Modified phosphogypsum foam concrete material and preparation method thereof

By adding calcium carbide slag and ultrasonic shock treatment to phosphogypsum, the impact of phosphogypsum impurities on concrete performance is solved, efficient and environmentally friendly modification treatment is achieved, and the strength and production efficiency of phosphogypsum foam concrete is improved, and pollution is avoided. High energy consumption.

CN118993682APending Publication Date: 2024-11-22GUIZHOU TEMEIDA TECHNOLOGY BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213959.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The method of removing impurities of modified phosphogypsum in the prior art has problems of high energy consumption and pollution of the environment, especially the corrosion and calcination methods of water washing equipment are large and it is difficult to achieve large-scale mass production.

Method used

The neutralization method is used to adjust the hydration environment of phosphogypsum by adding calcium carbide slag, and combined with ultrasonic oscillation, the water-soluble phosphorus in the phosphogypsum forms insoluble apatite, thereby improving the concrete strength and avoiding high-temperature calcination and acidic wastewater generation.

Benefits of technology

The strength of phosphogypsum foam concrete is improved, energy consumption and pollution are reduced, environmentally friendly industrial production is achieved, and the alkaline phenomenon is controlled, and environmental pollution is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to a modified ardealite foam concrete material and a preparation method thereof, and the modified ardealite foam concrete material comprises 50-70 parts of undisturbed ardealite, 20-30 parts of fly ash, 6-10 parts of carbide slag, 0.2-0.5 part of polyaluminum chloride, 0.2-0.5 part of calcium formate, 0.01-0.02 part of rubber powder, 0.03-0.05 part of cellulose ether, 0.4-0.6 part of a composite superplasticizer, 25-40 parts of cement and 0.1-0.2 part of a foaming agent. Compared with the prior art, a proper amount of carbide slag is added, so that the technical problems of energy consumption and environmental pollution when the phosphogypsum is modified to eliminate the influence of impurities on the performance of the phosphogypsum building material in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a modified phosphogypsum foam concrete material and a preparation method thereof. Background Art

[0002] Phosphogypsum is a byproduct of the production process of phosphoric acid extraction by sulfuric acid method. It is also an industrial waste residue with calcium sulfate dihydrate as the main component. Its main components are resources such as sulfur and calcium, which have many potential uses. It also contains impurities such as phosphorus, fluorine, alkali metal elements, silicon, aluminum, iron, magnesium, etc. that are harmful to the environment and comprehensive utilization. With the rapid development of the phosphate fertilizer industry, the discharge and stockpiling of phosphogypsum have shown a significant year-on-year increase. The unscientific discharge of phosphogypsum not only increases the land area, but also pollutes the environment, becoming an industrial waste residue that urgently needs to be recycled. Therefore, the conversion and consumption of phosphogypsum has become an urgent problem to be solved.

[0003] Using phosphogypsum as an industrial raw material to produce foamed concrete building materials is currently one of the main conversion and consumption pathways. However, phosphogypsum is rich in impurities such as water-soluble phosphorus and fluorine. Direct use as a building material raw material will affect the strength of the building materials and pollute the environment. Therefore, foamed concrete building materials made from phosphogypsum can usually only be used as indoor building materials with low strength requirements and low waterproof properties. This greatly limits the conversion and consumption of phosphogypsum. In order to broaden the conversion pathways of phosphogypsum and maximize the value of phosphogypsum, it is usually necessary to modify the phosphogypsum to increase the strength of phosphogypsum products.

[0004] At present, in order to eliminate the influence of impurities in phosphogypsum on the performance of phosphogypsum products, researchers have come up with the idea of ​​using water washing or calcination to remove water-soluble impurities such as phosphorus and fluorine in phosphogypsum, or to react impurities to generate inert substances to eliminate the adverse effects of impurities on the performance of building materials. However, these methods themselves have certain defects. The water washing method is difficult to achieve large-scale industrial production, and because phosphogypsum has strong acidity, it is easy to cause equipment corrosion during the water washing process, and the cost of wastewater treatment is high. In addition to removing water-soluble phosphorus, the calcination method can also remove eutectic phosphorus in phosphogypsum crystals, but the calcination temperature is high and the energy consumption is large. At the same time, this method is difficult to achieve large-scale mass production and it is difficult to meet the production process requirements of foam concrete.

[0005] In order to solve the above-mentioned defects, this scheme proposes a modified phosphogypsum foam concrete material and a preparation method thereof, which are used to solve the technical problems of energy consumption and environmental pollution existing in the prior art when modifying phosphogypsum to eliminate the influence of impurities on the performance of phosphogypsum building materials. Summary of the invention

[0006] The present invention aims to provide a modified phosphogypsum foam concrete material and a preparation method thereof, which are mainly used to solve the technical problems of energy consumption and environmental pollution existing in the prior art when modifying phosphogypsum to eliminate the influence of impurities on the performance of phosphogypsum building materials.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] A modified phosphogypsum foam concrete material comprises the following raw materials in parts by weight: 50-70 parts of original phosphogypsum, 20-30 parts of fly ash, 6-10 parts of carbide slag, 0.2-0.5 parts of polyaluminum, 0.2-0.5 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.4-0.6 parts of composite high-efficiency water reducing agent, 25-40 parts of cement and 0.1-0.2 parts of foaming agent.

[0009] Preferably, the composite high-efficiency water reducer is a compound of a naphthalene-based high-efficiency water reducer and a wood-based sodium sulfonate, and the water reduction rate is not less than 20%.

[0011] Preferably, the foaming agent is a plant protein foaming agent.

[0012] A method for preparing a modified phosphogypsum foam concrete material comprises the following steps:

[0013] S1: Add 60-75 parts by weight of phosphogypsum admixture, 25-40 parts of cement, and 45-50 parts of water into a stirring device and mix for 2-3 minutes to obtain a modified phosphogypsum foam concrete mixed slurry;

[0014] S2: adding a foaming agent dilution liquid to a foam making device to prepare foam, and then sending the prepared foam into a modified phosphogypsum concrete slurry through a foam control system for full mixing to obtain a modified phosphogypsum foam concrete pouring slurry;

[0015] S3: The prepared modified phosphogypsum foam concrete pouring slurry is poured on site or molded through a foam concrete equipment pumping system, and naturally cured to obtain a modified phosphogypsum foam concrete material.

[0016] Preferably, in step s1, the phosphogypsum admixture is obtained by mixing and stirring 70-99 parts of modified phosphogypsum powder, 0.2-0.5 parts of polyaluminum, 0.2-0.5 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, and 0.4-0.6 parts of composite high-efficiency water reducing agent, in parts by weight.

[0017] Preferably, in step s1, the preparation of modified phosphogypsum powder comprises the following steps:

[0018] S11: by weight, 50-70 parts of original phosphogypsum, 20-30 parts of fly ash, and 6-10 parts of carbide slag are mixed and stirred in a mixer to obtain a mixture, and the mixture is stored for 40-50 hours for aging to obtain a modified phosphogypsum raw material;

[0019] S12: drying the modified phosphogypsum raw material at 180° C. until the water content is 7%-8%, thereby obtaining the modified phosphogypsum dry material;

[0020] S13: Grinding the modified phosphogypsum dry material to obtain modified phosphogypsum powder.

[0021] Preferably, in step S3, methyl hydrogen silicone oil is evenly applied on the surface of the modified phosphogypsum foam concrete material after natural curing.

[0022] Preferably, the foaming agent dilution is obtained by diluting 0.1-0.2 parts of foaming agent with water at a ratio of 1:30, and the foaming agent is pure plant protein type, with a solid content of 18% and a foaming multiple of 30.

[0023] Preferably, in step S13, the modified phosphogypsum dry material is crushed into 40-200 mesh particles.

[0024] Preferably, in step S11, the mixture is further subjected to ultrasonic vibration for 20 minutes and then aged.

[0025] The beneficial effects of this program are as follows:

[0026] 1. The water-soluble phosphorus impurities in phosphogypsum will hinder the hydration of phosphogypsum, thereby reducing the final strength of concrete. This scheme mainly adopts the neutralization method to modify the original phosphogypsum, because the original phosphogypsum is a strong acidic material, and carbide slag is a strong alkaline material. In the process of concrete preparation, carbide slag is added as a neutralizer, which can increase the pH value in the modified phosphogypsum foam concrete mixed slurry. Under a higher pH value environment, the water-soluble phosphorus dissolved in the phosphogypsum will first combine with the hydroxide ions in the slurry to form insoluble apatite, so that the subsequent hydration of the phosphogypsum can be carried out in an environment without water-soluble phosphorus, eliminating the adverse effects of water-soluble impurities, thereby improving the strength of the final foam concrete material; compared with the existing water washing and calcination method, this method of removing water-soluble phosphorus does not produce a large amount of acidic wastewater, and does not require high-temperature calcination of phosphogypsum. It is environmentally friendly and energy-saving, and solves the technical problems of energy consumption and environmental pollution when modifying phosphogypsum to eliminate the influence of impurities on the performance of phosphogypsum building materials in the prior art.

[0027] 2. The main function of adding carbide slag is to adjust the pH value of the hydration environment of phosphogypsum. When the amount of carbide slag added is too large, the neutralization effect is good, but it may cause serious alkali blooming in the final modified phosphogypsum foam concrete material. After the modified phosphogypsum foam concrete material with serious alkali blooming comes into contact with water, the soluble alkali enters the water and greatly pollutes the natural environment. This scheme strictly controls the amount of carbide slag added, and reduces the degree of alkali blooming while ensuring the final strength of the concrete product. According to the test results, when the amount of carbide slag added is 6-10 parts, the strength of the concrete material is not significantly reduced, but the degree of alkali blooming is greatly reduced.

[0028] 3. After the phosphogypsum and carbide slag are stirred, the mixture is subjected to ultrasonic vibration to fully dissolve the soluble impurities in the phosphogypsum and form an inert precipitate, so that the phosphogypsum can be fully hydrated and the strength of the final modified phosphogypsum foam concrete material is improved. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] A modified phosphogypsum foamed concrete comprises the following raw materials in parts by weight: 50 parts of original phosphogypsum, 20 parts of fly ash, 6 parts of carbide slag, 0.2 parts of polyaluminum, 0.2 parts of calcium formate, 0.01 parts of rubber powder, 0.03 parts of cellulose ether, 0.4 parts of composite high-efficiency water reducing agent, 25 parts of cement, and 0.1 parts of vegetable protein foaming agent. The composite high-efficiency water reducing agent is a 1:1 compound of naphthalene-based high-efficiency water reducing agent and sodium lignin sulfonate.

[0032] A method for preparing a modified phosphogypsum foam concrete material comprises the following steps:

[0033] S1: Preparation of modified phosphogypsum foam concrete mixed slurry:

[0034] S11: 50 parts by weight of original phosphogypsum, 20 parts of fly ash and 6 parts of carbide slag are mixed and stirred in a mixer to obtain a mixture, and the mixture is stored for 48 hours for aging to obtain a modified phosphogypsum raw material;

[0035] S12: drying the modified phosphogypsum raw material at 180° C. until the moisture content is 8%, thereby obtaining the modified phosphogypsum dry material;

[0036] S13: grinding the modified phosphogypsum dry material into 100 mesh particles to obtain modified phosphogypsum powder;

[0037] S14: The modified phosphogypsum powder obtained in step S13, 0.2 parts of polyaluminum, 0.2 parts of calcium formate, 0.01 parts of rubber powder, 0.03 parts of cellulose ether, and 0.4 parts of composite high-efficiency water reducing agent are mixed and stirred to obtain a phosphogypsum admixture;

[0038] S15: adding 60 parts of phosphogypsum admixture, 25 parts of cement, and 45 parts of water into a stirring device and mixing for 3 minutes to obtain a modified phosphogypsum foam concrete mixed slurry;

[0039] S2: diluting 0.1 part of a plant protein foaming agent with water at a ratio of 1:30 to obtain a foaming agent dilution solution, adding the foaming agent dilution solution to a foam making device to prepare foam, and then feeding the prepared foam into a modified phosphogypsum foam concrete slurry through a foam control system for full mixing to obtain a modified phosphogypsum foam concrete pouring slurry;

[0040] S3: The prepared modified phosphogypsum foam concrete pouring slurry is poured on site or molded through a foam concrete equipment pumping system, and naturally cured to obtain a modified phosphogypsum foam concrete material. Methyl hydrogenated silicone oil is evenly applied on the surface of the modified phosphogypsum foam concrete material after natural curing.

[0041] The modified phosphogypsum foam concrete material can be a common foam concrete block or a foam concrete board.

[0042] The main components of the original phosphogypsum used in this scheme are 91.3% calcium sulfate dihydrate, 3.81% phosphorus pentoxide, 38.11% sulfur trioxide, 24.46% water, and a pH value of 2.24.

[0043] The carbide slag used is a by-product of industrial production of acetylene, wherein calcium oxide is greater than 60%, silicon oxide is greater than 3.5%, aluminum oxide is greater than 2.5%, and the water content is 20-25%.

[0044] Embodiment 2:

[0045] Different from Example 1, in a modified phosphogypsum foam concrete and a preparation method thereof, the weight proportions of raw materials used are as follows: 60 parts of original phosphogypsum, 25 parts of fly ash, 8 parts of carbide slag, 0.3 parts of polyaluminum, 0.3 parts of calcium formate, 0.01 parts of glue powder, 0.04 parts of cellulose ether, 0.5 parts of composite high-efficiency water reducing agent, 30 parts of cement, and 0.1 parts of plant protein foaming agent; and 70 parts of phosphogypsum admixture.

[0046] Embodiment 3:

[0047] Different from Example 1, in a modified phosphogypsum foam concrete and a preparation method thereof, the weight proportions of raw materials used are as follows: 70 parts of original phosphogypsum, 30 parts of fly ash, 10 parts of carbide slag, 0.5 parts of polyaluminum, 0.5 parts of calcium formate, 0.02 parts of glue powder, 0.05 parts of cellulose ether, 0.6 parts of composite high-efficiency water reducing agent, 40 parts of cement, and 0.2 parts of plant protein foaming agent; and 75 parts of phosphogypsum admixture.

[0048] Embodiment 4:

[0049] Different from Example 1, in step S11, after stirring and mixing, the mixture is ultrasonically vibrated in an ultrasonic oscillator for 20 minutes at a vibration frequency of 40 Khz, and then aged.

[0050] Comparative Example 1:

[0051] The difference from Example 3 is that the amount of carbide slag added is 11 parts.

[0052] Comparative Example 2:

[0053] The difference from Example 3 is that the amount of carbide slag added is 12 parts.

[0054] Comparative Example 3:

[0055] The difference from Example 3 is that the amount of carbide slag added is 13 parts.

[0056] Comparative Example 4:

[0057] The difference from Example 3 is that the amount of carbide slag added is 14 parts.

[0058] Comparative Example 5:

[0059] The difference from Example 3 is that the amount of carbide slag added is 15 parts.

[0060] Comparative Example 6:

[0061] The difference from Example 3 is that the amount of carbide slag added is 16 parts.

[0062] The modified phosphogypsum foamed concrete materials produced in the above embodiments and the above comparative examples, preferably concrete blocks, were tested for cube compressive strength according to the provisions of GB / T 11969. Six concrete blocks were selected for each sample for testing, and the average value of the test results was recorded as the final test value. The test values ​​are shown in Table 1:

[0063] Test Example Compressive strength(MPa) Example 1 3.5 Example 2 3.6 Example 3 3.5 Example 4 3.9 Comparative Example 1 3.4 Comparative Example 2 3.7 Comparative Example 3 3.7 Comparative Example 4 3.1 Comparative Example 5 3.3 Comparative Example 6 2.8

[0064] Table 1

[0065] From the above results, we can know that:

[0066] 1. Generally, the concrete block has a bulk density of 700 kg per cubic meter and an average compressive strength of not less than 3.5 MPa. It can be seen from the test data of Examples 1 to 3 that with the increase in the proportion of carbide slag added, the strength of the concrete block increases linearly, proving that the addition of carbide slag has a certain promoting effect on the strength improvement of the concrete block; the test data of Comparative Examples 1-5 show that when the addition amount of carbide slag continues to increase, the strength of the block shows a downward trend. According to research and analysis, the reason may be that there are too many inert precipitates, which cover the crystal nuclei and hinder the hydration of phosphogypsum, resulting in a decrease in the strength of the final concrete material.

[0067] 2. In Example 4, the mixture of phosphogypsum and carbide slag was subjected to ultrasonic oscillation without further increasing the amount of carbide slag added. The strength of the final concrete block was significantly improved compared with that in Example 1, with an improvement rate of 11.4%.

[0068] The modified phosphogypsum foam concrete material produced in the above embodiment and the above comparative example, preferably the concrete block, is subjected to leachate detection. The test method is as follows: 3 concrete blocks in each group of the above embodiment and the comparative example are respectively immersed in water for 7 days. After 7 days, the pH value of the immersion liquid is detected. The average value of each group of data is taken as the final data record. The test results are as follows:

[0069] As shown in Table 2:

[0070]

[0071]

[0072] Table 2

[0073] The results show that in Examples 1-4, the amount of carbide slag added accounts for 7%-9% of the phosphogypsum admixture, and the soaking liquid is close to neutral. When the amount of carbide slag added is greater than 9% of the phosphogypsum admixture, the pH of the soaking liquid gradually becomes alkaline, or even strongly alkaline, which proves that when the amount of carbide slag added is too large, it not only reduces the strength of the concrete blocks, but also leads to an increase in soluble alkali in the concrete material, polluting the environment.

[0074] The concrete blocks were taken out after being soaked for seven days and dried for 48 hours. The whitening of the surface of the concrete blocks was observed. The results are shown in Table 3:

[0075] Test Example Whitening Example 1 No whitening Example 2 No whitening Example 3 No whitening Example 4 No whitening Comparative Example 1 No whitening Comparative Example 2 Slightly white Comparative Example 3 Slightly white Comparative Example 4 Slightly white Comparative Example 5 Whitening Comparative Example 6 Whitening

[0076] Table 3

[0077] The results show that the concrete blocks in Examples 1-4 did not show any whitening on the surface after soaking and drying, and the surface alkali efflorescence was not serious; in Comparative Examples 1 to Comparative Examples 6, as the amount of calcium carbide slag added increased, the whitening on the surface of the concrete blocks gradually worsened, and the alkali efflorescence was serious.

[0078] From the above analysis, the samples of Examples 1-4 have good compressive strength and almost no efflorescence occurs. However, with the addition of carbide slag, the strength of the concrete blocks decreases and the efflorescence is serious. Among the above embodiments and comparative examples, Comparative Example 1 has no efflorescence phenomenon and its compressive strength is comparable to that of Example 1. However, because it adds more carbide slag and the overall performance is not significantly improved, the technical scheme of Comparative Example 1 is not adopted. From a comprehensive analysis, the amount of carbide slag used in Example 4 is relatively small, which can avoid efflorescence and pollute the environment, and has excellent compressive strength, because Example 4 is the optimal embodiment of this patent.

[0079] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A modified phosphogypsum foam concrete material, comprising the following raw materials in parts by weight: 50-70 parts of original phosphogypsum, 20-30 parts of fly ash, 6-10 parts of carbide slag, 0.2-0.5 parts of polyaluminum, 0.2-0.5 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, 0.4-0.6 parts of composite high-efficiency water reducing agent, 25-40 parts of cement, and 0.1-0.2 parts of foaming agent.

2. A modified phosphogypsum foam concrete material according to claim 1, characterized in that: The composite high-efficiency water reducer is a 1:1 mixture of a naphthalene-based high-efficiency water reducer and sodium lignin sulfonate.

3. The modified phosphogypsum foam concrete material according to claim 1, characterized in that: The foaming agent is a vegetable protein foaming agent.

4. A method for preparing a modified phosphogypsum foam concrete material, applied to any one of claims 1 to 3, characterized in that: The steps include: S1: Add 60-75 parts by weight of phosphogypsum admixture, 25-40 parts of cement, and 45-50 parts of water into a stirring device and mix for 2-3 minutes to obtain a modified phosphogypsum foam concrete mixed slurry; S2: adding a foaming agent dilution liquid to a foam making device to prepare foam, and then sending the prepared foam into a modified phosphogypsum concrete slurry through a foam control system for full mixing to obtain a modified phosphogypsum foam concrete pouring slurry; S3: The prepared modified phosphogypsum foam concrete pouring slurry is poured on site or molded through a foam concrete equipment pumping system, and naturally cured to obtain a modified phosphogypsum foam concrete material.

5. A method for preparing a modified phosphogypsum foam concrete material according to claim 4, characterized in that: In the step s1, the phosphogypsum admixture is obtained by mixing and stirring 70-99 parts of modified phosphogypsum powder, 0.2-0.5 parts of polyaluminum, 0.2-0.5 parts of calcium formate, 0.01-0.02 parts of rubber powder, 0.03-0.05 parts of cellulose ether, and 0.4-0.6 parts of composite high-efficiency water reducing agent, by weight.

6. The method for preparing a modified phosphogypsum foam concrete material according to claim 5, characterized in that: In the step s1, the preparation of modified phosphogypsum powder comprises the following steps: S11: by weight, 50-70 parts of original phosphogypsum, 20-30 parts of fly ash, and 6-10 parts of carbide slag are mixed and stirred in a mixer to obtain a mixture, and the mixture is stored for 40-50 hours for aging to obtain a modified phosphogypsum raw material; S12: drying the modified phosphogypsum raw material at 180° C. until the water content is 7%-8%, thereby obtaining the modified phosphogypsum dry material; S13: Grinding the modified phosphogypsum dry material to obtain modified phosphogypsum powder.

7. A method for preparing a modified phosphogypsum foam concrete material according to claim 6, characterized in that: In the step S3, methyl hydrogen silicone oil is evenly applied on the surface of the modified phosphogypsum foam concrete material after natural curing.

8. The method for preparing a modified phosphogypsum foam concrete material according to claim 7, characterized in that: The foaming agent diluent is obtained by diluting 0.1-0.2 parts of the foaming agent with water at a ratio of 1:

30. The foaming agent is pure plant protein type, has a solid content of 18%, and a foaming multiple of 30.

9. A method for preparing a modified phosphogypsum foam concrete material according to claim 8, characterized in that: In step S13, the modified phosphogypsum dry material is crushed into 40-200 mesh particles.

10. A method for preparing a modified phosphogypsum foam concrete material according to claim 9, characterized in that: In the step S11, the mixture is further subjected to ultrasonic vibration for 20 minutes and then aged.