Magnetic high-entropy perovskite wave-absorbing material and preparation method thereof
Magnetic high entropy perovskite absorbing materials were prepared by sol-gel method, which solved the shortcomings of perovskite-type absorbing materials in synergistically with dielectric loss and magnetic loss, and achieved efficient electromagnetic wave absorption performance at low thickness. The process is environmentally friendly and low cost, and is suitable for industrial production.
Patent Information
- Application Number
- CN202411105265.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The existing perovskite-type wave absorbing materials have shortcomings in the synergistic effect of electromagnetic wave dielectric loss and magnetic loss, and have failed to effectively achieve material optimization.
Magnetic high entropy perovskite absorbing materials are prepared by sol-gel method, and mixed metal salts are formed by mixing lanthanum salts, barium salts, strontium salts, calcium salts, sodium salts, manganese salts, water, complexing agents and dispersants. The solution was heated and stirred in a water bath, dried and calcined to obtain a magnetic high entropy perovskite absorbing material with the chemical formula of (La0.2Ba0.2Sr0.2Ca0.2)MnO3.
The synergistic effect of dielectric loss and magnetic loss is achieved. The material has an effective absorption frequency bandwidth and high absorption strength under low thickness, and is environmentally friendly in process and low cost, which is suitable for large-scale industrial production.
Smart Images

Figure CN118993733A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high entropy ceramic materials, and in particular to a magnetic high entropy perovskite absorbing material and a preparation method thereof. Background Art
[0002] Since the 21st century, the rapid development of science and technology, especially electronic information technology, has brought great convenience to our lives and work. However, the excessive use of electronic products will lead to serious electromagnetic radiation and interference. The widespread application of electromagnetic waves in science and technology has also brought a series of social problems, which not only affects communication, but also directly or indirectly harms human health. A large number of electronic products have brought convenience while also bringing great harm. Electromagnetic radiation has become another major source of pollution after air pollution, water pollution, and light pollution in the 21st century. At the same time, with the in-depth development of precision-guided weapons, stealth weapons have become a key research project for the armaments of various countries. Absorbing materials are one of the key materials in the fields of national defense and civilian use, such as military stealth, microwave communications, and electromagnetic radiation protection. Absorbents with good absorbing properties are the core of absorbing materials. In order to meet the requirements of use under more demanding conditions, the research on absorbents has also developed in the direction of anti-oxidation, high efficiency, compatibility, and intelligence.
[0003] Perovskite material is a kind of absorbing material with strong dielectric loss and good stability. It is a kind of dielectric loss absorbing material that has attracted much attention. Zhao Biao and others from Fudan University have achieved the regulation of grain boundaries, oxygen defects and ultra-high density distorted lattices of high entropy perovskite ceramic materials by regulating the high entropy effect of components. 0.2 Sr 0.2 Ba 0.2 La 0.2 Pb 0.2 )TiO 3 The EAB of perovskite materials is almost twice that of barium titanate. It also shows that there are a large number of interfaces and defects inside high-entropy perovskite materials. When interacting with electromagnetic waves, the interfaces and defects will produce polarization effects, which improves its ability to attenuate electromagnetic waves. At the same time, the super-density strain caused by severe lattice distortion provides multiple transport channels for electronic carriers, leading to the generation of dielectric dissipation; and the results of electron holography show that the accumulation of positive / negative charges inside high-entropy ceramics at grain boundaries and strain concentration locations increases, resulting in more dielectric polarization losses; Che Renchao's team at Fudan University used a hydrothermal method to prepare BaTiO 3 The nanowire has a minimum reflection loss of -24.6dB at 9.04GHz and an effective absorption bandwidth of 2.4GHz. At present, the research on perovskite-type absorbing materials mainly focuses on the doping of materials to construct composite absorbing materials, and the optimization of the dielectric loss capacity of the materials, but has not achieved the synergistic effect of dielectric loss and magnetic loss on electromagnetic waves.
[0004] Therefore, how to obtain a magnetic high-entropy perovskite absorbing material and its preparation method is a technical problem that needs to be solved at present. Summary of the invention
[0005] The object of the present invention is to provide a magnetic high entropy perovskite absorbing material and a preparation method thereof, so as to solve the above-mentioned technical problems.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a magnetic high entropy perovskite wave absorbing material, comprising the following steps:
[0008] (1) mixing lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, water, a complexing agent and a dispersant to obtain a mixed metal salt solution;
[0009] (2) A mixed metal salt solution is prepared into a precursor by a sol-gel method, and the precursor is calcined to obtain a magnetic high-entropy perovskite absorbing material.
[0010] Furthermore, the lanthanum salt comprises lanthanum nitrate, the barium salt comprises barium chloride, the strontium salt comprises strontium chloride, the calcium salt comprises calcium chloride, the sodium salt comprises sodium nitrate, and the manganese salt comprises manganese chloride.
[0011] Furthermore, the complexing agent comprises citric acid, and the dispersant comprises ethylene glycol.
[0012] Furthermore, the molar ratio of the lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, complexing agent and dispersant is 1:1:1:1:1:5:10:8-15.
[0013] Furthermore, the sol-gel method is: placing a mixed metal salt solution in a water bath, heating and stirring to obtain a sol-like product, and drying the sol-like product to obtain a precursor;
[0014] The heating temperature is 70-85° C., and the stirring time is 5-7 hours.
[0015] Furthermore, the drying temperature is 80-95° C., and the drying time is 40-50 hours.
[0016] Furthermore, the calcination temperature is 1200-1450°C, the holding time is 3-5h, and the heating rate from room temperature to the calcination temperature is 3-8°C / min.
[0017] The present invention also provides a magnetic high entropy perovskite absorbing material, the chemical formula of the magnetic high entropy perovskite absorbing material is (La 0.2 Ba 0.2 Sr 0.2Ca 0.2 Na 0.2 )MnO 3 .
[0018] Beneficial effects of the present invention:
[0019] (1) The high entropy perovskite electromagnetic wave absorption material has both dielectric loss and magnetic loss properties. When the composite ratio with paraffin is 9:1 and the thickness is 1.0 mm, the minimum reflection loss can reach -60.86 dB; when the thickness is 1.1 mm, the effective absorption bandwidth can reach 3.26 GHz; therefore, the high entropy perovskite (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Electromagnetic wave absorbing materials have the characteristics of wide effective absorption frequency band and high absorption intensity at low thickness;
[0020] (2) At the same time, the present invention uses water as a solvent, does not require the use of highly toxic chemical reagents, is environmentally friendly and pollution-free; and the preparation process is simple and low-cost, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 To implement the (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 XRD pattern of
[0022] Figure 2 is the (La obtained in Example 1 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 SEM images of
[0023] Figure 3 is the (La obtained in Example 2 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 SEM images of
[0024] Figure 4 is the (La obtained in Example 3 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na0.2 )MnO 3 SEM images of
[0025] Figure 5 is the (La obtained in Example 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 SEM images of
[0026] Figure 6 For Examples 1, 2, 3, and 4 (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Reflection loss diagram at a thickness of 1.0 mm;
[0027] Figure 7 S(La) prepared in Examples 1, 2, 3, and 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Impedance matching diagram at a thickness of 1.0 mm;
[0028] Figure 8 The (La obtained in Example 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Reflection loss plot at different thicknesses.
[0029] Fig. 9 The (La obtained in Example 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Hysteresis loop diagram under ±2T magnetic field.
[0030] Fig.10 The (La obtained in Example 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Magnetic susceptibility temperature curve under 200Oe magnetic field. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a magnetic high entropy perovskite wave absorbing material, comprising the following steps:
[0032] (1) mixing lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, water, a complexing agent and a dispersant to obtain a mixed metal salt solution;
[0033] (2) A mixed metal salt solution is prepared into a precursor by a sol-gel method, and the precursor is calcined to obtain a magnetic high-entropy perovskite absorbing material.
[0034] In the present invention, the lanthanum salt is preferably lanthanum nitrate hexahydrate, the barium salt is preferably barium chloride monohydrate, the strontium salt is preferably strontium chloride hexahydrate, the calcium salt is preferably anhydrous calcium chloride, the sodium salt is preferably sodium nitrate, and the manganese salt is preferably manganese chloride tetrahydrate.
[0035] In the present invention, the complexing agent is preferably citric acid, and the dispersant is preferably ethylene glycol.
[0036] In the present invention, the molar ratio of the lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, complexing agent and dispersant is 1:1:1:1:1:5:10:8-15, preferably 1:1:1:1:1:5:10:10.
[0037] In the present invention, the amount of water used is sufficient to dissolve the metal salt.
[0038] In the present invention, the sol-gel method is: placing a mixed metal salt solution in a water bath, heating and stirring to obtain a sol-like product, and drying the sol-like product to obtain a precursor;
[0039] The heating temperature is 70-85° C., preferably 80° C.; the stirring time is 5-7 hours, preferably 6 hours.
[0040] In the present invention, the drying temperature is 80-95° C., preferably 90° C.; the drying time is 40-50 h, preferably 48 h.
[0041] In the present invention, the calcination temperature is 1200-1450°C, preferably 1300-1400°C, and more preferably 1400°C; the holding time is 3-5h, preferably 4h; the heating rate from room temperature to the calcination temperature is 3-8°C / min, preferably 5°C / min.
[0042] In the present invention, the calcination treatment is performed in an air atmosphere.
[0043] The present invention also provides a magnetic high entropy perovskite absorbing material, the chemical formula of the magnetic high entropy perovskite absorbing material is (La 0.2 Ba0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 .
[0044] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0045] Example 1
[0046] The method for preparing the magnetic high entropy perovskite absorbing material of this embodiment comprises the following steps:
[0047] (1) Preparation of precursors by sol-gel method
[0048] Weigh 2.16505g of lanthanum nitrate hexahydrate, 1.223g of barium chloride monohydrate, 1.3331g of strontium chloride hexahydrate, 0.5549g of anhydrous calcium chloride, 0.42495g of sodium nitrate, and 4.94755g of manganese chloride tetrahydrate and dissolve them in 50mL of distilled water to form a uniform solution. Weigh 10.507g of citric acid monohydrate and 4.2mL of ethylene glycol and stir until completely dissolved. Heat and stir the above solution at 80°C to form a sol. Put the sol product into a forced air drying oven at 90°C and dry it for 48h. Take it out after it naturally cools to room temperature to obtain a precursor.
[0049] (2) Sintering preparation of perovskite high entropy ceramics
[0050] The precursor obtained in step 1 was placed in a muffle furnace and calcined in air atmosphere at 1200°C for 4 hours with a heating rate of 5°C / min. After natural cooling, the product (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 .
[0051] Example 2
[0052] The method for preparing the magnetic high entropy perovskite absorbing material of this embodiment comprises the following steps:
[0053] (1) Preparation of precursors by sol-gel method
[0054] Weigh 2.16505g of lanthanum nitrate hexahydrate, 1.223g of barium chloride monohydrate, 1.3331g of strontium chloride hexahydrate, 0.5549g of anhydrous calcium chloride, 0.42495g of sodium nitrate, and 4.94755g of manganese chloride tetrahydrate and dissolve them in 50mL of distilled water to form a uniform solution. Weigh 10.507g of citric acid monohydrate and 4.2mL of ethylene glycol and stir until completely dissolved. Heat and stir the above solution at 80°C to form a sol. Put the sol product into a forced air drying oven at 90°C and dry it for 48h. Take it out after it naturally cools to room temperature to obtain a precursor.
[0055] (2) Sintering preparation of perovskite high entropy ceramics
[0056] The precursor obtained in step 1 was placed in a muffle furnace and calcined in air atmosphere at 1300°C for 4 hours with a heating rate of 5°C / min. After natural cooling, the product (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 .
[0057] Example 3
[0058] The method for preparing the magnetic high entropy perovskite absorbing material of this embodiment comprises the following steps:
[0059] (1) Preparation of precursors by sol-gel method
[0060] Weigh 2.16505g of lanthanum nitrate hexahydrate, 1.223g of barium chloride monohydrate, 1.3331g of strontium chloride hexahydrate, 0.5549g of anhydrous calcium chloride, 0.42495g of sodium nitrate, and 4.94755g of manganese chloride tetrahydrate and dissolve them in 50mL of distilled water to form a uniform solution. Weigh 10.507g of citric acid monohydrate and 4.2mL of ethylene glycol and stir until completely dissolved. Heat and stir the above solution at 80°C to form a sol. Put the sol product into a forced air drying oven at 90°C and dry it for 48h. Take it out after it naturally cools to room temperature to obtain a precursor.
[0061] (2) Sintering preparation of perovskite high entropy ceramics
[0062] The precursor obtained in step 1 was placed in a muffle furnace and calcined in air atmosphere at 1400°C for 4 hours with a heating rate of 5°C / min. After natural cooling, the product (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 .
[0063] Example 4
[0064] The method for preparing the magnetic high entropy perovskite absorbing material of this embodiment comprises the following steps:
[0065] (1) Preparation of precursors by sol-gel method
[0066] Weigh 2.16505g of lanthanum nitrate hexahydrate, 1.223g of barium chloride monohydrate, 1.3331g of strontium chloride hexahydrate, 0.5549g of anhydrous calcium chloride, 0.42495g of sodium nitrate, and 4.94755g of manganese chloride tetrahydrate and dissolve them in 50mL of distilled water to form a uniform solution. Weigh 10.507g of citric acid monohydrate and 4.2mL of ethylene glycol and stir until completely dissolved. Heat and stir the above solution at 80°C to form a sol. Put the sol product into a forced air drying oven at 90°C and dry it for 48h. Take it out after it naturally cools to room temperature to obtain a precursor.
[0067] (2) Sintering preparation of perovskite high entropy ceramics
[0068] The precursor obtained in step 1 was placed in a muffle furnace and calcined in air atmosphere at 1450°C for 4 hours with a heating rate of 5°C / min. After natural cooling, the product (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 .
[0069] Figure 1 The results of different sintering temperatures (La) obtained in Examples 1, 2, 3, and 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 From the X-ray diffraction diagram, it can be seen that at a treatment temperature of 1200°C, Example 1 has a second phase with a non-perovskite structure. At a temperature of 1300°C, the number of diffraction peaks of the second phase of Example 2 becomes weaker and decreases. When the temperature rises to 1400°C, the peak intensity of the second phase of Example 3 further decreases. As the temperature further rises, the second phase peak of Example 4 disappears, forming a single phase.
[0070] Figure 2 , 3 , 4, 5 are respectively the sintering temperatures (La) obtained in Examples 1, 2, 3, 4 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3From the SEM picture, it can be seen that with the increase of temperature, the particle size continues to increase.
[0071] Figure 6 The results of the present invention are shown in Table 1. The results of the present invention are shown in Table 1. 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The reflection loss graph at a thickness of 1.1 mm shows that the material exhibits excellent electromagnetic wave absorption performance when the sintering temperature is 1450°C, with a minimum reflectivity of -60.86 dB and an effective absorption bandwidth of 3.26 GHz (14.74-18 GHz). A sintering temperature that is too low (1200°C) is not conducive to improving the electromagnetic wave absorption performance of the material.
[0072] Figure 7 The results of the present invention are shown in Table 1. The results of the present invention are shown in Table 1. 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The impedance matching diagram at a thickness of 1.0 mm shows that relatively excellent wave impedance matching characteristics are exhibited at sintering temperatures of 1400°C and 1450°C, while the wave impedance matching characteristics at 1200°C and 1300°C are poor.
[0073] Figure 8 (La obtained in Example 4 of the present invention 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The reflection loss diagram under different thicknesses shows that: (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 It exhibits effective electromagnetic wave absorption performance in the thickness range of 1-5mm, and its effective absorption bandwidth can effectively cover about 2-18GHz.
[0074] Fig. 9 (La obtained in Example 4 of the present invention 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO3 Hysteresis loop, as can be seen from the figure: (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 It exhibits ferromagnetism, has a narrow hysteresis loop, and has the characteristics of a soft magnetic material.
[0075] Fig.10 (La obtained in Example 4 of the present invention 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The magnetic permeability changes with temperature. It can be seen from the figure that: (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The field-cooling and zero-field-cooling curves overlap, showing ferromagnetism at about 5-360°C.
[0076] It can be seen from the above embodiments that the present invention provides a magnetic high entropy perovskite absorbing material and a preparation method thereof. The magnetic high entropy perovskite absorbing material of the present invention uses a simple sol-gel method to prepare the perovskite microwave absorbing material, and its optimal absorbing performance can be obtained by calcining the dried precursor at 1450°C in a muffle furnace for 4 hours. (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 The loss of the material is mainly attributed to the synergistic effect of dielectric loss and magnetic loss. 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO 3 Compared with traditional microwave absorbers, magnetic high-entropy perovskite absorbing materials have the characteristics of wide effective absorption bandwidth and high absorption intensity at low thickness; at the same time, the present invention uses water as a solvent, does not require the use of highly toxic chemical reagents, is environmentally friendly and pollution-free; and has a simple preparation process and low cost, and is suitable for large-scale industrial production.
[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a magnetic high entropy perovskite absorbing material, characterized in that: The following steps are involved: (1) mixing lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, water, a complexing agent and a dispersant to obtain a mixed metal salt solution; (2) A mixed metal salt solution is prepared into a precursor by a sol-gel method, and the precursor is calcined to obtain a magnetic high-entropy perovskite absorbing material.
2. The preparation method according to claim 1, characterized in that: The lanthanum salt comprises lanthanum nitrate, the barium salt comprises barium chloride, the strontium salt comprises strontium chloride, the calcium salt comprises calcium chloride, the sodium salt comprises sodium nitrate, and the manganese salt comprises manganese chloride.
3. The preparation method according to claim 2, characterized in that: The complexing agent comprises citric acid, and the dispersing agent comprises ethylene glycol.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The molar ratio of the lanthanum salt, barium salt, strontium salt, calcium salt, sodium salt, manganese salt, complexing agent and dispersant is 1:1:1:1:1:5:10:8-15.
5. The preparation method according to claim 4, characterized in that: The sol-gel method comprises: placing a mixed metal salt solution in a water bath, heating and stirring to obtain a sol-like product, and drying the sol-like product to obtain a precursor; The heating temperature is 70-85° C., and the stirring time is 5-7 hours.
6. The preparation method according to claim 5, characterized in that: The drying temperature is 80-95° C., and the drying time is 40-50 hours.
7. The preparation method according to claim 6, characterized in that: The calcination temperature is 1200-1450° C., the heat preservation time is 3-5 hours, and the heating rate from room temperature to the calcination temperature is 3-8° C. / min.
8. The magnetic high entropy perovskite absorbing material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The chemical formula of the magnetic high entropy perovskite absorbing material is (La 0.2 Ba 0.2 Sr 0.2 Ca 0.2 Na 0.2 )MnO3.
Citation Information
Patent Citations
High-entropy perovskite type electromagnetic wave absorbing material and preparation method thereof
CN116282214A
Perovskite type ceramic material and preparation method and application thereof
CN116589264A
A and B-site co-doped BaTiO3-based high-entropy dielectric film and preparation method thereof
CN117756171A
Catalyst for catalytic degradation of volatile organic compounds, and preparation method and application thereof
CN118267984A
Rare earth perovskite colloidal dispersion and method for the production thereof
WO2004103546A2
Cited By
High-entropy ceramic wave-absorbing material and design method and preparation method thereof
CN121168022A
Associated electronic material of double-phase high-entropy heterojunction microstructure based on high-entropy perovskite reconstruction as well as high-throughput preparation method and application of associated electronic material
CN122559218A