Preparation method of flue castable for reducing gas corrosion in fluidized bed boiler

By using mixed powder and reinforcement materials prepared by barium sulfate powder and other materials, combined with materials such as polytetrafluoroethylene film to form a splicing layer, the problem of insufficient corrosion resistance of traditional flue castables in high-temperature flue gas and acidic environments is solved, and the corrosion resistance performance of traditional flue castables is insufficient in high-temperature flue gas and acidic environments is achieved. It has higher corrosion resistance and mechanical strength, simplified construction and adapted to complex working conditions.

CN118993749AActive Publication Date: 2024-11-22YIXING HAIKE REFRACTORY PROD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411088117.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional flue castables have insufficient corrosion resistance in high-temperature flue gas erosion and acidic environments, and are complex and inflexible in construction, making them difficult to meet the needs of complex working conditions, which affects the service life and operation safety of fluidized bed boilers.

Method used

Mixed powder is prepared by barium sulfate powder, microsilicon powder, zinc oxide powder, gamma-alumina powder and aluminum-chromium slag powder, and combined with polytetrafluoroethylene film, basalt fiber cloth and mesh galvanized steel wire to form a splicing layer. Reinforcement materials and surface materials are prepared by titanium carbide powder, biochar powder and other materials to form comprehensive castable materials to improve corrosion resistance and mechanical strength.

Benefits of technology

It significantly improves the corrosion resistance and mechanical strength of the flue castable, enhances its resistance to acidic environment, simplifies the construction process, improves the durability and service life of the material, and adapts to different working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993749A_ABST
    Figure CN118993749A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flue castable materials, in particular to a preparation method of a flue castable material for reducing gas corrosion in a fluidized bed boiler, and the preparation method comprises the following steps: S1, preparing mixed powder, S2, preparing a splicing layer, S3, preparing a reinforcing material, and S4, preparing an anti-corrosion flue castable material. According to the invention, the splicing layer is adopted, so that the corrosion resistance, especially the gas corrosion resistance, of the flue castable is remarkably improved, and the mechanical strength and the impact resistance of the material are improved; the reinforcing material is poured, the surface layer material is poured after airing, the three materials are combined for use, and the corrosion-resistant flue pouring layer with high comprehensive quality is obtained; the strength and the wear resistance of the pouring layer are further improved by pouring the reinforcing material; and a long-acting protective layer with high temperature resistance, acid medium resistance and chemical smoke corrosion resistance is formed through the surface layer material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flue castables, and in particular to a method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler. Background Art

[0002] In modern industrial production, fluidized bed boilers are widely used in the fields of electricity, chemical industry, metallurgy, etc. due to their high efficiency and environmental protection. During the operation of fluidized bed boilers, acidic gases (such as SOx, NOx, etc.) in the flue gas will cause serious corrosion to the metal parts inside the boiler, affecting the service life and operation safety of the equipment. In order to solve this problem, the traditional approach is to use refractory castables inside the boiler for protection.

[0003] Although traditional refractory castables can resist the erosion of high-temperature flue gas to a certain extent, their acid resistance is not ideal, especially when exposed to an environment containing acidic gas for a long time, their corrosion resistance will gradually decrease; traditional castables are prone to cracks when the temperature changes drastically, resulting in material peeling and damage, thereby reducing the service life of the boiler; the construction process of traditional castables is complicated, requiring professional technicians to operate, and the construction period is long, affecting the progress and cost of the project; the performance of traditional castables in different working environments varies greatly, making it difficult to meet the needs of various complex working conditions. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler.

[0005] The technical solution of the present invention is: a method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler, comprising the following steps:

[0006] S1. Mixed powder ingredients

[0007] By mass percentage, 12-14% of barium sulfate powder, 10-12% of microsilicon powder, 3-8% of alloy fiber, 1-8% of zinc oxide powder, 3-5% of γ-alumina powder and the remainder of aluminum-chromium slag powder are mixed uniformly to obtain a mixed powder;

[0008] S2. Preparation of splicing layer

[0009] The size of the flue to be cast is measured, and several sheet molds matching the size are selected, wherein the thickness of the mold is 0.5 to 3 cm, and the mixed powder is introduced into the mold, and the mold is pressed and formed, and the mixture is kept at 1000 to 1800° C. for 0.5 to 1 hour. After cooling, a layer of polytetrafluoroethylene film is laid on the surface, and then a layer of basalt fiber cloth or aramid fiber cloth is laid on the polytetrafluoroethylene film, and then another layer of polytetrafluoroethylene film is laid, and finally a layer of mesh galvanized steel wire is evenly laid, and the mixture is kept at 90 to 110° C. for 12 to 24 hours, and the mold is demolded after cooling to obtain a splicing layer; the thickness of the two polytetrafluoroethylene films is 0.08 to 0.3 mm, the thickness of the basalt fiber cloth or aramid fiber cloth is 0.4 to 0.5 mm, and the average thickness of the mesh galvanized steel wire is 0.5 to 2.5 mm;

[0010] S3. Preparation of reinforcement material

[0011] By mass percentage, 15-25% of titanium carbide powder, 15-18% of biochar powder, 10-15% of perlite, 2-15% of fused magnesia powder, 8-14% of glass microspheres, 5-10% of polyacrylic acid microspheres, 2-7% of polyvinyl alcohol, 2-5% of sodium polyacrylate and the remainder of cement are added with an appropriate amount of water at 90-110° C. and mixed evenly to obtain a reinforcement material;

[0012] S4. Preparation of anti-corrosion flue casting material

[0013] S4-1, pre-treatment of glass flakes;

[0014] S4-2, preparing surface material;

[0015] S4-3. Adjust the viscosity of the surface material, splice the splicing layer on the inner wall of the flue, then pour the reinforcement material, and finally pour the surface material. Combine the raw materials according to the above operations to obtain a flue castable that reduces gas corrosion.

[0016] Description: When using, measure the size of the flue, prepare several splicing layers, lay the splicing layers inside the flue, pour the reinforcement material, pour the surface material after drying, and use the three materials in combination to pour the flue;

[0017] Zinc oxide in the mixed powder can react with other ingredients such as γ-alumina and fused magnesia powder at high temperatures to form refractory minerals, thereby improving the refractory properties of the castable. Zinc oxide has good light stability and antioxidant properties, which can improve the weather resistance of the castable. The addition of zinc oxide may help reduce the shrinkage of the castable during the cooling process, thereby reducing the generation of cracks. Zinc oxide can improve the corrosion resistance of the castable, especially in an acidic environment.

[0018] The polytetrafluoroethylene film can act as an isolation between the galvanized steel wire and the basalt fiber cloth or aramid fiber cloth, absorb and disperse the stress caused by temperature changes, and prevent it from being directly transmitted to the basalt fiber cloth or aramid fiber cloth, thereby protecting the anti-corrosion layer and reducing damage; during the high-temperature melting thermoplasticization process, the various layers of materials are fused together at high temperatures to form a tightly combined overall structure. This process helps to improve the overall strength and sealing of the anti-corrosion layer, making it more resistant to the effects of temperature changes; the polytetrafluoroethylene film has a smooth surface and an extremely low friction coefficient, which helps to reduce friction between materials, thereby reducing the risk of damage and falling off caused by friction. The polytetrafluoroethylene film can maintain its physical and chemical properties over a wide temperature range, which means that they can be used in high and low temperature environments without losing their anti-corrosion properties.

[0019] Furthermore, in S1, the particle size of the barium sulfate powder is 50-60 μm, the particle size of the microsilicon powder is 30-40 μm, the average length of the alloy fiber is 1-3 mm, the particle size of the zinc oxide powder is 20-40 μm, the particle size of the γ-alumina powder is 20-30 μm, and the particle size of the aluminum chromium slag powder is 0.2-5 mm.

[0020] Description: Particles of different sizes can fill the space better, form a tight stack, and improve the density and overall performance of the material; smaller particles can fill the gaps between large particles, increase the contact points, and improve the density and strength of the material; mixing particles of different sizes can increase the contact area between particles, which helps to improve the interfacial bonding between the components, thereby enhancing the mechanical properties and corrosion resistance of the material; by optimizing the particle size distribution, the durability and service life of the material can be improved, which is especially important for materials such as flue castables that need to work for a long time in harsh environments.

[0021] Furthermore, the method for pretreating glass flakes described in S4-1 is: cleaning the glass flake raw materials with acetone having a mass concentration of 95-98% or alcohol having a mass concentration of 99-99.9%, polishing the surface of the glass flakes, and then acid-washing after drying.

[0022] Description: Use acetone with a mass concentration of 95-98% or alcohol with a mass concentration of 99-99.9% to clean the glass flake raw materials to remove oil, dust and other contaminants on the surface, and polish the surface of the glass flakes to remove the rough parts and uneven edges of the surface to improve its smoothness; the cleaned and processed glass flakes need to be dried to remove surface moisture to prevent the introduction of moisture during the subsequent mixing and construction process, which will lead to performance degradation, and the oxide layer and other inorganic impurities on the surface of the glass flakes are removed by acid pickling.

[0023] Furthermore, the particle sizes of the glass flakes include 20 mesh, 60 mesh, and 110 mesh, and the mass ratios are 9 to 10:1:1, respectively.

[0024] Description: Glass flakes of different particle sizes can form a multi-layer staggered structure in the coating, effectively blocking the penetration of corrosive media and improving the corrosion resistance of the coating; the appropriate glass flake particle size and proportion can enhance the adhesion and toughness of the coating and reduce the risk of cracking and peeling of the coating; when the glass flake coating as the surface layer is subjected to friction, even if damage occurs, it is limited to a local area and will not affect the wear resistance of the entire coating; the glass flake itself has a small thermal expansion coefficient, can adapt to high-temperature working environments, and has good thermal shock resistance.

[0025] Furthermore, the method for preparing the surface material described in S4-2 is: by mass percentage, 50-60% of the glass flakes pretreated by S4-1, 1-3% of the curing agent, 1-3% of the accelerator, 1-2% of the thixotropic stabilizer, 1-12% of the low shrinkage agent, 0.2-1.2% of the silane coupling agent, 0.2-1% of the defoaming agent, 0.1-3% of the nano-silica and the remainder of the vinyl ester resin are mixed evenly to obtain the surface material.

[0026] Description: The high proportion of glass flakes enhances the corrosion resistance and wear resistance of the coating, especially when facing strong acids, strong alkalis or other corrosive media, while curing agents, accelerators and thixotropic stabilizers help to improve the curing speed and construction performance of the coating: The addition of low shrinkage agents helps to reduce the volume shrinkage of the coating during curing, avoid stress and cracks caused by shrinkage, and improve the integrity and durability of the coating; the use of silane coupling agents can improve the interfacial bonding between glass flakes and the resin matrix, and enhance the adhesion and durability of the coating; the addition of thixotropic stabilizers and defoamers helps to improve the rheology of the coating while reducing the generation of bubbles; the addition of nano-silica can improve the weather resistance and UV radiation resistance of the coating and extend the service life of the coating.

[0027] Furthermore, the curing agent is 328E; the accelerator is an organic tin compound and a tertiary amine compound; the thixotropic stabilizer is BYK-R605; the low shrinkage agent is polyamide; the defoaming agent is BYK-555; and the silane coupling agent is propyltrimethoxysilane.

[0028] Description: 328E is an epoxy resin curing agent that can react with vinyl ester resin to achieve rapid curing and shorten production cycle; 328E has good compatibility with vinyl ester resin and helps to form a uniform coating structure; organic tin compounds and tertiary amine compounds are used as accelerators to accelerate the reaction rate between the curing agent and the resin and improve production efficiency; these accelerators help control the exothermic reaction during the curing process to avoid coating defects caused by overheating;

[0029] BYK-R605 is a highly efficient thixotropic stabilizer that can improve the rheology of the coating, maintain its shape in a static state, and prevent sagging; the use of thixotropic stabilizers helps to improve the convenience of construction and the uniformity of the coating; polyamide, as a low shrinkage agent, can effectively reduce the volume shrinkage of the coating during curing and avoid internal stress and cracks caused by shrinkage; reducing shrinkage helps to improve the integrity and durability of the coating; BYK-555 is a highly efficient defoamer that can effectively eliminate bubbles generated during mixing and construction and improve the appearance and performance of the coating; the use of defoamers helps to obtain a smoother and defect-free coating surface.

[0030] Furthermore, the method for adjusting the viscosity of the surface material in S4-3 is: during the stirring process, a proper amount of diluent or thickener is evenly added to adjust the pouring viscosity of the surface material to 0.5-1 Pa·s.

[0031] Description: Adjusting the viscosity can make the surface material easier to pour, improving the convenience and efficiency of construction; the appropriate viscosity helps the surface material to form a uniform coating during pouring, avoiding the difficulty in flowing due to too high viscosity or the sagging caused by too low viscosity, thereby ensuring the quality and consistency of the coating; by adjusting the viscosity, the reaction rate and heat release during the curing process can be indirectly controlled, which helps to avoid coating defects caused by too fast or too slow curing; different construction environments and conditions require different viscosity settings; by adjusting the viscosity, the surface material can adapt to different construction temperatures, humidity and other environmental factors, improving the adaptability and flexibility of the material; the adjustment of viscosity also helps to improve the physical and chemical properties of the coating, such as corrosion resistance, wear resistance and weather resistance.

[0032] Furthermore, the diluent is one or a combination of methanol, ethanol, acetone, methyl ethyl ketone, butyl ester, ethyl acetate, and the thickener is one or a combination of two of fumed silica or bentonite.

[0033] Description: Solvents such as methanol, ethanol, acetone, methyl ethyl ketone, butyl ester, and ethyl acetate have good solubility and volatility, and are suitable for a variety of resin systems. They can effectively reduce the viscosity and make the surface material easier to pour; these diluents usually have a faster volatilization rate, which helps to dry quickly after construction, reduce waiting time, and improve construction efficiency; the viscosity can be precisely adjusted by selecting a single diluent or a combination of them to meet different construction requirements;

[0034] Fumed silica is a highly efficient thickener that can increase viscosity without significantly changing the chemical properties of the resin system, providing good thixotropy and fluidity control; bentonite is a natural mineral thickener with excellent thickening effect and suspension stability, which can increase the viscosity and stability of the surface material and prevent sedimentation and stratification; fumed silica and bentonite can not only thicken, but also improve the heat resistance and chemical resistance of the coating, enhancing the overall performance of the coating.

[0035] The beneficial effects of the present invention are:

[0036] (1) The present invention can significantly improve the corrosion resistance of flue casting materials, especially the ability to resist gas corrosion, by using materials such as barium sulfate powder, microsilicon powder, zinc oxide powder, γ-alumina powder and aluminum chromium slag powder; the addition of alloy fiber can enhance the mechanical strength and impact resistance of the material; when the present invention is in use, a plurality of splicing layers are arranged inside the flue, and the reinforcement material is poured, and the surface material is poured after drying, and the three materials are used in combination to obtain a flue casting layer with strong comprehensive quality and corrosion resistance; when preparing the splicing layer, the mixed powder is pressed into shape and kept warm for a long time, which helps to improve the structural stability and high temperature resistance of the material; by preparing the splicing layer, it can be customized according to the actual size of the flue, which improves the flexibility and convenience of construction; the splicing layer is stabilized by the reinforcement material, and the corrosion resistance of the flue is enhanced by the surface material.

[0037] (2) The present invention strengthens the strength of the castable by galvanized steel wire, making it easier to bear the weight of the castable and the pressure during the construction process, while having good durability to ensure its long-term use; the corrosion resistance is improved by hot-dip galvanizing; the mesh structure allows it to have a certain deformation space when heated or cooled, thereby compensating for the expansion or contraction caused by temperature changes and reducing the tensile or compressive stress on the anti-corrosion layer; after high-temperature thermoplasticization, the room temperature cooling process allows the anti-corrosion layer to gradually solidify and reach the final physical state; the various components of the anti-corrosion layer will adapt to each other's size and shape to form a stable composite structure, thereby reducing the internal stress and potential risk of falling off caused by temperature changes.

[0038] (3) The zinc oxide in the splicing layer of the present invention can react and hydrate with the components in the cement in the reinforcement material to form a harder structure, thereby improving the mechanical strength of the castable; the combination of titanium carbide powder, biochar powder, perlite, fused magnesia powder and other materials in the reinforcement material further improves the strength and wear resistance of the material; by using anti-corrosion mortar as the surface material, a long-lasting protective layer that is easy to construct and resistant to high temperature, acidic media and chemical fumes can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is a bar graph of the compressive strength test of samples of Examples 1 to 7, 12, 13 of the present invention and Comparative Examples 1 to 4;

[0040] Figure 2 It is a bar graph of the line change test after burning of the samples of Examples 1 to 7, 12, 13 of the present invention and Comparative Examples 1 to 4. DETAILED DESCRIPTION

[0041] In order to further illustrate the method and effect of the present invention, the technical solution of the present invention will be clearly and completely described in combination with experiments.

[0042] Embodiment 1:

[0043] A method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler comprises the following steps:

[0044] S1. Mixed powder ingredients

[0045] By mass percentage, 13% of barium sulfate powder, 11% of microsilicon powder, 5.5% of alloy fiber, 4.5% of zinc oxide powder, 4% of γ-alumina powder and the remainder of aluminum chromium slag powder are mixed uniformly to obtain a mixed powder;

[0046] The particle size of the barium sulfate powder is 54.5-55 μm, the particle size of the microsilica powder is 34.5-35 μm, the average length of the alloy fiber is 1.5-2 mm, the particle size of the zinc oxide powder is 29.5-30 μm, the particle size of the γ-alumina powder is 24.5-25 μm, and the particle size of the aluminum chromium slag powder is 2.5-2.6 mm;

[0047] S2. Preparation of splicing layer

[0048] The size of the flue to be cast is measured, and several sheet molds matching the size are selected, wherein the thickness of the mold is 1.25 cm, and the mixed powder is introduced into the mold, and the mold is pressed and formed, and the mold is kept at 1400° C. for 0.75 h. After cooling, a layer of polytetrafluoroethylene film is laid on the surface, and then a layer of basalt fiber cloth or aramid fiber cloth is laid on the polytetrafluoroethylene film, and then another layer of polytetrafluoroethylene film is laid, and finally a layer of mesh galvanized steel wire is evenly laid, and the mold is kept at 100° C. for 18 h. After cooling, the mold is demolded to obtain a splicing layer; the thickness of the two polytetrafluoroethylene films is 0.2 mm, the thickness of the basalt fiber cloth or aramid fiber cloth is 0.45 mm, and the average thickness of the mesh galvanized steel wire is 1.5 mm;

[0049] S3. Preparation of reinforcement material

[0050] By mass percentage, 20% of titanium carbide powder, 16.5% of biochar powder, 12.5% ​​of perlite, 8.5% of fused magnesia powder, 11% of glass microspheres, 7.5% of polyacrylic acid microspheres, 4.5% of polyvinyl alcohol, 3.5% of sodium polyacrylate and the rest of cement are added with an appropriate amount of water at 100° C. and mixed evenly to obtain a reinforcement material;

[0051] S4. Preparation of anti-corrosion flue casting material

[0052] S4-1. Pretreatment of glass flakes

[0053] The method for pretreating glass flakes is: washing the raw material of glass flakes with acetone having a mass concentration of 96.5%, polishing the surface of the glass flakes, drying and then pickling; the particle sizes of the glass flakes include 20 mesh, 60 mesh, and 110 mesh, and the mass ratios are 9.5:1:1 respectively;

[0054] S4-2. Preparation of surface material

[0055] The method for preparing the mixed raw materials is: according to mass percentage, 55% of glass flakes pretreated with S4-1, 2% of curing agent, 2% of accelerator, 1.5% of thixotropic stabilizer, 6.5% of low shrinkage agent, 0.7% of silane coupling agent, 0.6% of defoaming agent, 2% of nano-silicon dioxide and the rest of vinyl ester resin are mixed evenly to obtain a surface material;

[0056] The curing agent is 328E; the accelerator is an organic tin compound and a tertiary amine compound; the thixotropic stabilizer is BYK-R605; the low shrinkage agent is polyamide; the defoamer is BYK-555; and the silane coupling agent is propyl trimethoxy silane.

[0057] S4-3. Adjust the viscosity of the surface material

[0058] The method for adjusting the viscosity of the surface material is: during the stirring process, a proper amount of diluent or thickener is evenly added to adjust the casting viscosity of the surface material to 0.75 Pa·s; the diluent is methanol, and the thickener is bentonite. The splicing layer is arranged inside the flue, and then the reinforcement material is poured, and the surface material is poured after drying, and the combination is used in sequence to obtain the anti-corrosion flue castable.

[0059] Example 2: This example is basically the same as Example 1, except that, by mass percentage, 12% barium sulfate powder, 10% microsilicon powder, 3% alloy fiber, 1% zinc oxide powder, 3% γ-alumina powder and the remainder aluminum chromium slag powder are mixed evenly to obtain a mixed powder.

[0060] Example 3: This example is basically the same as Example 1, except that, by mass percentage, 14% barium sulfate powder, 12% microsilicon powder, 8% alloy fiber, 8% zinc oxide powder, 5% γ-alumina powder and the remainder aluminum chromium slag powder are mixed evenly to obtain a mixed powder.

[0061] Example 4: This example is basically the same as Example 1, except that the mold thickness is 0.5 cm, the mixed powder is introduced into the mold, pressed into shape, and kept warm at 1000°C for 0.5 h. After cooling, a layer of polytetrafluoroethylene film is laid on the surface, and then a layer of basalt fiber cloth or aramid fiber cloth is laid on the polytetrafluoroethylene film, followed by another layer of polytetrafluoroethylene film, and finally a layer of mesh galvanized steel wire is evenly laid. The mold is kept warm at 90°C for 12 h, and demolded after cooling to obtain a splicing layer.

[0062] Example 5: This example is basically the same as Example 1, except that the mold thickness is 3 cm, the mixed powder is introduced into the mold, pressed into shape, and kept warm at 1800°C for 1 hour. After cooling, a layer of polytetrafluoroethylene film is laid on the surface, and then a layer of basalt fiber cloth or aramid fiber cloth is laid on the polytetrafluoroethylene film, followed by another layer of polytetrafluoroethylene film, and finally a layer of mesh galvanized steel wire is evenly laid. The mold is kept warm at 110°C for 24 hours, and demolded after cooling to obtain a splicing layer.

[0063] Example 6: This example is basically the same as Example 1, except that, by mass percentage, 15% of titanium carbide powder, 15% of biochar powder, 10% of perlite, 2% of fused magnesia powder, 8% of glass beads, 5% of polyacrylic acid microspheres, 2% of polyvinyl alcohol, 2% of sodium polyacrylate and the remainder of cement are added with an appropriate amount of water at 90°C and mixed evenly to obtain a reinforcement material.

[0064] Example 7: This example is basically the same as Example 1, except that, by mass percentage, 25% of titanium carbide powder, 18% of biochar powder, 15% of perlite, 15% of fused magnesia powder, 14% of glass beads, 10% of polyacrylic acid microspheres, 7% of polyvinyl alcohol, 5% of sodium polyacrylate and the remainder of cement are added with an appropriate amount of water at 110°C and mixed evenly to obtain a reinforcement material.

[0065] Example 8: This example is basically the same as Example 1, except that the particle size of the barium sulfate powder is 50-50.5 μm, the particle size of the microsilicon powder is 30-30.5 μm, the average length of the alloy fiber is 1-1.5 mm, the particle size of the zinc oxide powder is 20-20.5 μm, the particle size of the γ-alumina powder is 20-20.5 μm, and the particle size of the aluminum chromium slag powder is 0.2-0.25 mm.

[0066] Example 9: This example is basically the same as Example 1, except that the particle size of the barium sulfate powder is 59.5-60μm, the particle size of the microsilicon powder is 39.5-40μm, the average length of the alloy fiber is 2.95-3mm, the particle size of the zinc oxide powder is 39.5-40μm, the particle size of the γ-alumina powder is 29.5-30μm, and the particle size of the aluminum chromium slag powder is 4.5-5mm.

[0067] Example 10: This example is basically the same as Example 1, except that the particle sizes of the glass flakes include 20 mesh, 60 mesh, and 110 mesh, and the mass ratios are 9:1:1 respectively.

[0068] Example 11: This example is basically the same as Example 1, except that the particle sizes of the glass flakes include 20 mesh, 60 mesh, and 110 mesh, and the mass ratios are 10:1:1 respectively.

[0069] Example 12: This example is basically the same as Example 1, except that the method for preparing the mixed raw materials is as follows: by mass percentage, 50% of the glass flakes pretreated with S4-1, 1% of the curing agent, 1% of the accelerator, 1% of the thixotropic stabilizer, 1% of the low shrinkage agent, 0.2% of the silane coupling agent, 0.2% of the defoaming agent, 0.1% of the nano-silica and the remainder of the vinyl ester resin are mixed evenly to obtain the surface material.

[0070] Example 13: This example is basically the same as Example 1, except that the method for preparing the mixed raw materials is as follows: by mass percentage, 60% of glass flakes pretreated with S4-1, 3% of a curing agent, 3% of an accelerator, 2% of a thixotropic stabilizer, 12% of a low shrinkage agent, 1.2% of a silane coupling agent, 1% of a defoaming agent, 3% of nano-silica and the remainder of vinyl ester resin are mixed evenly to obtain a surface material.

[0071] Comparative Example 1: Taking Example 1 as a reference, no splicing layer is arranged, and the reinforcement material is directly poured into the flue, and the surface material is poured after drying.

[0072] Comparative Example 2: Using Example 1 as a reference, the surface material is directly poured without pouring the reinforcement material.

[0073] Comparative Example 3: Using Example 1 as a reference, no surface material is poured.

[0074] Comparative Example 4: Using Example 1 as a reference, no mesh galvanized steel wire is laid when preparing the splicing layer.

[0075] In order to explore the performance of the castables produced in Examples 1 to 7, 12, 13 and Comparative Examples 1 to 4, the main materials were determined according to the experimental formula and 13 groups of samples were prepared for testing. The specific exploration is as follows:

[0076] Figure 2 Middle: Condition 1 is placed at 200℃ for 3h; Condition 2 is placed at 200℃ for 36h;

[0077] 1. Explore the influence of mixed powder ratio on castable performance:

[0078] like Figure 1 , 2 As shown, by comparing Examples 1 to 3, it can be seen that Example 1 has better comprehensive performance; changing the mixed powder ratio parameters will have a certain impact on the prepared castable sample, among which the castable prepared by the process parameter values ​​close to Example 1 has better comprehensive performance.

[0079] 2. Investigate the influence of process parameters for preparing splicing layers on castable properties:

[0080] like Figure 1 , 2 As shown, by comparing Examples 1, 4, and 5, it can be seen that: it can be seen that the comprehensive performance of Example 1 is better; changing the process parameters for preparing the splicing layer will have a certain impact on the prepared castable sample, among which the castable prepared with the process parameter value closer to Example 1 has the best comprehensive performance.

[0081] like Figure 1 , 2As shown, by comparing Example 1 with Control Example 1, it can be seen that the comprehensive performance of Example 1 is significantly better than that of Control Example 1. Compared with not laying out a splicing layer, directly pouring the reinforcement material into the flue, and pouring the surface material after drying, the sample with a splicing layer has better comprehensive performance; by comparing Example 1 with Control Example 4, it can be seen that the compressive strength performance of Example 1 is significantly better than that of Control Example 4, and the addition of mesh galvanized steel wire has a more obvious effect on the durability and compressive strength of the castable.

[0082] 3. Explore the influence of the ratio of reinforcement material on the performance of castables:

[0083] like Figure 1 , 2 As shown, by comparing Examples 1, 6, and 7, it can be seen that the castable prepared according to the method of Example 1 has the best comprehensive performance. It can be seen that the ratio of the reinforcement material can have a certain effect on the performance of the castable, but the effect is not obvious. The ratio of the reinforcement material will affect the compressive strength and weather resistance of the castable. The appropriate ratio can improve the comprehensive performance.

[0084] From the comparison between Example 1 and Control Example 2, it can be seen that the compressive strength performance of Example 1 is significantly better than that of Control Example 2, and the reinforcement material has a more obvious effect on the castable material.

[0085] 4. Explore the influence of the ratio of surface material on the performance of castables:

[0086] like Figure 1 , 2 As shown, by comparing Examples 1, 12, and 13, it can be seen that: the compressive strength of Examples 1, 12, and 13 are close, the castable prepared in Example 1 has the best weather resistance, and the ratio of the surface material has a certain influence on the performance of the castable, but the effect is not obvious; compared with Example 3, there is little difference in the compressive strength performance of Example 1, but the difference in durability is more obvious.

Claims

1. A method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler, characterized in that: The following steps are involved: S1. Mixed powder ingredients By mass percentage, 12-14% of barium sulfate powder, 10-12% of microsilicon powder, 3-8% of alloy fiber, 1-8% of zinc oxide powder, 3-5% of γ-alumina powder and the remainder of aluminum-chromium slag powder are mixed uniformly to obtain a mixed powder; S2. Preparation of splicing layer The size of the flue to be cast is measured, and several sheet molds matching the size are selected, wherein the thickness of the mold is 0.5 to 3 cm, and the mixed powder is introduced into the mold, and the mold is pressed and formed, and the mixture is kept at 1000 to 1800° C. for 0.5 to 1 hour. After cooling, a layer of polytetrafluoroethylene film is laid on the surface, and then a layer of basalt fiber cloth or aramid fiber cloth is laid on the polytetrafluoroethylene film, and then another layer of polytetrafluoroethylene film is laid, and finally a layer of mesh galvanized steel wire is evenly laid, and the mixture is kept at 90 to 110° C. for 12 to 24 hours, and the mold is demolded after cooling to obtain a splicing layer; the thickness of the two polytetrafluoroethylene films is 0.08 to 0.3 mm, the thickness of the basalt fiber cloth or aramid fiber cloth is 0.4 to 0.5 mm, and the average thickness of the mesh galvanized steel wire is 0.5 to 2.5 mm; S3. Preparation of reinforcement material By mass percentage, 15-25% of titanium carbide powder, 15-18% of biochar powder, 10-15% of perlite, 2-15% of fused magnesia powder, 8-14% of glass microspheres, 5-10% of polyacrylic acid microspheres, 2-7% of polyvinyl alcohol, 2-5% of sodium polyacrylate and the remainder of cement are added with an appropriate amount of water at 90-110° C. and mixed evenly to obtain a reinforcement material; S4. Preparation of anti-corrosion flue casting material S4-1, pre-treatment of glass flakes; S4-2, preparing surface material; S4-3, adjust the viscosity of the surface material, splice the splicing layer on the inner wall of the flue, then pour the reinforcement material, pour the surface material after drying, and combine the raw materials according to the above operations to obtain a flue castable that reduces gas corrosion.

2. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 1, characterized in that: S1 The particle size of the barium sulfate powder is 50-60 μm, the particle size of the microsilicon powder is 30-40 μm, the average length of the alloy fiber is 1-3 mm, the particle size of the zinc oxide powder is 20-40 μm, the particle size of the γ-alumina powder is 20-30 μm, and the particle size of the aluminum chromium slag powder is 0.2-5 mm.

3. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 1, characterized in that: The method for pretreating glass flakes described in S4-1 is: clean the glass flake raw materials with acetone with a mass concentration of 95-98% or alcohol with a mass concentration of 99-99.9%, polish the surface of the glass flakes, and then pickle them after drying.

4. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 3, characterized in that: The particle sizes of the glass flakes include 20 mesh, 60 mesh, and 110 mesh, and the mass ratios are 9 to 10:1:1 respectively.

5. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 1, characterized in that: The method for preparing the surface material described in S4-2 is: by mass percentage, 50-60% of the glass flakes pretreated by S4-1, 1-3% of the curing agent, 1-3% of the accelerator, 1-2% of the thixotropic stabilizer, 1-12% of the low shrinkage agent, 0.2-1.2% of the silane coupling agent, 0.2-1% of the defoaming agent, 0.1-3% of the nano-silica and the remainder of the vinyl ester resin are mixed evenly to obtain the surface material.

6. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 5, characterized in that: The curing agent is 328E; the accelerator is an organic tin compound and a tertiary amine compound; the thixotropic stabilizer is BYK-R605; the low shrinkage agent is polyamide; the defoaming agent is BYK-555; and the silane coupling agent is propyltrimethoxysilane.

7. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 1, characterized in that: S4-3 The method for adjusting the viscosity of the surface material is: during the stirring process, a proper amount of diluent or thickener is evenly added to adjust the pouring viscosity of the surface material to 0.5-1 Pa·s.

8. The method for preparing a flue castable for reducing gas corrosion in a fluidized bed boiler according to claim 7, characterized in that: The diluent is one or a combination of methanol, ethanol, acetone, methyl ethyl ketone, butyl ester, and ethyl acetate, and the thickener is one or a combination of fumed silica or bentonite.

Citation Information

Patent Citations

  • Refractory aggregate of long-life blast-furnace tapping sand hole

    CN104150919A

  • Impact-resistant high-temperature-resistant composite material seawater pipeline and forming method thereof

    CN116336265A

  • Refractory adhesive composition for repair and reinforcement

    KR101941677B1

  • Steel materials using ceramic composition and glass flake and ceramic coating material for concrete structure and coating method using thereof

    KR101954615B1

  • Ceramic fiber reinforced refractory

    US4558016A