for wet mixing, the mass of the added water is 10% of the mass of the dry mixture.

9. The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to claim 6, characterized in that: When water is added to the dry mixture for wet mixing in step 2, an alkalinity regulator is added as an external admixture to adjust the pH of the mixture system to a range of 11.5 to 13.

10. The method for preparing a hardened body of a high-dosage phosphogypsum gel material according to claim 6, characterized in that: The hardened body of the high-dosage phosphogypsum gel material finally obtained in step three has a 28d compressive strength of not less than 60 MPa and a softening coefficient of more than 0.8.

Citation Information

Patent Citations

  • Phosphogypsum hydraulic cementing material as well as preparation method and application thereof

    CN115872644A

Cited By

  • Mine pit repairing material as well as preparation method and application thereof

    CN119390399A