Ceramic material with photoluminescence and energy storage performance
By synthesizing mesoporous silicone and alkaline earth aluminate composite materials and depositing bismuth oxide layers, the performance degradation of existing ceramic materials in long-term ultraviolet light irradiation or humid environments is solved, and higher photoluminescence intensity and stability are achieved improves the overall performance of the material.
Patent Information
- Application Number
- CN202411002465.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing luminescent ceramic materials are prone to glaze decomposition, decreased brightness, poor high temperature resistance and prone to cracking under long-term ultraviolet light exposure or humid environments, resulting in low luminous brightness, short afterglow time and poor material quality.
By synthesizing mesoporous silicone materials and alkaline earth aluminate to form a composite material, and depositing bismuth oxide layer on its surface to form a photoluminescent and energy storage ceramic material, avoiding poor bonding between the glaze and the blank and enhances the photoluminescence effect.
Improve the photoluminescence intensity and stability of the material, extend the luminescence time, enhance the optical and electrical effects, improve the binding strength with alkaline earth aluminate and bismuth oxide, and improve the high-temperature oxidation resistance and capacity expansion of the material. .
Smart Images

Figure BDA0004961981800000071 
Figure BDA0004961981800000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of physical materials, and in particular relates to a ceramic material with photoluminescence and energy storage properties. Background Art
[0002] The application of ceramic materials at this stage has far exceeded the scope of handicrafts, and is increasingly used in the fields of automobiles, aircraft, etc. It is widely used due to its fireproof and heat-insulating protective properties, light weight, high melting temperature, high tensile strength and chemical inertness.
[0003] Luminescent ceramic material is a high-purity cutting-edge material made by subjecting light-storing materials to high temperature and high pressure. It can absorb sunlight or other scattered light, store light and then activate to emit strong light. It has good applications in the design of nighttime lighting and various decorations of buildings in areas with power shortages, such as luminous plaster ceilings, hanging sheds, neon decorations, decorative paintings, luminous tiles, etc.
[0004] The conventional method of preparing luminescent ceramics is to apply a layer of glaze on the surface. Under normal conditions, the performance of the glaze is stable and the luminescence is stable. However, under long-term ultraviolet light or in a humid environment for a long time, the surface glaze layer will decompose, causing the surface to become black and the brightness to decrease. Glazes made of different materials will have low luminous brightness, short afterglow time, reduced high temperature resistance, poor glaze quality, easy cracking, poor water resistance and other reasons. Summary of the invention
[0005] The purpose of the present invention is to provide a ceramic material with photoluminescence and energy storage properties. The photoluminescence and energy storage ceramic material is obtained by synthesizing a mesoporous organosilicon material and preparing a composite material with alkaline earth aluminate, and then depositing a layer of bismuth oxide on the composite material.
[0006] The technical problem to be solved by the present invention is as follows: The present invention changes the conventional idea of preparing luminescent ceramics, and integrates ceramics and luminescent materials into a whole, thereby avoiding the poor bonding between the glaze or coating and the body, the easy generation of defects such as glaze cracks, and the low luminous brightness. In addition, by modifying the ceramic material, the energy storage limit is increased, the luminous time is extended, and the photoluminescence effect of the material is increased by depositing a bismuth layer, thereby enhancing the light intensity.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A ceramic material with photoluminescence and energy storage properties, the preparation method comprising the following steps:
[0009] A1. Disperse 1 g of chitosan in 25 mL of 1.5% acetic acid solution, stir evenly, add 2-3 g of vinyltriethoxysilane, and stir continuously at room temperature overnight to obtain a silicon-based solution;
[0010] A2, a suspension containing 120 mL of liquid paraffin and 5.5 g of sorbitan trioleate was dispersed in a reactor and stirred for 30 minutes, then the silicon-based solution was added and stirred at 1400 rpm for 60 minutes, and then 3 g of polyoxyethylene sorbitan trioleate was added thereto and stirred for another 60 minutes;
[0011] A3. A solution containing 3 mL of 28% ammonia and 7 mL of isopropanol was added dropwise to the reactor and stirred for 1 hour. After vacuum filtration and washing with petroleum ether, ethanol and deionized water, the sample was freeze-dried at -60°C for 24 hours and then carbonized in an Ar / H2 atmosphere for 3 hours to obtain a mesoporous organosilicon material.
[0012] Further, the contents of Ar / H2 atmosphere are 95% and 5%, respectively.
[0013] Furthermore, the carbonization temperature is 1000°C.
[0014] Furthermore, the specific operation of preparing the composite material from the organic silicon material and the alkaline earth aluminate is as follows:
[0015] B1, dissolving alkaline earth aluminate raw material in deionized water, adding nitric acid solution and urea, and then heating the mixture for 5-10 minutes;
[0016] B2, transferring the heated mixture into a ceramic crucible, and dehydrating and decomposing at 500-900° C. for 3-5 minutes to obtain a fluffy alkaline earth aluminate product;
[0017] In the above reaction process, the redox combustion reaction of metal nitrate and organic reducing agent in their aqueous solution at a moderately low ambient temperature is used, with nitrate as the oxidant and urea as the reducing agent. The raw materials are dissolved in the aqueous solution to form a uniform solution. After heating and dehydration, the solution can be burned to complete the reaction. The ignition temperature of the combustion reaction will drop to 500°C, producing a fluffy and porous product.
[0018] B3. After fully grinding the alkaline earth aluminate product, add the mesoporous organosilicon material at a mixing ratio of 1:1 to obtain an alkaline earth aluminate / organosilicon composite material.
[0019] Furthermore, the alkaline earth aluminate raw materials include Sr(NO3)2, Al(NO3)3˙9H2O, Eu2O3, and Dy2O3.
[0020] Furthermore, the molar ratio of the raw materials Sr(NO3)2, Al(NO3)3˙9H2O, Eu2O3, and Dy2O3 is: 0.5-1:1:0.01:0.02.
[0021] Further, the specific operation of depositing bismuth on the alkaline earth aluminate / organosilicon composite material is:
[0022] Add Bi(NO3)3˙5H2O to the alkaline earth aluminate / organosilicon composite material, stir evenly, and then heat at 400°C for 10-20 minutes. After evaporating H2O and HNO3 substances, the alkaline earth aluminate / organosilicon composite material with a deposited Bi film is obtained, which is a ceramic material with photoluminescence and energy storage properties.
[0023] Beneficial effects of the present invention:
[0024] (1) In the technical solution of the present invention, mesoporous organosilicon is used as the raw material. In addition to high porosity, excellent high-temperature oxidation resistance, mechanical properties, etc., it also has good optical and electrical effects. Compared with other porous silicons, it has higher stability and capacity expansion, and increases the bonding strength with alkaline earth aluminate and bismuth oxide.
[0025] (2) In the technical solution of the present invention, a bismuth layer is used to wrap the organosilicon / alkaline earth aluminate composite material. During the deposition of the bismuth layer, the mesoporous organosilicon is passivated, and new combinations of Bi-O-Si and Bi-O occur. The saturation of dangling bonds and the metallic behavior of the bismuth oxide ultra-thin film caused by the free charge promote the absorption of light by the composite material.
[0026] (3) In the technical solution of the present invention, alkaline earth aluminate is used as the raw material of the ceramic material, and is combined with mesoporous silicone, which increases the material's absorption spectrum and the material's luminescence duration. Alkaline earth aluminate can absorb and store visible light, black light and lamplight, and silicone combined with a bismuth layer can absorb ultraviolet light and infrared light, and both materials have the ability to emit light to enhance the luminescence brightness. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] Disperse 1 g of chitosan in 25 mL of 1.5% acetic acid solution, stir evenly, add 2 g of vinyltriethoxysilane, and continue stirring at room temperature overnight to obtain a silicon-based solution;
[0030] Subsequently, a suspension containing 120 mL of liquid paraffin and 5.5 g of sorbitan trioleate was dispersed in a reactor and stirred for 30 minutes, and then the silicon-based solution was added to the reactor and stirred at 1400 rpm for 60 minutes, and then 3 g of polyoxyethylene sorbitan trioleate was added thereto and stirred for another 60 minutes;
[0031] Then, a solution containing 3 mL of 28% ammonia and 7 mL of isopropanol was added dropwise to the reactor and stirred for 1 hour. After vacuum filtration and washing with petroleum ether, ethanol and deionized water, the sample was freeze-dried at -60°C for 24 hours and then carbonized in an Ar / H2 atmosphere for 3 hours to obtain a mesoporous organosilicon material. The contents of the Ar / H2 atmosphere were 95% and 5% respectively, and the carbonization temperature was 1000°C to obtain mesoporous organosilicon.
[0032] Example 2
[0033] Disperse 1 g of chitosan in 25 mL of 1.5% acetic acid solution, stir evenly, add 2.5 g of vinyltriethoxysilane, and continue stirring at room temperature overnight to obtain a silicon-based solution;
[0034] Subsequently, a suspension containing 120 mL of liquid paraffin and 5.5 g of sorbitan trioleate was dispersed in a reactor and stirred for 30 minutes, and then the silicon-based solution was added to the reactor and stirred at 1400 rpm for 60 minutes, and then 3 g of polyoxyethylene sorbitan trioleate was added thereto and stirred for another 60 minutes;
[0035] Then, a solution containing 3 mL of 28% ammonia and 7 mL of isopropanol was added dropwise to the reactor and stirred for 1 hour. After vacuum filtration and washing with petroleum ether, ethanol and deionized water, the sample was freeze-dried at -60°C for 24 hours and then carbonized in an Ar / H2 atmosphere for 3 hours to obtain a mesoporous organosilicon material. The contents of the Ar / H2 atmosphere were 95% and 5% respectively, and the carbonization temperature was 1000°C to obtain mesoporous organosilicon.
[0036] Example 3
[0037] Disperse 1 g of chitosan in 25 mL of 1.5% acetic acid solution, stir evenly, add 3 g of vinyltriethoxysilane, and continue stirring at room temperature overnight to obtain a silicon-based solution;
[0038] Subsequently, a suspension containing 120 mL of liquid paraffin and 5.5 g of sorbitan trioleate was dispersed in a reactor and stirred for 30 minutes, and then the silicon-based solution was added to the reactor and stirred at 1400 rpm for 60 minutes, and then 3 g of polyoxyethylene sorbitan trioleate was added thereto and stirred for another 60 minutes;
[0039] Then, a solution containing 3 mL of 28% ammonia and 7 mL of isopropanol was added dropwise to the reactor and stirred for 1 hour. After vacuum filtration and washing with petroleum ether, ethanol and deionized water, the sample was freeze-dried at -60°C for 24 hours and then carbonized in an Ar / H2 atmosphere for 3 hours to obtain a mesoporous organosilicon material. The contents of the Ar / H2 atmosphere were 95% and 5% respectively, and the carbonization temperature was 1000°C to obtain mesoporous organosilicon.
[0040] Example 4
[0041] Alkaline earth aluminate raw materials, including 3.27 g Sr(NO3)2, 6.53 g Al(NO3)3˙9H2O, 0.065 g Eu2O3, and 0.13 g Dy2O3, were dissolved in deionized water, 1.0 g nitric acid solution and 2.0 g urea were added, and the mixture was then heated for 5-10 minutes;
[0042] The heated mixture is then transferred to a ceramic crucible and dehydrated at 700°C for 3-5 minutes to obtain a fluffy alkaline earth aluminate product;
[0043] Subsequently, the alkaline earth aluminate product was fully ground, and then the mesoporous organosilicon material prepared in Example 1 was added at a mixing ratio of 1:1 to obtain an alkaline earth aluminate / organosilicon composite material.
[0044] Example 5
[0045] Alkaline earth aluminate raw materials, including 4.05 g Sr(NO3)2, 5.78 g Al(NO3)3˙9H2O, 0.057 g Eu2O3, and 0.115 g Dy2O3, were dissolved in deionized water, 1.2 g nitric acid solution and 2 g urea were added, and the mixture was then heated for 5-10 minutes;
[0046] The heated mixture is then transferred to a ceramic crucible and dehydrated at 700°C for 3-5 minutes to obtain a fluffy alkaline earth aluminate product;
[0047] Subsequently, the alkaline earth aluminate product was fully ground, and then the mesoporous organosilicon material prepared in Example 2 was added at a mixing ratio of 1:1 to obtain an alkaline earth aluminate / organosilicon composite material.
[0048] Example 6
[0049] Alkaline earth aluminate raw materials, including 4.93 g Sr(NO3)2, 4.93 g Al(NO3)3˙9H2O, 0.049 g Eu2O3, and 0.098 g Dy2O3, were dissolved in deionized water, 1.5 g nitric acid solution and 2 g urea were added, and the mixture was then heated for 5-10 minutes;
[0050] The heated mixture is then transferred to a ceramic crucible and dehydrated at 700°C for 3-5 minutes to obtain a fluffy alkaline earth aluminate product;
[0051] Subsequently, the alkaline earth aluminate product was fully ground, and then the mesoporous organosilicon material prepared in Example 3 was added at a mixing ratio of 1:1 to obtain an alkaline earth aluminate / organosilicon composite material.
[0052] Now the alkaline earth aluminate / organic silicon composite materials prepared in Examples 4-6 were tested for photoluminescence effect. Using the F-4500 instrument, a quartz glass sheet was laid flat in the middle of the tablet pressing mold. After the sample was ground, it was evenly dispersed on the glass sheet. The knob was covered on the groove, and the emission spectrum and laser spectrum were scanned. Each sample was tested 3 times, and the emission spectrum and the excitation spectrum were superimposed. The highest peak intensity of the photoluminescence was recorded, and the average value was recorded. The test results are shown in Table 1:
[0053] Table 1: Photoluminescence effect test of alkaline earth aluminate / organic silicon composite materials prepared in Examples 4-6
[0054]
[0055]
[0056] From the test results in Table 1, the highest peak intensity value of Example 6>Example 5>Example 4 indicates that Example 6 generates the most photons after the recombination of photogenerated electrons and holes, and the intensity of photoluminescence is the strongest.
[0057] Example 7
[0058] Bi(NO3)3˙5H2O was added to the alkaline earth aluminate / organosilicon composite material prepared in Example 4, stirred evenly, and then heated at 400°C for 10-20 minutes to obtain an alkaline earth aluminate / organosilicon composite material with a deposited Bi film, thereby obtaining a ceramic material with photoluminescence and energy storage properties.
[0059] Example 8
[0060] Bi(NO3)3˙5H2O is added to the alkaline earth aluminate / organosilicon composite material prepared in Example 5, stirred evenly, and then heated at 400°C for 10-20 minutes to obtain an alkaline earth aluminate / organosilicon composite material with a deposited Bi film, which is a ceramic material with photoluminescence and energy storage properties.
[0061] Example 9
[0062] Bi(NO3)3˙5H2O is added to the alkaline earth aluminate / organosilicon composite material prepared in Example 6, stirred evenly, and then heated at 400°C for 10-20 minutes to obtain an alkaline earth aluminate / organosilicon composite material with a deposited Bi film, which is a ceramic material with photoluminescence and energy storage properties.
[0063] Now the photoluminescence effect test of the ceramic materials prepared in Examples 7-9 was carried out. The F-4500 instrument was used to lay a quartz glass sheet flat in the middle of the tablet pressing mold. After the sample was ground, it was evenly dispersed on the glass sheet. The knob was covered on the groove, and the emission spectrum and laser spectrum were scanned. Each sample was tested 3 times, and the emission spectrum and the excitation spectrum were superimposed. The highest peak intensity of the photoluminescence was recorded, and the average value was recorded. The test results are shown in Table 2:
[0064] Table 2: Photoluminescence effect test of ceramic materials prepared in Examples 7-9
[0065]
[0066]
[0067] From the test results in Table 2, the highest peak intensity value of Example 9>Example 8>Example 7 indicates that Example 9 generates the most photons after the recombination of photogenerated electrons and holes, and the intensity of photoluminescence is the strongest.
[0068] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0069] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A ceramic material having photoluminescence and energy storage properties, characterized in that: The preparation method comprises the following steps: (1) preparing mesoporous organosilicon materials; (2) preparing a composite material from an organosilicon material and an alkaline earth aluminate; (3) Deposition of bismuth on alkaline earth aluminate / organic silicon composites.
2. A ceramic material having photoluminescence and energy storage properties according to claim 1, characterized in that: The preparation method of mesoporous organosilicon material is as follows: A1. Disperse chitosan in acetic acid solution, stir evenly, add vinyltriethoxysilane, and stir continuously overnight at room temperature to obtain a silicon-based solution; A2, dispersing a suspension containing liquid paraffin and sorbitan trioleate in a reactor and stirring for 30 minutes, then adding the silicon-based solution and continuing stirring for 60 minutes, and then adding polyoxyethylene sorbitan trioleate thereto and stirring for 60 minutes; A3. Add an isopropanol solution containing 28% ammonia dropwise into the reactor and stir for 1 hour. After vacuum filtration and washing with petroleum ether, ethanol and deionized water, freeze-dry the sample at -60°C for 24 hours and then carbonize it in an Ar / H2 atmosphere for 3 hours to obtain a mesoporous organosilicon material.
3. The ceramic material having photoluminescence and energy storage properties according to claim 1, characterized in that: The specific operation of preparing the composite material of organic silicon material and alkaline earth aluminate is as follows: B1, dissolving alkaline earth aluminate raw material in deionized water, adding nitric acid solution and urea, and then heating the mixture for 5-10 minutes; B2, transferring the heated mixture into a ceramic crucible, and dehydrating and decomposing at 500-900° C. for 3-5 minutes to obtain a fluffy alkaline earth aluminate product; B3. After fully grinding the alkaline earth aluminate product, add the mesoporous organosilicon material at a mixing ratio of 1:1 to obtain an alkaline earth aluminate / organosilicon composite material.
4. The ceramic material having photoluminescence and energy storage properties according to claim 3, characterized in that: The alkaline earth aluminate is SrAl2O4, SrAl 14 O 25 , SrAl4O7 and SrAl 12 O 19 One of them.
5. The ceramic material having photoluminescence and energy storage properties according to claim 1, characterized in that: The specific operation of depositing bismuth on the alkaline earth aluminate / organic silicon composite material is as follows: Bi(NO3)3˙5H2O is added to the alkaline earth aluminate / organosilicon composite material, stirred evenly, and then heated at 400°C for 10-20 minutes to obtain the alkaline earth aluminate / organosilicon composite material with a deposited Bi film.
6. The ceramic material having photoluminescence and energy storage properties according to claim 3, characterized in that: The alkaline earth aluminate raw materials include Sr(NO3)2, Al(NO3)3˙9H2O, Eu2O3, and Dy2O3, wherein the molar ratio of the raw materials Sr(NO3)2, Al(NO3)3˙9H2O, Eu2O3, and Dy2O3 is: 0.5-1:1:0.01:0.02.
Citation Information
Cited By
Cement-based grouting material based on periodic mesoporous organosilicon and preparation method thereof
CN120590129A
A periodic mesoporous organosilica-based cement-based grouting material and a preparation method thereof
CN120590129B