Lightweight building external wall thermal insulation composite material and preparation method and application thereof
Through nano-inorganic fiber aerogel and three-dimensional woven basalt fiber mesh composite, the existing lightweight flame-retardant building insulation boards have solved the shortcomings in fire resistance and energy-saving effects, and achieved low density, high heat insulation and high flame-retardant The building insulation material is suitable for building exterior walls and interior insulation systems.
Patent Information
- Application Number
- CN202410805320.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-22
Smart Images

Figure CN118993692A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to a lightweight building exterior wall thermal insulation composite material and a preparation method and application thereof. Background Art
[0002] Generally, lightweight flame-retardant building insulation boards are an important insulation material in the construction field. They have the advantages of flame retardancy, lightness, durability, etc., and are widely used in building insulation systems. With the improvement of fire safety standards and people's attention to building safety, especially in public buildings, commercial buildings and other places with strict requirements on fire resistance, the demand for lightweight flame-retardant building insulation boards continues to increase. At present, research on lightweight flame-retardant building insulation boards mainly focuses on material modification, performance optimization and construction technology to meet the needs of building environmental protection, energy saving and safety. The present invention aims to provide a high-performance lightweight building insulation composite material to meet the requirements of modern buildings for safety, energy saving and environmental protection. Summary of the invention
[0003] The technical task of the present invention is to solve the deficiencies of the prior art and provide a lightweight building exterior wall thermal insulation composite material and a preparation method and use thereof.
[0004] The technical solution of the present invention is implemented in the following manner: a lightweight building exterior wall thermal insulation composite material of the present invention, wherein the composite material is obtained by:
[0005] First, prepare a stable silica sol-organic composite precursor solution.
[0006] The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the nanofibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane;
[0007] The organic silicon hybrid nanofiber membrane is dried to remove moisture, and calcined at high temperature to remove organic components in the fiber to obtain an inorganic silicon nanofiber membrane;
[0008] The inorganic silicon nanofiber membrane is cut into pieces, soaked in deionized water, and dispersed by a high-speed homogenizer to obtain a homogeneous micro-nano fiber dispersion;
[0009] transferring the homogenized micro-nanofiber dispersion into the pre-prepared mold;
[0010] Then, the three-dimensional woven basalt fiber grid is immersed in the dispersion in the mold;
[0011] Next, the mold containing the three-dimensional woven basalt fiber grid and the dispersion was placed in a foam box;
[0012] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0013] Finally, the frozen blocks were transferred to a freeze dryer for vacuum freeze drying to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0014] The steps for obtaining the composite material are:
[0015] Step (1) Preparation of precursor solution:
[0016] First, H3PO4 phosphoric acid solution was quickly added drop by drop into a mixed solution of H2O water and TEOS tetraethyl silicate;
[0017] The molar ratio of H3PO4, H2O and TEOS in the mixed solution is 0.01:1:10;
[0018] and stirring for 4 to 8 hours to obtain silica sol;
[0019] Meanwhile, the PVA polyvinyl alcohol powder was dissolved in deionized water at 80° C. by stirring for 5 h to form a PVA polyvinyl alcohol solution with a mass concentration of 10 wt %;
[0020] Subsequently, the silica sol and the PVA polyvinyl alcohol solution of the same mass are mixed, and stirred for 4 to 8 hours to obtain a stable precursor solution;
[0021] Step (2) Inorganic silicon nanofiber membrane:
[0022] The inorganic silicon nanofiber membrane is composed of SiO2 silicon oxide nanofibers, which are prepared by combining the sol-gel method and electrospinning technology, as follows:
[0023] The precursor solution prepared in step (1) is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the fibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane;
[0024] Among them, the spinning voltage was set to 15-20 kV, the perfusion speed was set to 0.5-1.5 mL / h, the spinning distance was set to 15-20 cm, and the drum speed was set to 100 rpm;
[0025] The spinning environment temperature and humidity were 25 ± 2 °C and 45 ± 5%, respectively;
[0026] Subsequently, the prepared PVA / SiO2 nanofiber membrane with organosilicon hybrid was dried in a vacuum oven at 80°C for 2 h to remove moisture, and then placed in a programmed temperature muffle furnace for high-temperature calcination to remove the organic components in the fiber to obtain a SiO2 nanofiber membrane. The heating rate was 5°C / min and the calcination temperature was 600-800°C.
[0027] Finally, an inorganic silicon nanofiber membrane is obtained;
[0028] Step (3) Preparation of inorganic fiber aerogel precursor slurry:
[0029] First, 0.5-1.5 g of electrospun SiO2 nanofiber membrane was weighed, cut into pieces, and immersed in 200 g of deionized water;
[0030] Then, a high-speed homogenizer was used to disperse for 20 minutes to obtain a homogeneous micro-nano fiber dispersion; that is, an inorganic fiber aerogel precursor slurry;
[0031] Step (4) is as follows:
[0032] Transferring the inorganic fiber aerogel precursor slurry prepared in step (3) into a pre-prepared mold;
[0033] Then, the three-dimensional woven basalt fiber grid was immersed in the dispersion;
[0034] Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box;
[0035] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0036] Finally, the frozen block was transferred to a freeze dryer and vacuum freeze-dried for 12 to 18 hours to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0037] The characteristic parameters of the thermal insulation composite material are:
[0038] Thermal conductivity is 0.020W / m·K~0.030W / m·K;
[0039] Bulk density is 10kg / m 3 ~50kg / m 3 ;
[0040] Porosity is 85% to 95%;
[0041] It does not burn at 800-1000℃;
[0042] It has excellent thermal insulation performance and can reach A1 fire protection grade.
[0043] The three-dimensional woven basalt fiber grid is a basalt fiber grid that is woven in three-dimensional directions: horizontal, longitudinal, and vertical.
[0044] The composite material is composed of nano inorganic fiber aerogel and three-dimensional woven basalt fiber grid.
[0045] A method for preparing a lightweight building exterior wall thermal insulation composite material, the preparation method comprising:
[0046] First, prepare a stable silica sol-organic composite precursor solution.
[0047] The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the nanofibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane;
[0048] The organic silicon hybrid nanofiber membrane is dried to remove moisture, and calcined at high temperature to remove organic components in the fiber to obtain an inorganic silicon nanofiber membrane;
[0049] The inorganic silicon nanofiber membrane is cut into pieces, soaked in deionized water, and dispersed by a high-speed homogenizer to obtain a homogeneous micro-nano fiber dispersion;
[0050] transferring the homogenized micro-nanofiber dispersion into the pre-prepared mold;
[0051] Then, the three-dimensional woven basalt fiber grid is immersed in the dispersion in the mold;
[0052] Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box;
[0053] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0054] Finally, the frozen blocks were transferred to a freeze dryer for vacuum freeze drying to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0055] The precursor solution is prepared as follows:
[0056] First, H3PO4 phosphoric acid solution was quickly added drop by drop into a mixed solution of H2O water and TEOS tetraethyl silicate;
[0057] The molar ratio of H3PO4, H2O and TEOS in the mixed solution is 0.01:1:10;
[0058] and stirring for 4 to 8 hours to obtain silica sol;
[0059] Meanwhile, the PVA polyvinyl alcohol powder was dissolved in deionized water at 80° C. by stirring for 5 h to form a PVA polyvinyl alcohol solution with a mass concentration of 10 wt %;
[0060] Subsequently, the silica sol and the PVA polyvinyl alcohol solution of the same mass are mixed and stirred for 4 to 8 hours to obtain a stable precursor solution.
[0061] The inorganic silicon nanofiber membrane is composed of SiO2 silicon oxide nanofibers, which are prepared by combining the sol-gel method and electrospinning technology, as follows:
[0062] The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of an electric field force, and the fibers are continuously accumulated to form a nanofiber membrane;
[0063] Among them, the spinning voltage was set to 15-20 kV, the perfusion speed was set to 0.5-1.5 mL / h, the spinning distance was set to 15-20 cm, and the drum speed was set to 100 rpm;
[0064] The spinning environment temperature and humidity were 25 ± 2 °C and 45 ± 5%, respectively;
[0065] Subsequently, the prepared PVA / SiO2 organosilicon hybrid nanofiber membrane was dried in a vacuum oven at 80°C for 2 h to remove moisture, and then placed in a programmed temperature muffle furnace for high-temperature calcination to remove the organic components in the fiber to obtain a SiO2 nanofiber membrane. The heating rate was 5°C / min and the calcination temperature was 600-800°C.
[0066] Finally, an inorganic silicon nanofiber membrane is obtained.
[0067] The preparation of inorganic fiber aerogel precursor slurry is as follows:
[0068] First, 0.5-1.5 g of electrospun SiO2 nanofiber membrane was weighed, cut into pieces, and immersed in 200 g of deionized water;
[0069] Then, a high-speed homogenizer was used to disperse for 20 minutes to obtain a homogeneous micro-nano fiber dispersion; that is, an inorganic fiber aerogel precursor slurry;
[0070] transferring the prepared inorganic fiber aerogel precursor slurry into a pre-prepared mold;
[0071] Then, the three-dimensional woven basalt fiber grid was immersed in the dispersion;
[0072] Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box;
[0073] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0074] Finally, the frozen block was transferred to a freeze dryer and vacuum freeze-dried for 12 to 18 hours to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0075] The lightweight building exterior wall thermal insulation composite material is used in building exterior wall external thermal insulation and internal thermal insulation system products.
[0076] Compared with the prior art, the present invention has the following beneficial effects:
[0077] The invention discloses a lightweight building exterior wall thermal insulation composite material, a preparation method and use thereof. The material is composited from nano inorganic fiber aerogel and three-dimensional woven basalt fiber grids and can be used for exterior thermal insulation and interior thermal insulation systems of building exterior walls.
[0078] This material has the characteristics of low bulk density, good flame retardancy and excellent thermal insulation effect. It is suitable for external insulation and internal insulation systems of building exterior walls. It is easy to industrialize and has stable product performance, making it suitable for large-scale promotion and application.
[0079] The material can be used for external insulation of building exterior walls and internal insulation systems. The material is obtained through a special preparation process and has the advantages of low bulk density, high flame retardant grade, good insulation effect, and convenient construction.
[0080] The material is prepared by combining sol-gel technology, electrostatic spinning technology, high-temperature calcination technology and freeze-drying technology.
[0081] The lightweight building exterior wall thermal insulation composite material and the preparation method and use thereof of the present invention have reasonable design, simple material preparation, safe and reliable performance, convenient use and easy maintenance, and have good promotion and use value. BRIEF DESCRIPTION OF THE DRAWINGS
[0082] Attached Figure 1 It is a schematic diagram of the structure of the three-dimensional woven basalt fiber grid of the present invention;
[0083] Attached Figure 2 It is a structural schematic diagram of a lightweight building exterior wall thermal insulation composite material of the present invention, namely, a nano inorganic fiber aerogel and a three-dimensional woven basalt fiber grid composite material.
[0084] The symbols in the accompanying drawings represent:
[0085] 1. Nano inorganic fiber aerogel, 2. Three-dimensional woven basalt fiber grid. DETAILED DESCRIPTION
[0086] The following is a detailed description of a lightweight building exterior wall thermal insulation composite material, a preparation method and uses thereof of the present invention in conjunction with the accompanying drawings.
[0087] As shown in the accompanying drawings, a lightweight building exterior wall thermal insulation composite material and a preparation method and use thereof of the present invention, wherein the preparation method comprises:
[0088] First, prepare a stable silica sol-organic composite precursor solution.
[0089] The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the nanofibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane;
[0090] The organic silicon hybrid nanofiber membrane is dried to remove moisture, and calcined at high temperature to remove organic components in the fiber to obtain an inorganic silicon nanofiber membrane;
[0091] The inorganic silicon nanofiber membrane is cut into pieces, soaked in deionized water, and dispersed by a high-speed homogenizer to obtain a homogeneous micro-nano fiber dispersion;
[0092] transferring the homogenized micro-nanofiber dispersion into the pre-prepared mold;
[0093] Then, the three-dimensional woven basalt fiber grid is immersed in the dispersion in the mold;
[0094] Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box;
[0095] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0096] Finally, the frozen blocks were transferred to a freeze dryer for vacuum freeze drying to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0097] The precursor solution is prepared as follows:
[0098] First, H3PO4 phosphoric acid solution was quickly added drop by drop into a mixed solution of H2O water and TEOS tetraethyl silicate;
[0099] The molar ratio of H3PO4, H2O and TEOS in the mixed solution is 0.01:1:10;
[0100] and stirring for 4 to 8 hours to obtain silica sol;
[0101] Meanwhile, the PVA polyvinyl alcohol powder was dissolved in deionized water at 80° C. by stirring for 5 h to form a PVA polyvinyl alcohol solution with a mass concentration of 10 wt %;
[0102] Subsequently, the silica sol and the PVA polyvinyl alcohol solution of the same mass are mixed and stirred for 4 to 8 hours to obtain a stable precursor solution.
[0103] The inorganic silicon nanofiber membrane is composed of SiO2 silicon oxide nanofibers, which are prepared by combining the sol-gel method and electrospinning technology, as follows:
[0104] The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of an electric field force, and the fibers are continuously accumulated to form a nanofiber membrane;
[0105] Among them, the spinning voltage was set to 15-20 kV, the perfusion speed was set to 0.5-1.5 mL / h, the spinning distance was set to 15-20 cm, and the drum speed was set to 100 rpm;
[0106] The spinning environment temperature and humidity were 25 ± 2 °C and 45 ± 5%, respectively;
[0107] Subsequently, the prepared PVA / SiO2 organosilicon hybrid nanofiber membrane was dried in a vacuum oven at 80°C for 2 h to remove moisture, and then placed in a programmed temperature muffle furnace for high-temperature calcination to remove the organic components in the fiber to obtain a SiO2 nanofiber membrane. The heating rate was 5°C / min and the calcination temperature was 600-800°C.
[0108] Finally, an inorganic silicon nanofiber membrane is obtained.
[0109] The preparation of inorganic fiber aerogel precursor slurry is as follows:
[0110] First, 0.5-1.5 g of electrospun SiO2 nanofiber membrane was weighed, cut into pieces, and immersed in 200 g of deionized water;
[0111] Then, a high-speed homogenizer was used to disperse for 20 minutes to obtain a homogeneous micro-nano fiber dispersion; that is, an inorganic fiber aerogel precursor slurry;
[0112] transferring the prepared inorganic fiber aerogel precursor slurry into a pre-prepared mold;
[0113] Then, the three-dimensional woven basalt fiber grid was immersed in the dispersion;
[0114] Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box;
[0115] Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block;
[0116] Finally, the frozen block was transferred to a freeze dryer and vacuum freeze-dried for 12 to 18 hours to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
[0117] The thickness of the three-dimensional woven basalt fiber mesh ranges from 0.5 to 10 cm.
[0118] The characteristic parameters of the thermal insulation composite material obtained by the present invention are:
[0119] Thermal conductivity is 0.020W / m·K~0.030W / m·K;
[0120] Bulk density is 10kg / m 3 ~50kg / m 3 ;
[0121] Porosity is 85% to 95%;
[0122] It does not burn at 800-1000℃;
[0123] It has excellent thermal insulation performance and can reach A1 fire protection grade.
Claims
1. A lightweight building exterior wall thermal insulation composite material, Features The composite material is obtained by: First, prepare a stable silica sol-organic composite precursor solution. The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the nanofibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane; The organic silicon hybrid nanofiber membrane is dried to remove moisture, and calcined at high temperature to remove organic components in the fiber to obtain an inorganic silicon nanofiber membrane; The inorganic silicon nanofiber membrane is cut into pieces, soaked in deionized water, and dispersed by a high-speed homogenizer to obtain a homogeneous micro-nano fiber dispersion; transferring the homogenized micro-nanofiber dispersion into the pre-prepared mold; Then, the three-dimensional woven basalt fiber grid is immersed in the dispersion in the mold; Next, the mold containing the three-dimensional woven basalt fiber grid and the dispersion was placed in a foam box; Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block; Finally, the frozen blocks were transferred to a freeze dryer for vacuum freeze drying to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
2. A lightweight building exterior wall thermal insulation composite material according to claim 1, Features The steps for obtaining the composite material are: Step (1) Preparation of precursor solution: First, H 3 PO 4 Phosphoric acid solution was added drop by drop quickly into H 2 O in a mixed solution of water and TEOS tetraethyl silicate; H in the mixed solution 3 PO 4 , H 2 The molar ratio of O and TEOS is 0.01:1:10; and stirring for 4 to 8 hours to obtain silica sol; Meanwhile, the PVA polyvinyl alcohol powder was dissolved in deionized water at 80° C. by stirring for 5 h to form a PVA polyvinyl alcohol solution with a mass concentration of 10 wt %; Subsequently, the silica sol and the PVA polyvinyl alcohol solution of the same mass are mixed, and stirred for 4 to 8 hours to obtain a stable precursor solution; Step (2) Inorganic silicon nanofiber membrane: The inorganic silicon nanofiber membrane is composed of SiO 2 Silica nanofibers are prepared by combining sol-gel method and electrospinning technology, as follows: The precursor solution prepared in step (1) is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the fibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane; Among them, the spinning voltage was set to 15-20 kV, the perfusion speed was set to 0.5-1.5 mL / h, the spinning distance was set to 15-20 cm, and the drum speed was set to 100 rpm; The spinning environment temperature and humidity were 25 ± 2 °C and 45 ± 5%, respectively; Then, the prepared PVA / SiO 2 The organosilicon hybrid nanofiber membrane was dried in a vacuum oven at 80 °C for 2 h to remove moisture, and then placed in a programmed temperature muffle furnace for high-temperature calcination to remove the organic components in the fiber and obtain SiO 2 Nanofiber membrane, heating rate is 5℃ / min, calcination temperature is 600~800℃; Finally, an inorganic silicon nanofiber membrane is obtained; Step (3) Preparation of inorganic fiber aerogel precursor slurry: First, weigh 0.5-1.5 g of electrospun SiO 2 Nanofiber membranes were cut into pieces and immersed in 200 g of deionized water; Then, a high-speed homogenizer was used to disperse for 20 minutes to obtain a homogeneous micro-nano fiber dispersion; that is, an inorganic fiber aerogel precursor slurry; Step (4) is as follows: Transferring the inorganic fiber aerogel precursor slurry prepared in step (3) into a pre-prepared mold; Then, the three-dimensional woven basalt fiber grid was immersed in the dispersion; Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box; Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block; Finally, the frozen block was transferred to a freeze dryer and vacuum freeze-dried for 12 to 18 hours to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
3. A lightweight building exterior wall thermal insulation composite material according to claim 1, Features: The characteristic parameters of the thermal insulation composite material are: Thermal conductivity is 0.020W / m·K~0.030W / m·K; Bulk density is 10kg / m 3 ~50kg / m 3 ; Porosity is 85% to 95%; It does not burn at 800-1000℃; It has excellent thermal insulation performance and can reach A1 fire protection grade.
4. A lightweight building exterior wall thermal insulation composite material according to claim 1, Features: The three-dimensional woven basalt fiber grid is a basalt fiber grid that is woven in three-dimensional directions: horizontal, longitudinal, and vertical.
5. A lightweight building exterior wall thermal insulation composite material according to claim 1, Features: The composite material is composed of nano inorganic fiber aerogel and three-dimensional woven basalt fiber grid.
6. A method for preparing a lightweight building exterior wall thermal insulation composite material, Features: The preparation method comprises: First, prepare a stable silica sol-organic composite precursor solution. The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of the electric field force, and the nanofibers are continuously accumulated to form an organosilicon hybrid nanofiber membrane; The organic silicon hybrid nanofiber membrane is dried to remove moisture, and calcined at high temperature to remove organic components in the fiber to obtain an inorganic silicon nanofiber membrane; The inorganic silicon nanofiber membrane is cut into pieces, soaked in deionized water, and dispersed by a high-speed homogenizer to obtain a homogeneous micro-nano fiber dispersion; transferring the homogenized micro-nanofiber dispersion into the pre-prepared mold; Then, the three-dimensional woven basalt fiber grid is immersed in the dispersion in the mold; Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box; Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block; Finally, the frozen blocks were transferred to a freeze dryer for vacuum freeze drying to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
7. A method for preparing a lightweight building exterior wall thermal insulation composite material according to claim 6, Features: The precursor solution is prepared as follows: First, H 3 PO 4 Phosphoric acid solution was added drop by drop quickly into H 2 O in a mixed solution of water and TEOS tetraethyl silicate; H in the mixed solution 3 PO 4 , H 2 The molar ratio of O and TEOS is 0.01:1:10; and stirring for 4 to 8 hours to obtain silica sol; Meanwhile, the PVA polyvinyl alcohol powder was dissolved in deionized water at 80° C. by stirring for 5 h to form a PVA polyvinyl alcohol solution with a mass concentration of 10 wt %; Subsequently, the silica sol and the PVA polyvinyl alcohol solution of the same mass are mixed and stirred for 4 to 8 hours to obtain a stable precursor solution.
8. A method for preparing a lightweight building exterior wall thermal insulation composite material according to claim 6, Features: The inorganic silicon nanofiber membrane is composed of SiO 2 Silica nanofibers are prepared by combining sol-gel method and electrospinning technology, as follows: The precursor solution is transferred to an electrospinning machine, and the droplets are stretched into nanofibers under the action of an electric field force, and the fibers are continuously accumulated to form a nanofiber membrane; Among them, the spinning voltage was set to 15-20 kV, the perfusion speed was set to 0.5-1.5 mL / h, the spinning distance was set to 15-20 cm, and the drum speed was set to 100 rpm; The spinning environment temperature and humidity were 25 ± 2 °C and 45 ± 5%, respectively; Then, the prepared PVA / SiO 2 The organosilicon hybrid nanofiber membrane was dried in a vacuum oven at 80 °C for 2 h to remove moisture, and then placed in a programmed temperature muffle furnace for high-temperature calcination to remove the organic components in the fiber and obtain SiO 2 Nanofiber membrane, heating rate is 5℃ / min, calcination temperature is 600~800℃; Finally, an inorganic silicon nanofiber membrane is obtained.
9. A method for preparing a lightweight building exterior wall thermal insulation composite material according to claim 6, Features: The preparation of inorganic fiber aerogel precursor slurry is as follows: First, weigh 0.5-1.5 g of electrospun SiO 2 Nanofiber membranes were cut into pieces and immersed in 200 g of deionized water; Then, a high-speed homogenizer was used to disperse for 20 minutes to obtain a homogeneous micro-nano fiber dispersion; that is, an inorganic fiber aerogel precursor slurry; transferring the prepared inorganic fiber aerogel precursor slurry into a pre-prepared mold; Then, the three-dimensional woven basalt fiber grid was immersed in the dispersion; Next, the mold containing the three-dimensional woven fiber grid and the dispersion is placed in a foam box; Subsequently, liquid nitrogen was poured into the foam box, and the liquid nitrogen flow rate was controlled so that it just covered the bottom of the mold to obtain a directional frozen block; Finally, the frozen block was transferred to a freeze dryer and vacuum freeze-dried for 12 to 18 hours to obtain a three-dimensional fluffy inorganic fiber aerogel / three-dimensional woven basalt fiber grid thermal insulation composite material.
10. Use of the lightweight building exterior wall thermal insulation composite material as claimed in claim 1 in building exterior wall external thermal insulation and internal thermal insulation system products.