Phosphorus-containing compound and manufacturing method thereof, resin composition and product thereof

By using a specially made polyphenylene ether resin composition with double bonds of phosphorus-containing compounds and unsaturated carbon-carbon in the circuit substrate material, the problem of insufficient performance of halogen-free circuit substrate materials in the prior art is solved, and high performance and environmental protection are achieved. It is suitable for semi-cured sheets, resin films, laminated boards and printed circuit boards.

CN118994237APending Publication Date: 2024-11-22ELITE ELECTRONIC MATERIAL (KUNSHAN) CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310572481.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing halogen-free circuit substrate materials are difficult to meet the requirements of excellent dielectricity, high tension to copper foil, high glass conversion temperature, low thermal expansion rate and excellent hygroscopic heat resistance, and traditional halogen-containing circuit substrates will be generated when they are abandoned and burned. Toxic and harmful substances lead to the dual challenges of environmental protection and high performance.

Method used

A phosphorus-containing compound is used, and its structure is obtained by a specific reaction of halogen benzocyclobutene format reagent and diallyl bisphenol. It combines with an unsaturated carbon-carbon double bond to perform prepolymerization reaction, forming an excellent A resin composition with comprehensive properties is used to prepare semi-cured sheets, resin films, laminated plates and printed circuit boards.

Benefits of technology

It achieves high glass conversion temperature, low dielectric loss, excellent flame retardant, low thermal expansion rate and high tension on copper foil, and is halogen-free flame retardant, avoiding the generation of toxic substances and meeting the dual requirements of environmental protection and high performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994237A_ABST
    Figure CN118994237A_ABST
Patent Text Reader

Abstract

The invention provides a phosphorus-containing compound with a structure shown in a formula (1), a resin composition containing the phosphorus-containing compound and a product prepared from the resin composition. The phosphorus-containing compound can meet the requirements of excellent dielectric property, high copper foil tension, high glass transition temperature, low thermal expansion rate, excellent moisture absorption and heat resistance and the like while realizing halogen-free flame retardance. The resin composition comprises the following components or prepolymers thereof: (A) 100 parts by weight of polyphenyl ether resin containing unsaturated carbon-carbon double bonds; (B) 15-90 parts by weight of a phosphorus-containing compound having a structure represented by formula (1); wherein the prepolymer is obtained by performing a prepolymerization reaction on a mixture, and the mixture at least comprises the component (A) and the component (B). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a phosphorus-containing compound and a method for producing the same, a resin composition and an article made from the resin composition, and in particular to a phosphorus-containing compound and a resin composition which can be applied to a prepreg, a resin film, a laminate and a printed circuit board. Background Art

[0002] In recent years, with the rapid development of 5G electronic information technology, the signal processing speed and transmission frequency of various electronic devices used in the communication field have increased significantly, the power of electronic devices has continued to increase, and their operating temperature has also continued to increase. In order to maintain the normal operation of electronic components, the circuit substrate must not only have excellent dielectric properties, but also have high reliability such as flame retardancy, high glass transition temperature, low thermal expansion coefficient and excellent moisture absorption and heat resistance.

[0003] Traditional circuit substrates mainly achieve flame retardancy by adding bromine-containing flame retardants to the main resin or by brominating the main resin. However, such electronic products containing bromine and other halogens will produce a large amount of toxic and harmful substances such as dioxins and hydrogen halides during their waste combustion. With the continuous improvement of people's environmental awareness, such halogen-containing circuit substrates are gradually being eliminated, and halogen-free circuit substrate materials have become a research hotspot in the industry. At present, the industry mainly achieves the purpose of halogen-free flame retardancy by adding phosphorus-containing compounds to resin compositions. However, there is no phosphorus-containing compound in the prior art that can achieve halogen-free flame retardancy while meeting the requirements of excellent dielectric properties, high tensile strength against copper foil, high glass transition temperature, low thermal expansion coefficient and excellent moisture absorption and heat resistance. Therefore, under the dual requirements of strict environmental protection and high performance, new halogen-free flame retardant materials with good comprehensive performance have become the direction of joint and active development in the industry. Summary of the invention

[0004] The present invention provides a phosphorus-containing compound capable of solving the above-mentioned problems, a method for producing the same, a resin composition containing the phosphorus-containing compound, and products such as a prepreg, a resin film, a laminate, and a printed circuit board made from the resin composition.

[0005] The phosphorus-containing compound of the present invention has a structure as shown in formula (1):

[0006]

[0007] In the structural formula (1), X is a covalent bond or a C1-C3 alkyl group,

[0008] R is independently a group represented by formula (2), formula (3) or formula (4),

[0009]

[0010] Among them, R1~R28 Each is independently a hydrogen atom or a C1-C3 alkyl group.

[0011] Preferably, the phosphorus-containing compound is any one of the phosphorus-containing compounds represented by the structures of formula (5) to formula (9).

[0012]

[0013] The method for producing the phosphorus-containing compound comprises the following steps:

[0014] Step (1): preparing a halogen benzocyclobutene Grignard reagent in a reaction vessel;

[0015] Step (2): In another reaction vessel, diallyl bisphenol is reacted with one or more compounds RH to obtain an intermediate product 1, wherein H in the compound RH represents a hydrogen atom, and R is a group represented by formula (2), formula (3) or formula (4).

[0016]

[0017] Among them, R1~R 28 Each is independently a hydrogen atom or a C1-C3 alkyl group;

[0018] Step (3): reacting the halogen benzocyclobutene Grignard reagent obtained in step (1) with the intermediate 1 to obtain a phosphorus-containing compound represented by formula (1).

[0019] In the method for producing a phosphorus-containing compound, the reaction temperature of step (1) is 0° C. to 100° C., the reaction time of step (1) is 1 to 10 hours, in step (2), RH is diphenylphosphine oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenyl phosphonate or bis(2,6-dimethylphenyl)phosphonate, and the molar ratio of RH to diallyl bisphenol is 2:1 to 3:1,

[0020] The reaction temperature of step (2) is 80° C. to 160° C., and the reaction time of step (2) is 1 to 6 hours.

[0021] The reaction temperature of step (3) is -20°C to 120°C, and the reaction time of step (3) is 3 to 30 hours.

[0022] The present invention also provides a resin composition comprising the following components or prepolymers thereof:

[0023] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds;

[0024] (B) 15 to 90 parts by weight of the phosphorus-containing compound of claim 1;

[0025] The prepolymer is obtained by prepolymerizing a mixture, and the mixture at least comprises the component (A) and the component (B).

[0026] Preferably, the component (A) includes any one of (meth)acryl polyphenylene ether resin, vinylbenzyl polyphenylene ether resin, vinyl polyphenylene ether resin, or a combination of two or more thereof.

[0027] Preferably, the phosphorus-containing compound comprises: any one or a combination of two or more of the phosphorus-containing compounds represented by formula (5) to formula (9).

[0028]

[0029] Preferably, the prepolymer is formed by a prepolymerization reaction of the component (A) and the component (B), and the conversion rate of the prepolymerization reaction is between 10% and 99%.

[0030] The resin composition may further include any one or a combination of two or more of a cross-linking agent containing unsaturated carbon-carbon double bonds, a silicone resin, a benzoxazine resin, an epoxy resin, a polyester resin, a phenolic resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, and a maleimide triazine resin.

[0031] The resin composition may further include any one or a combination of two or more of a hardening accelerator, a polymerization inhibitor, an inorganic filler, a surface treatment agent, a dye, and a solvent.

[0032] The present application provides a product made of the above resin composition, wherein the product includes a prepreg, a resin film, a laminate or a printed circuit board.

[0033] The product has one, more or all of the following characteristics:

[0034] The glass transition temperature measured by the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 240°C.

[0035] The dielectric constant Dk measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 3.20,

[0036] The dielectric loss Df measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.0020,

[0037] The flame retardancy measured according to the method described in UL94 is V0.

[0038] The Z-axis thermal expansion rate measured by the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.5%,

[0039] The products were tested for moisture absorption and heat resistance according to the methods of IPC-TM-650 2.6.16.1 and IPC-TM-650 2.4.23, and no board explosion occurred.

[0040] The copper foil tensile force measured in accordance with IPC-TM-650 2.4.8 is greater than or equal to 3.2 lb / in. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is the FTIR spectrum of P1 which is an example of the phosphorus-containing compound in Examples. DETAILED DESCRIPTION

[0042] In order to enable those skilled in the art to understand the characteristics and effects of the present application, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used herein have the common meanings understood by those skilled in the art for the present application. In case of conflict, the definitions in this specification shall prevail.

[0043] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present application in any way, that is, the content of the present application can be implemented without being limited by any specific theory or mechanism.

[0044] This document uses "one", "an", "a" or similar expressions to describe the components and technical features described in this application. Such description is only for the convenience of expression and to provide a general meaning to the scope of this application. Therefore, such description should be understood to include one or at least one, and the singular also includes the plural, unless it is obvious that it refers to another meaning.

[0045] As used herein, the terms "comprises," "includes," "has," "contains," or any other similar terms are open-ended transitional phrases, which are intended to cover non-exclusive inclusions. For example, a composition or article comprising a plurality of elements encompasses any one or any one of the listed elements, and is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or article. In addition, unless expressly stated to the contrary, the term "or" refers to an inclusive "or" rather than an exclusive "or." For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist). In addition, in this article, the terms "comprising", "including", "having", and "containing" should be interpreted as specifically disclosed and simultaneously covering closed conjunctions such as "consisting of", "consisting of", and "the remainder is", as well as open conjunctions such as "consisting essentially of", "mainly consisting of", "mainly consisting of", "basically containing", "essentially consisting of", "essentially consisting of", and "essentially containing".

[0046] As used herein, “or a combination thereof” means “or any combination thereof”, covering any combination of two or more of the listed elements; “any one”, “any one”, “any one” means “any one”, “any one”, “any one”. For example, “a composition or its product includes A, B, C or a combination thereof”, when interpreted, covers the following situations: A is true (or exists) and B and C are false (or do not exist), B is true (or exists) and A and C are false (or do not exist), C is true (or exists) and B and C are false (or do not exist), A and B are true (or exist) and C is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A, B and C are all true (or exist), and other elements not explicitly listed but that are typically inherent to the composition or its product.

[0047] In this article, all features or conditions defined in the form of numerical ranges or percentage ranges, such as numerical values, quantities, contents and concentrations, are only for simplicity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible sub-ranges and individual numerical values ​​(including integers and fractions) within the range, especially integer values. For example, the range description of "1.0 to 8.0" or "between 1.0 and 8.0" should be deemed to have specifically disclosed all sub-ranges such as 1.0 to 8.0, 1.0 to 7.0, 2.0 to 8.0, 2.0 to 6.0, 3.0 to 6.0, 4.0 to 8.0, 3.0 to 8.0, etc., and should be deemed to cover endpoint values, especially sub-ranges defined by integer values, and should be deemed to have specifically disclosed individual numerical values ​​such as 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, etc. Unless otherwise specified, the above-mentioned interpretation method is applicable to all contents of the full text of this application, regardless of whether the scope is extensive or not.

[0048] If the quantity, concentration or other numerical value or parameter is expressed as a range, a preferred range (or a better range) or a series of upper and lower limits, it should be understood that all ranges consisting of any pair of the upper limit or preferred value (or a better value) of the range and the lower limit or preferred value (or a better value) of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.

[0049] In this document, numerical values ​​should be understood to have the accuracy of the number of significant digits of the numerical value, provided that the purpose of the invention can be achieved. For example, the number 40.0 should be understood to cover the range of 39.50 to 40.49.

[0050] In this article, for the use of Markush groups or optional terms to describe the features or examples of the present application, those skilled in the art should understand that all subgroups or any individual elements in the Markush group or option list can also be used to describe the present application. For example, if X is described as "selected from the group consisting of X1, X2 and X3", it also means that the claim that X is X1 and the claim that X is X1 and / or X2 and / or X3 have been fully described. Furthermore, for the use of Markush groups or optional terms to describe the features or examples of the present application, those skilled in the art should understand that any combination of subgroups or individual members of all elements in the Markush group or option list can also be used to describe the present application. Accordingly, for example, if X is described as "selected from the group consisting of X1, X2 and X3", and Y is described as "selected from the group consisting of Y1, Y2 and Y3", it means that the claim that X is X1 and / or X2 and / or X3 and Y is Y1 and / or Y2 and / or Y3 has been fully described.

[0051] Unless otherwise specified, in this application, a compound refers to a chemical substance formed by two or more elements connected by chemical bonds, including small molecule compounds and polymer compounds, but not limited thereto. The interpretation of a compound in this article is not limited to a single chemical substance, but can also be interpreted as the same type of chemical substances with the same composition or the same properties.

[0052] If not otherwise specified, in the present invention, polymer refers to the product formed by the polymerization reaction of monomers, often including many polymer aggregates, each polymer is composed of many simple structural units repeatedly connected by covalent bonds, and the monomer is a compound of synthetic polymer. Polymers can include homopolymers, copolymers, prepolymers, etc., and are not limited to this. Homopolymers refer to polymers polymerized from a monomer. Copolymers include random copolymers (structures such as -AABABBBAAABBA-), alternating copolymers (structures such as -ABABABAB-), graft copolymers (structures such as -AA(A-BBBB)AA(A-BBBB)AAA-) and block copolymers (structures such as -AAAAA-BBBBBB-AAAAA-) and the like. For example, the styrene-butadiene copolymer described in the present invention, when interpreted, should be understood to include styrene-butadiene random copolymers, styrene-butadiene alternating copolymers, styrene-butadiene graft copolymers, styrene-butadiene block copolymers or combinations thereof. Prepolymer refers to a polymer with a lower molecular weight between the monomer and the final polymer, and the prepolymer contains reactive functional groups that can further undergo polymerization to obtain a fully cross-linked or hardened product with a higher molecular weight. Polymers of course include oligomers, but are not limited to them. Oligomers, also known as low polymers, are polymers composed of 2 to 20 repeating units, usually 2 to 5 repeating units.

[0053] Unless otherwise specified, the "resin" in this application is a customary name for a synthetic polymer, which may include monomers, polymers thereof, combinations of monomers, combinations of polymers thereof, or combinations of monomers and polymers thereof, etc., and is not limited thereto.

[0054] If not otherwise specified, in the present application, modified products include products after modification of reactive functional groups of each resin, products after prepolymerization of each resin with other resins, products after crosslinking of each resin with other resins, products after copolymerization of each resin with other resins, and the like.

[0055] If not otherwise specified, the unsaturated bonds described in the present application refer to reactive unsaturated bonds, such as but not limited to unsaturated double bonds that can undergo cross-linking reactions with other functional groups, such as but not limited to unsaturated carbon-carbon double bonds that can undergo cross-linking reactions with other functional groups.

[0056] The unsaturated carbon-carbon double bonds described in the present application preferably include, but are not limited to, vinyl, vinylbenzyl, (meth)acryloyl, allyl or a combination thereof. Vinyl should be interpreted to include vinyl and vinylidene. (Meth)acryloyl should be interpreted to include acryloyl and methacryloyl.

[0057] Unless otherwise specified, the alkyl, alkenyl, and monomer described in this application include their various isomers when interpreted. For example, propyl should be interpreted as including n-propyl and isopropyl.

[0058] Unless otherwise specified, in this application, parts by weight represent relative parts by weight in the composition, which may be any weight unit, such as but not limited to kilograms, kilograms, grams, pounds, etc. For example, 100 parts by weight of polyphenylene ether resin containing unsaturated carbon-carbon double bonds may represent 100 kilograms of polyphenylene ether resin containing unsaturated carbon-carbon double bonds or 100 pounds of polyphenylene ether resin containing unsaturated carbon-carbon double bonds.

[0059] It should be understood that the features disclosed in the various embodiments herein may be arbitrarily combined to form the technical solution of the present application, as long as there is no contradiction in the combination of these features.

[0060] The present application will be described below with specific embodiments and examples. It should be understood that these specific embodiments and examples are merely exemplary and are not intended to limit the scope of the present application and its use. The methods, reagents and conditions used in the examples are, unless otherwise stated, conventional methods, reagents and conditions in the art.

[0061] The present application discloses a phosphorus-containing compound, the structure of which is shown in formula (1):

[0062]

[0063] In the structural formula (1), X is a covalent bond or a C1-C3 alkyl group (such as methyl, ethyl or propyl), and R is independently a group represented by formula (2), formula (3) or formula (4).

[0064]

[0065] Among them, R1~R 28 Each is independently a hydrogen atom or a C1-C3 alkyl group (eg, methyl, ethyl or propyl).

[0066] In one embodiment, for example, the phosphorus-containing compound having the structure of formula (1) includes: any one or a combination of phosphorus-containing compounds having the structures of formula (5) to formula (9),

[0067]

[0068]

[0069] The phosphorus-containing compound having the structure of formula (1) described in the present application can be prepared by various methods known to those skilled in the art. For example, the phosphorus-containing compound represented by formula (1) may include the following steps:

[0070] Step (1): preparing a halogenated benzocyclobutene Grignard reagent in a reaction vessel, for example but not limited to adding magnesium powder, an organic solvent, elemental iodine and bromobenzocyclobutene into the reaction vessel to react and prepare a bromobenzocyclobutene Grignard reagent;

[0071] Step (2): In another reaction vessel, diallyl bisphenol is reacted with one or more compounds RH to obtain an intermediate product 1;

[0072] Step (3): reacting a halogen benzocyclobutene Grignard reagent with the intermediate 1 to obtain a phosphorus-containing compound represented by formula (1).

[0073] The organic solvent in step (1) includes but is not limited to anhydrous tetrahydrofuran.

[0074] The reaction temperature of step (1) is 0°C to 100°C.

[0075] The reaction time of step (1) is 1 to 10 hours.

[0076] In step (2), an organic solvent may be further added, including but not limited to toluene, xylene or a combination thereof.

[0077] In step (2), the definition of R in RH is the same as that of R in the above formula (1), H represents a hydrogen atom, and the RH includes but is not limited to diphenylphosphine oxide (DPO), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), diphenyl phosphonate or bis(2,6-dimethylphenyl)phosphonate. The molar ratio of the RH to diallyl bisphenol is 2:1 to 3:1.

[0078] The reaction temperature of step (2) is 80°C to 160°C.

[0079] The reaction time of step (2) is 1 to 6 hours.

[0080] The reaction temperature of step (3) is -20°C to 120°C.

[0081] The reaction time of step (3) is 3 to 30 hours.

[0082] The present application further discloses a resin composition comprising the following components or prepolymers thereof,

[0083] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds;

[0084] (B) 15 to 90 parts by weight of a phosphorus-containing compound represented by the above formula (1);

[0085] The prepolymer is obtained by prepolymerizing a mixture, and the mixture at least comprises the component (A) and the component (B).

[0086] In one embodiment, for example, compared to a total of 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the added amount of the phosphorus-containing compound having the structure represented by formula (1) can be 15, 25, 40, 50, 80, or 90 parts by weight, and is not limited thereto.

[0087] In another embodiment, for example, the resin composition includes a prepolymer, which is formed by prepolymerization of 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 15 to 90 parts by weight of the phosphorus-containing compound shown in formula (1). The prepolymer of the present invention contains residual unsaturated carbon-carbon double bonds, and the conversion rate of the reaction raw materials and the molecular weight of the prepolymer are both within a controllable range. In one embodiment, the residual unsaturated carbon-carbon double bonds in the prepolymer can react with other components (such as a cross-linking agent containing unsaturated carbon-carbon double bonds in the resin composition described herein), such as polymerization reaction or cross-linking reaction. In the present invention, the presence and content of the residual unsaturated carbon-carbon double bonds in the prepolymer are controlled by controlling the conversion rate of the phosphorus-containing compound shown in formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds. The conversion rate of the phosphorus-containing compound shown in formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds is controlled by means known in the art, such as a hardening accelerator and / or a molecular weight regulator, as well as reaction temperature and reaction time. For example, the conversion rate of the phosphorus-containing compound shown in formula (1) may be between 10% and 99%, preferably between 30% and 95%, between 50% and 95%, between 50% and 90%, or between 75% and 90%. For example, when the conversion rate of the phosphorus-containing compound shown in formula (1) is 0%, it means that the phosphorus-containing compound shown in formula (1) is completely unreacted and the prepolymer of the present invention cannot be formed. When the conversion rate of the phosphorus-containing compound shown in formula (1) is 100%, it means that the phosphorus-containing compound shown in formula (1) is completely reacted, and the prepolymer of the present invention cannot be formed at this time.

[0088] For example, the prepolymer disclosed in the present invention can be prepared by the following method: a mixture of at least 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 15 to 90 parts by weight of a phosphorus-containing compound represented by the formula (1) is subjected to a prepolymerization reaction under appropriate conditions. For example, the prepolymerization reaction can be carried out in the presence of a hardening accelerator and / or a molecular weight regulator. The types of hardening accelerators are described in detail later. In one or more embodiments, the molecular weight regulator includes: n-butyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, mercaptoethanol, 2,4-diphenyl-4-methyl-1-pentene, 4,4'-butylenebis(6-tert-butyl-3-methylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. The amount of the hardening accelerator and / or molecular weight regulator used in the present invention is not particularly limited, and can be 0.01 to 5 parts by weight, for example, 0.1 to 3 parts by weight, respectively, relative to 100 parts by weight of the total amount of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds and the phosphorus-containing compound shown in formula (1), and is not limited thereto. Usually, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the phosphorus-containing compound shown in formula (1) and the optional hardening accelerator and / or molecular weight regulator are dissolved in a solvent for prepolymerization. The solvent can be a solvent conventionally used in the art for the polymerization reaction between the monomer or oligomer containing unsaturated carbon-carbon double bonds and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, including but not limited to toluene. The temperature of the prepolymerization reaction is usually higher than room temperature, for example, between 50°C and 140°C, preferably between 80°C and 120°C. The reaction time is usually 0.5 to 6 hours, preferably 1 to 4 hours. The reaction is usually carried out under stirring conditions. Usually, before the reaction starts, the reaction temperature is first raised to above room temperature. After a period of reaction, the temperature is lowered to room temperature (about 25° C.) to obtain a solution, and a filter is used to filter out impurities in the solution. After the solution is purified, a prepolymer product is obtained, i.e., a prepolymer obtained by prepolymerizing the phosphorus-containing compound represented by formula (1) with a polyphenylene ether resin containing unsaturated carbon-carbon double bonds.

[0089] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds applicable to the present application is not particularly limited, and may be any one or more polyphenylene ether resin containing unsaturated carbon-carbon double bonds applicable to the production of prepregs, resin films, laminates or printed circuit boards, and may be any one or more commercially available products, homemade products or combinations thereof, such as but not limited to (meth)acryloyl polyphenylene ether resin, vinylbenzyl polyphenylene ether resin, vinyl polyphenylene ether resin or combinations thereof.

[0090] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds used in the present application all have unsaturated carbon-carbon double bonds and a phenylene ether skeleton, wherein the unsaturated carbon-carbon double bonds are reactive functional groups, which can self-polymerize after being heated, and can also undergo free radical polymerization with other unsaturated bond-containing components in the resin composition and finally cross-link and cure. The cured product has the characteristics of high heat resistance and low dielectric. Preferably, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes a polyphenylene ether resin containing unsaturated carbon-carbon double bonds substituted with 2,6-dimethyl on the phenylene ether skeleton, and the methyl groups after substitution form a steric hindrance so that the oxygen atoms on the ether are not easy to produce hydrogen bonds or van der Waals forces and absorb moisture, thereby having lower dielectric properties.

[0091] In certain embodiments, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes, but is not limited to, a (meth)acryl polyphenylene ether resin having a number average molecular weight of about 1900 to 2300 (e.g., SA9000, available from Sabic), a vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 1200 (e.g., OPE-2st 1200, available from Mitsubishi Gas Chemical), a vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 2200 (e.g., OPE-2st 2200, available from Mitsubishi Gas Chemical), a vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 2400 to 2800 (e.g., vinylbenzyl bisphenol A polyphenylene ether resin), a vinyl polyphenylene ether resin having a number average molecular weight of about 2200 to 3000, or a combination thereof. The vinyl polyphenylene ether resin may include various types of polyphenylene ether resins disclosed in U.S. Patent Application US20160185904A1, all of which are incorporated herein by reference. The vinylbenzyl polyphenylene ether resin includes, but is not limited to, vinylbenzyl biphenyl polyphenylene ether resin, vinylbenzyl bisphenol A polyphenylene ether resin or a combination thereof.

[0092] For example, in one embodiment, the resin composition of the present invention may further contain a cross-linking agent containing unsaturated carbon-carbon double bonds, a silicone resin, a benzoxazine resin, an epoxy resin, a polyester resin, a phenolic resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, a maleimide triazine resin or a combination thereof as needed.

[0093] In the present invention, for example, the cross-linking agent containing unsaturated carbon-carbon double bonds may be any cross-linking agent containing unsaturated carbon-carbon double bonds known in the art, and specific examples include bis(vinylphenyl)ethane, bisvinylbenzyl ether, divinylbenzene, divinylnaphthalene, divinylbiphenyl, tert-butylstyrene, triallyl isocyanurate, triallyl cyanurate, trivinylcyclohexane, diallylbisphenol A, styrene, butadiene, decadiene, octadiene, vinylcarbazole, acrylate or a combination thereof.

[0094] If not otherwise specified, the amount of the cross-linking agent containing unsaturated carbon-carbon double bonds used in the present invention can be adjusted as needed. For example, but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the cross-linking agent containing unsaturated carbon-carbon double bonds can be 1 to 20 parts by weight, for example, 1 part by weight, 5 parts by weight, 10 parts by weight, 15 parts by weight or 20 parts by weight.

[0095] In the present invention, for example, the silicone resin may be any type of silicone resin known in the art, and specific examples include but are not limited to polyalkyl silicone resin, polyaryl silicone resin, polyalkylaryl silicone resin, modified silicone resin or a combination thereof. Preferably, the silicone resin suitable for the present invention is an amino-modified silicone resin, such as, but not limited to, amino-modified silicone resins produced by Shin-Etsu Chemical Co., Ltd. under the trade names KF-8010, X-22-161A, X-22-161B, KF-8012, KF-8008, X-22-9409, X-22-1660B-3, etc., amino-modified silicone resins produced by Toray-Dow Corning Co., Ltd. under the trade names BY-16-853U, BY-16-853, BY-16-853B, etc., amino-modified silicone resins produced by Momentive Performance Materials JAPAN under the trade names XF42-C5742, XF42-C6252, XF42-C5379, etc., or combinations thereof.

[0096] If not otherwise specified, the amount of the silicone resin used in the present invention can be adjusted as needed. For example, but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the silicone resin can be 10 to 100 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight.

[0097] In the present invention, for example, the benzoxazine resin may be any type of benzoxazine resin known in the art. Specific examples include, but are not limited to, bisphenol A benzoxazine resin, bisphenol F benzoxazine resin, phenolphthalein benzoxazine resin, dicyclopentadiene benzoxazine resin, phosphorus-containing benzoxazine resin, diamino benzoxazine resin, and phenyl, vinyl or allyl modified benzoxazine resin. Suitable commercially available products include, for example, Huntsman sold under the trade names LZ-8270 (phenolphthalein benzoxazine resin), LZ-8298 (phenolphthalein benzoxazine resin), LZ-8280 (bisphenol F benzoxazine resin), LZ-8290 (bisphenol A benzoxazine resin), or sold under the trade names KZH-5031 (vinyl modified benzoxazine resin), KZH-5032 (phenyl modified benzoxazine resin) by Kolon Industries of Korea. The diaminobenzoxazine resin may be diaminodiphenylmethane benzoxazine resin, diaminodiphenyl ether benzoxazine resin, diaminodiphenyl sulfone benzoxazine resin, diaminodiphenyl sulfide benzoxazine resin or a combination thereof, and is not limited thereto.

[0098] If not otherwise specified, the amount of the benzoxazine resin used in the present invention can be adjusted as needed. For example, but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the benzoxazine resin can be 10 to 100 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight.

[0099] In the present invention, for example, the epoxy resin may be any epoxy resin known in the art. From the perspective of improving the heat resistance of the resin composition, the epoxy resin includes, but is not limited to, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol AD ​​epoxy resin, novolac epoxy resin, trifunctional epoxy resin, tetrafunctional epoxy resin, multifunctional novolac epoxy resin, dicyclopentadiene (DCPD) epoxy resin, phosphorus-containing epoxy resin, p-xylene epoxy resin, naphthalene epoxy resin (e.g., naphthol epoxy resin), benzofuran epoxy resin, isocyanate-modified epoxy resin, or a combination thereof. The novolac epoxy resin may be phenol novolac epoxy resin, bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, biphenyl novolac epoxy resin, phenol benzaldehyde epoxy resin, phenol aralkyl novolac epoxy resin or o-cresol novolac epoxy resin; the phosphorus-containing epoxy resin may be DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) epoxy resin, DOPO-HQ epoxy resin or a combination thereof.The DOPO epoxy resin may be selected from one or more of DOPO-containing phenol novolac epoxy resin, DOPO-containing o-cresol novolac epoxy resin and DOPO-containing bisphenol-A novolac epoxy resin; the DOPO-HQ epoxy resin may be selected from one or more of DOPO-HQ-containing phenol novolac epoxy resin, DOPO-HQ-containing o-cresol novolacepoxy resin and DOPO-HQ-containing bisphenol-A novolac epoxy resin, but is not limited thereto.

[0100] If not otherwise specified, the amount of epoxy resin used in the present invention can be adjusted as needed. For example, but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of epoxy resin can be 10 to 100 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight.

[0101] In the present invention, for example, the polyester resin may be various polyester resins known in the art. Specific examples include, but are not limited to, polyester resins containing dicyclopentadiene structures, polyester resins containing biphenyl structures, and polyester resins containing naphthalene ring structures. Specific examples include, but are not limited to, the trade names HPC-8000 or HPC-8150 sold by Dainippon Ink Chemical. If not specifically indicated, the amount of the polyester resin used in the present invention may be adjusted as needed, for example but not limited to, compared to 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the polyester resin may be 10 to 80 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, or 80 parts by weight.

[0102] In the present invention, for example, the phenol resin can be various phenol resins known in the art, and specific examples include but are not limited to phenolic resins or phenoxy resins, wherein the phenolic resin includes phenolic resin, o-methylphenolic resin, bisphenol A resin, naphthol resin, biphenyl resin and dicyclopentadiene resin, and is not limited thereto. If not specifically indicated, the amount of the phenolic resin used in the present invention can be adjusted as needed, for example but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the phenolic resin can be 10 to 80 parts by weight, such as 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight or 80 parts by weight.

[0103] In the present invention, for example, the amine curing agent can be various amine curing agents known in the art. Specific examples include but are not limited to at least one of diaminodiphenyl sulfone, diaminodiphenylmethane, diaminodiphenyl ether, diaminodiphenyl sulfide and dicyandiamide or a combination thereof. If not specifically indicated, the amount of the amine curing agent used in the present invention can be adjusted as needed, for example but not limited to, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of the amine curing agent can be 1 to 15 parts by weight, for example 1 part by weight, 4 parts by weight, 7.5 parts by weight, 12 parts by weight, or 15 parts by weight.

[0104] In the present invention, for example, the polyamide may be any polyamide known in the art, including but not limited to any commercially available polyamide resin products.

[0105] In the present invention, for example, the polyimide may be any polyimide known in the art, including but not limited to any commercially available polyimide resin products.

[0106] In the present invention, for example, the styrene maleic anhydride may be any type of styrene maleic anhydride known in the art, wherein the ratio of styrene (S) to maleic anhydride (MA) may be 1 / 1, 2 / 1, 3 / 1, 4 / 1, 6 / 1, 8 / 1 or 12 / 1. Specific examples include styrene maleic anhydride copolymers sold by Cray Valley under the trade names SMA-1000, SMA-2000, SMA-3000, EF-30, EF-40, EF-60 and EF-80, or styrene maleic anhydride copolymers sold by Polyscope under the trade names C400, C500, C700, C900, and the like, but are not limited thereto.

[0107] In the present invention, for example, the maleimide resin can be any maleimide resin known in the art. Specific examples include, but are not limited to, 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide (or oligomer of phenylmethane maleimide), bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, and bisphenol A diphenyl ether bismaleimide. bismaleimide), 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, N-2,3-xylylmaleimide, N-2,6-xylylmaleimide, N-phenylmaleimide, vinyl benzyl maleimide (VBM), maleimide containing biphenyl structure, maleimide resin containing aliphatic structure of 10 to 50 carbon atoms or combination thereof. Modifications of these components are also included in the interpretation. The modified material includes, but is not limited to, a prepolymer of a diallyl compound and a maleimide resin, a prepolymer of a diamine and a maleimide resin, a prepolymer of a multifunctional amine and a maleimide resin, a prepolymer of an acidic phenol compound and a maleimide resin, or a combination thereof.

[0108] For example, the maleimide resins include, but are not limited to, maleimide resins produced by Daiwakasei Industry with trade names such as BMI-1000, BMI-1000H, BMI-1100, BMI-1100H, BMI-2000, BMI-2300, BMI-3000, BMI-3000H, BMI-4000, BMI-5000, BMI-5100, BMI-TMH, BMI-7000 and BMI-7000H, or maleimide resins produced by KI Chemical Co., Ltd. with trade names such as BMI-70 and BMI-80, or maleimide resins produced by Nippon Kayaku Co., Ltd. with trade names such as MIR-3000 and MIR-5000.

[0109] For example, maleimide resins containing an aliphatic structure of 10 to 50 carbon atoms, or maleimide resins extended by imide, may include various types of maleimide resins extended by imide disclosed in Taiwan Patent Application Publication No. TW200508284A, which is incorporated herein by reference in its entirety. Maleimide resins containing aliphatic long chain structures suitable for the present application include, but are not limited to, maleimide resins produced by designer molecular companies under the trade names of BMI-689, BMI-1400, BMI-1500, BMI-1700, BMI-2500, BMI-3000, BMI-5000 and BMI-6000.

[0110] In the present invention, for example, the cyanate resin may be various types of cyanate resins known in the art. For example, a compound having an Ar-OC≡N structure, wherein Ar may be a substituted or unsubstituted aromatic group. From the perspective of improving the heat resistance of the resin composition, specific examples of cyanate resins include, but are not limited to, phenolic cyanate resins, bisphenol A cyanate resins, bisphenol F cyanate resins, cyanate resins containing dicyclopentadiene structures, cyanate resins containing naphthalene ring structures, phenolphthalein cyanate resins, adamantane cyanate resins, fluorene cyanate resins, or a combination thereof. Among them, the phenolic cyanate resin may be a bisphenol A phenolic cyanate resin, a bisphenol F phenolic cyanate resin, or a combination thereof. For example, the cyanate resin may be a cyanate resin produced by Lonza under the trade names of Primaset PT-15, PT-30S, PT-60S, BA-200, BA-230S, BA-3000S, BTP-2500, BTP-6020S, DT-4000, DT-7000, ULL950S, HTL-300, CE-320, LVT-50, LeCy, etc.

[0111] For example, if not specifically specified, the maleimide triazine resin used in the present invention is not particularly limited, and can be any one or more maleimide triazine resins suitable for the production of prepregs, resin films, laminates or printed circuit boards. For example, the maleimide triazine resin can be obtained by polymerizing the aforementioned cyanate resin and the aforementioned maleimide resin. The maleimide triazine resin can be, for example but not limited to, a bisphenol A type cyanate resin and a maleimide resin polymerized, a bisphenol F type cyanate resin and a maleimide resin polymerized, a phenol novolac type cyanate resin and a maleimide resin polymerized, or a cyanate resin containing a dicyclopentadiene structure and a maleimide resin polymerized. For example, the maleimide triazine resin can be obtained by polymerizing a cyanate resin and a maleimide resin in any molar ratio. For example, relative to 1 mole of maleimide resin, the cyanate resin can be 1 to 10 moles. For example, but not limited to, the amount of the cyanate resin is 1, 2, 4 or 6 moles relative to 1 mole of the maleimide resin.

[0112] In addition to the aforementioned components, the resin composition of the present invention may further include a hardening accelerator, a polymerization inhibitor, an inorganic filler, a surface treatment agent, a coloring agent, a solvent or a combination thereof as required.

[0113] For example, the hardening accelerator may include a catalyst such as a Lewis base or a Lewis acid. The Lewis base may include one or more of imidazole, boron trifluoride amine complex, ethyltriphenylphosphonium chloride, 2-methylimidazole (2MI), 2-phenyl-1H-imidazole (2PZ), 2-ethyl-4-methylimidazole (2E4MI), triphenylphosphine (TPP) and 4-dimethylaminopyridine (DMAP). The Lewis acid may include a metal salt compound such as a metal salt compound of manganese, iron, cobalt, nickel, copper, zinc, etc., such as a metal catalyst such as zinc octoate and cobalt octoate. The hardening accelerator also includes a hardening initiator, such as a peroxide that can generate free radicals, including but not limited to: diisopropylbenzene peroxide, tert-butyl peroxybenzoate, dibenzoyl peroxide (BPO), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (25B) and bis(tert-butylperoxyisopropyl)benzene or a combination thereof. For example, in one embodiment, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.1 to 5 parts by weight of the hardening accelerator, preferably 0.1 to 4 parts by weight of the hardening accelerator, and more preferably 0.1 to 3.0 parts by weight of the hardening accelerator, but the present invention is not limited thereto.

[0114] For example, the above-mentioned inhibitor may include, but is not limited to, 1,1-diphenyl-2-trinitrophenylhydrazine, methacrylonitrile, 2,2,6,6-tetramethyl-1-oxy-piperidine, dithioester, nitrogen oxide stable free radical, triphenylmethyl free radical, metal ion free radical, sulfur free radical, hydroquinone, p-methoxyphenol, p-benzoquinone, phenothiazine, β-phenylnaphthylamine, p-tert-butylcatechol, methylene blue, 4,4'-butylenebis(6-tert-butyl-3-methylphenol) and 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. For example, the above-mentioned nitrogen oxide stable free radical may include, but is not limited to, nitrogen oxide free radicals from cyclic hydroxylamines such as 2,2,6,6-substituted-1-piperidinyloxy free radical or 2,2,5,5-substituted-1-pyrrolidinyloxy free radical. As a substituent, an alkyl group with a carbon number of less than four, such as methyl or ethyl, is preferred. Specific nitrogen oxide free radical compounds are not limited, and examples include but are not limited to 2,2,6,6-tetramethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetraethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetramethyl-4-oxo-1-piperidinyloxy free radicals, 2,2,5,5-tetramethyl-1-pyrrolidinyloxy free radicals, 1,1,3,3-tetramethyl-2-isoindolinyloxy free radicals, N,N-di-tert-butylamineoxy free radicals, etc. Stable free radicals such as galvinoxyl free radicals can also be used to replace nitrogen oxide free radicals. The inhibitor suitable for the resin composition of the present invention can also be a product derived from the hydrogen atom or atomic group in the inhibitor being replaced by other atoms or atomic groups. For example, the hydrogen atom in the inhibitor is replaced by an atomic group such as an amino group, a hydroxyl group, a ketocarbonyl group, etc. For example, in one embodiment, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a polymerization inhibitor, preferably 0.01 to 10 parts by weight of a polymerization inhibitor, but not limited thereto.

[0115] For example, the inorganic filler can be any one or more inorganic fillers suitable for the production of prepregs, resin films, laminates or printed circuit boards, and specific examples include but are not limited to: silicon dioxide (molten, non-molten, porous or hollow), aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, calcium carbonate, aluminum nitride, boron nitride, aluminum silicon carbide, silicon carbide, titanium dioxide, barium titanate, lead titanate, strontium titanate, calcium titanate, magnesium titanate, barium zirconate, lead zirconate, magnesium zirconate, lead zirconate titanate, zinc molybdate, calcium molybdate, magnesium molybdate, ammonium molybdate, zinc molybdate modified talc, zinc oxide, zirconium oxide, mica, boehmite (boehmite, AlOOH), calcined talc, talc, silicon nitride, zirconium tungstate, petalite, calcined kaolin or a combination thereof. In addition, the inorganic filler can be spherical, fibrous, plate-like, granular, flaky or needle-like, and can be selectively pretreated with a silane coupling agent. For example, in one embodiment, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 10 to 300 parts by weight of an inorganic filler, preferably 30 to 250 parts by weight of an inorganic filler, and more preferably 60 to 200 parts by weight of an inorganic filler, but not limited thereto.

[0116] For example, the type of the surface treatment agent is not particularly limited. The main function of adding the surface treatment agent in the present application is to make the inorganic filler uniformly dispersed in the resin composition.

[0117] For example, the coloring agent may include but is not limited to dye or pigment.

[0118] For example, the solvent suitable for the resin composition of the present invention is not particularly limited, and can be any solvent suitable for dissolving the resin composition of the present invention, including but not limited to: methanol, ethanol, ethylene glycol monomethyl ether, acetone, butanone (also known as methyl ethyl ketone), methyl isobutyl ketone, cyclohexanone, toluene, xylene, methoxyethyl acetate, ethoxyethyl acetate, propoxyethyl acetate, ethyl acetate, dimethylformamide, dimethylacetamide, propylene glycol methyl ether acetate and the like solvents or mixed solvents thereof. The amount of solvent added is for the purpose of adjusting the overall solid content of the resin composition to a suitable range. For example, in one embodiment, the amount of solvent added is added to adjust the overall solid content of the resin composition to 50-85%, but is not limited thereto.

[0119] The resin compositions of the aforementioned embodiments can be made into various products, such as components suitable for various electronic products, including but not limited to prepregs, resin films, laminates or printed circuit boards.

[0120] For example, the resin composition of each embodiment of the present invention can be made into a semi-cured sheet, which includes a reinforcing material and a layered object arranged on the reinforcing material. The layered object is obtained by heating the aforementioned resin composition at a high temperature to form a semi-cured state (B-stage). The baking temperature for making the semi-cured sheet is between 120°C and 180°C, preferably between 120°C and 160°C. The reinforcing material can be any one of a fiber material, a woven fabric, and a non-woven fabric, and the woven fabric preferably includes a glass fiber cloth. The type of glass fiber cloth is not particularly limited, and can be various glass fiber cloths that can be used for printed circuit boards, such as E-type glass cloth, D-type glass cloth, S-type glass cloth, T-type glass cloth, L-type glass cloth, Q-type glass cloth or QL-type glass cloth (a glass cloth of a mixed structure made of Q glass and L glass); the types of glass fibers include yarns and rovings, etc., and the forms include open fiber or unopen fiber, and the end face shape includes a circular or flat shape. The aforementioned non-woven fabric preferably includes a liquid crystal resin non-woven fabric, such as a polyester non-woven fabric, a polyurethane non-woven fabric, etc., and is not limited thereto. The aforementioned fabric may also include a liquid crystal resin fabric, such as a polyester fabric or a polyurethane fabric, etc., and is not limited thereto. This reinforcing material can increase the mechanical strength of the prepreg. In a preferred embodiment, the reinforcing material can also be selectively pretreated with a silane coupling agent. The prepreg is subsequently heated and cured (C-stage) to form an insulating layer.

[0121] For example, the resin composition of each embodiment of the present invention can be made into a resin film, which is obtained by semi-curing the aforementioned resin composition after baking and heating. The resin composition can be selectively coated on a polyethylene terephthalate film (PET film), a polyimide film (PI film), a copper foil or a copper foil with adhesive, and then semi-cured after baking and heating, so that the resin composition forms a resin film.

[0122] For example, the resin composition described in the present application can be made into various laminates, which include at least two metal foils and at least one insulating layer, wherein the insulating layer is disposed between the two metal foils, and the insulating layer can be formed by curing the aforementioned resin composition under high temperature and high pressure (C-stage), and the applicable curing temperature is, for example, between 190°C and 220°C, preferably between 200°C and 210°C, and the curing time is 90 to 180 minutes, preferably 120 to 150 minutes. The aforementioned insulating layer can be obtained by curing the aforementioned semi-cured sheet or resin film. The material of the aforementioned metal foil can be copper, aluminum, nickel, platinum, silver, gold or their alloys, such as copper foil. In a preferred embodiment, the laminate is a copper foil substrate.

[0123] In one embodiment, the aforementioned laminate can be further processed into a printed circuit board.

[0124] One of the methods for making the printed circuit board of the present application can be to use a double-sided copper foil substrate (for example, product EM-827, which can be purchased from Taiwan Optoelectronics Materials) with a thickness of 28 mils and 1 ounce of HTE (High Temperature Elongation) copper foil, and then electroplating after drilling to form electrical conduction between the upper copper foil and the bottom copper foil. Then etch the upper copper foil and the bottom copper foil to form an inner layer circuit. Then the inner layer circuit is browned and roughened to form a concave-convex structure on the surface to increase the roughness. Then, the copper foil, the aforementioned prepreg, the aforementioned inner layer circuit board, the aforementioned prepreg, and the copper foil are stacked in sequence, and then a vacuum laminating device is used to heat for 90 to 180 minutes at a temperature of 190°C to 220°C to cure the insulating layer material of the prepreg. Then, various circuit board processes known in the art such as blackening, drilling, and copper plating are performed on the copper foil on the outermost surface to obtain a printed circuit board.

[0125] In one or more embodiments, the resin composition disclosed in the present application and various products prepared therefrom preferably have one, more or all of the following characteristics:

[0126] The glass transition temperature measured according to the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 240°C, for example, between 240°C and 277°C.

[0127] The dielectric constant Dk measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 3.20, for example, between 3.05 and 3.20.

[0128] The dielectric loss Df measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.0020, for example, between 0.0017 and 0.0020.

[0129] The flame retardancy measured according to the method described in UL94 is V0.

[0130] The Z-axis thermal expansion rate measured according to the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.5%, for example, between 0.6% and 1.5%.

[0131] The product was tested for moisture absorption and heat resistance according to the methods of IPC-TM-650 2.6.16.1 and IPC-TM-650 2.4.23, and no panel explosion occurred.

[0132] The tensile force on the copper foil measured by the method described in IPC-TM-650 2.4.8 is greater than or equal to 3.2 lb / in, for example, between 3.2 lb / in and 4.7 lb / in.

[0133] In the present application, the characteristic tests of the embodiments and comparative examples are performed by making the objects to be tested (samples) in the following manner and then performing the tests according to specific test conditions.

[0134] 1. Prepreg: The resin compositions in the embodiments or comparative examples are respectively selected and uniformly mixed to form a varnish, which is placed in an impregnation tank. A glass fiber cloth (e.g., L-glass fiber cloth with a specification of 2116, or L-glass fiber cloth with a specification of 1080, or L-glass fiber cloth with a specification of 1078, all purchased from Asahi Co., Ltd.) is then immersed in the impregnation tank to adhere the resin composition to the glass fiber cloth, and the mixture is heated at 150° C. to 170° C. to a semi-cured state (B-Stage), thereby obtaining a prepreg with a resin content of 53%.

[0135] 2. Copper foil substrate (8-ply, 8 prepregs pressed together): 2 ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and 8 2116 L-glass fiber cloths were prepared to impregnate the prepregs made from each sample to be tested (each group of embodiments or comparative examples). The resin content of each prepreg was about 53%. One HVLP copper foil, eight prepregs and one HVLP copper foil were stacked in the order of one HVLP copper foil, eight prepregs and one HVLP copper foil, and pressed together for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper foil substrate. Among them, the 8 stacked prepregs were cured to form an insulating layer between the two copper foils, and the resin content of the insulating layer was about 53%.

[0136] 3. Copper-free substrate (8-ply, formed by pressing together 8 prepregs): The above copper foil substrate (8-ply) is etched to remove 2 copper foils to obtain a copper-free substrate (8-ply). The copper-free substrate is formed by pressing together 8 prepregs, and the resin content of the copper-free substrate is about 53%.

[0137] 4. Copper-free substrate (2-ply, formed by laminating two prepregs): prepare two ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and two 1080 L-glass fiber cloths to impregnate the prepregs made from each sample to be tested (each group of embodiments or comparative examples), and stack them in the order of copper foil, two prepregs, and copper foil, and press them for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper-containing substrate (2-ply, formed by laminating two prepregs). Then, the copper-containing substrate (2-ply) is etched to remove the copper foils on both sides to obtain a copper-free substrate (2-ply), which is formed by laminating two prepregs, and the resin content of the copper-free substrate (2-ply) is about 70%.

[0138] The descriptions of each test method and its characteristic analysis items are as follows:

[0139] 1. Glass transition temperature (Tg)

[0140] The aforementioned copper-free substrate (8-ply) was selected as the sample to be tested, and the glass transition temperature of each sample to be tested was measured by a dynamic mechanical analyzer (DMA) with reference to the method described in IPC-TM-650 2.4.24.4, in degrees Celsius. The measuring temperature range was 50-400 degrees Celsius, and the temperature rise rate was 2 degrees Celsius / minute. The higher the glass transition temperature, the better.

[0141] 2. Dielectric constant (Dk) and dielectric loss factor (Df)

[0142] The aforementioned copper-free substrate (2-ply) was selected as the sample to be tested, and a microwave dielectric analyzer (microwave dielectrometer, purchased from AET, Japan) was used to measure each sample at room temperature (about 25°C) and at a frequency of 10 GHz, referring to the method described in JIS C2565. The lower the dielectric constant and dielectric loss, the better the dielectric properties of the sample to be tested. At a measurement frequency of 10 GHz and a range where the Df value is less than 0.005, a difference in the Df value greater than or equal to 0.0001 indicates that there is a significant difference in the dielectric loss of different substrates (there is a significant technical difficulty).

[0143] 3. Flame retardancy

[0144] The aforementioned copper-free substrate (8-ply) (125mm×13mm) was selected as the sample to be tested and measured according to the method described in UL94. The flame retardancy analysis results were expressed in V0, V1, and V2 grades, among which V0 flame retardancy was better than V1 flame retardancy, V1 flame retardancy was better than V2 flame retardancy, and the sample burnout was the worst.

[0145] 4. Percent thermal expansion, z-axis, Z-PTE

[0146] The aforementioned copper-free substrate (8-ply) was selected as the sample to be tested for thermal mechanical analysis (TMA). The sample was heated at a temperature rise rate of 10°C / min from 50°C to 260°C, and the Z-axis thermal expansion coefficient (in %) of each sample to be tested within the temperature range of 50°C to 260°C was measured with reference to the method described in IPC-TM-6502.4.24.5. The lower the Z-axis thermal expansion coefficient, the better. For copper foil substrates with a Z-axis thermal expansion coefficient of less than 2.0%, a difference in the Z-axis thermal expansion coefficient greater than or equal to 0.1% is considered to be significantly different.

[0147] 5. Pressure cooking test (PCT)

[0148] The aforementioned copper-free substrate (8-ply) was selected, and the pressure cooking test was performed for 3 hours of moisture absorption (test temperature 121°C and relative humidity 100%) according to the method described in IPC-TM-650 2.6.16.1, and then immersed in a tin furnace at a constant temperature of 288°C according to the method described in IPC-TM-650 2.4.23, and taken out after immersion for 20 seconds to observe whether there was a burst board (a burst board means failure, and a non-blow board means passing the test, O represents a test without a burst board, and X represents a test with a burst board phenomenon), and 3 samples were tested in each group. One X means that one sample burst board appeared in three PCT tests, two Xs represent that two samples burst board appeared in three PCT tests, and three Xs represent that three samples burst board appeared in three PCT tests. For example, interlayer delamination between insulating layers can be called a burst board. Interlayer delamination refers to the phenomenon of bubbling separation between any layers of the substrate.

[0149] 6. Copper foil pulling force (peeling strength, P / S)

[0150] The aforementioned copper foil substrate (8-ply) was cut into rectangular samples with a width of 24 mm and a length greater than 60 mm, and the surface copper foil was etched to leave only a long strip of copper foil with a width of 3.18 mm and a length greater than 60 mm. The strength required to pull the copper foil away from the surface of the substrate insulation layer was measured using a universal tensile strength tester at room temperature (about 25°C) according to the method described in IPC-TM-650 2.4.8, and the unit was lb / in.

[0151] The resin compositions of the embodiments of the present invention and the comparative examples of the present invention were prepared using various raw materials from the following sources according to the amounts shown in Tables 1 to 3, and were further prepared into various test samples.

[0152] The chemical raw materials used in the embodiments and comparative examples of the present invention are as follows:

[0153] Phosphorus-containing compounds P1 to P5 having the structure of formula (1) are self-made and described in detail below.

[0154] Prepolymers Y1 to Y3: homemade, detailed as follows.

[0155] Compound V1: Homemade, as described below.

[0156] Compound D1, with the following structural formula, was prepared in-house:

[0157]

[0158] Compound D2, with the following structural formula, was prepared in-house:

[0159]

[0160] Compound D3, with the following structural formula, was prepared in-house:

[0161]

[0162] Compound D4, with the following structural formula, was prepared in-house:

[0163]

[0164] SA9000: (meth)acryl polyphenylene ether resin, purchased from Sabic, Mn is about 1900-2300.

[0165] OPE-2st 1200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical, Mn is about 1200.

[0166] OPE-2st 2200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical, Mn is about 2200.

[0167] DABPA: diallyl bisphenol A, purchased from Laizhou Laiyu Chemical Co., Ltd.

[0168] 4-Bromobenzocyclobutene: purchased from Shanghai Haohong Biopharmaceutical Technology Co., Ltd.

[0169] DPO: diphenylphosphine oxide, purchased from Beijing Bailingwei Technology Co., Ltd.

[0170] DVB: divinylbenzene, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.

[0171] BVPE: bis(vinylphenyl)ethane, purchased from Linchuan Chemical.

[0172] 25B: 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, purchased from NOF Corporation.

[0173] SC-2500SVJ: spherical silica with the surface treated with a silane coupling agent, purchased from Admatechs.

[0174] Toluene: purchased from Sinopec. The content is expressed as "appropriate amount", which means that the content of toluene is adjusted to the overall solid content of the resin composition of 60% to 68% (solid content, S / C = 60% to 68%).

[0175] Preparation Example 1: Phosphorus-containing compound P1

[0176] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0177] S2. Under nitrogen protection, add 30.8 g (0.1 mol) of DABPA, 40.4 g (0.2 mol) of DPO and 50 ml of xylene to another 1000 ml three-necked flask, stir and react at 140°C for 4 hours to obtain an intermediate product solution, cool to room temperature, slowly add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 dropwise under ice-water bath conditions, and complete the addition in about 2 hours. After the addition is completed, stir and react for 8 hours, then raise the temperature to 40°C and stir and react for 2 hours. The product is distilled under reduced pressure, washed, filtered and dried to obtain the final product P1, as shown in formula (5).

[0178]

[0179] The product P1 obtained in Preparation Example 1 was analyzed by Fourier transform infrared spectroscopy (FTIR). Figure 1 As shown in the figure, it can be seen that 2961.5cm -1 、2925.2cm -1 The CH stretching vibration peak on the methyl and methylene groups is 949 cm -1 、1185cm -1 The 949cm-1 and 959cm-2 correspond to the characteristic absorption peaks of the PH bond and P=O bond in DPO. After the addition reaction between DPO and DABPA, the PH bond disappears and the PC bond is generated. -1 The characteristic peak at 1172.7 cm disappeared, and the characteristic peak of P=O moved to 1172.7 cm -1 , 3445cm -1 The OH stretching vibration absorption peak on DABPA is at 1266.4 cm. After the reaction of 4-bromobenzocyclobutene with DABPA, the peak disappears completely and a peak at 1266.4 cm appears. -1 The stretching vibration peak of aromatic ether bond at 2829cm -1 The methylene CH stretching vibration peak on the benzocyclobutene four-membered ring is 1400-1500 cm -1 The characteristic absorption peaks of benzene ring are at 1437.5cm -1 The characteristic absorption peak of the benzene ring in the DPO structure is 1474.3 cm -1 The peak at the center is the characteristic absorption peak of the benzene ring of the benzocyclobutene structure, proving that the phosphorus-containing compound P1 was successfully synthesized.

[0180] Preparation Example 2: Phosphorus-containing compound P2

[0181] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0182] S2. Under nitrogen protection, add 30.8 g (0.1 mol) of DABPA, 43.2 g (0.2 mol) of DOPO and 50 ml of xylene to another 1000 ml three-necked flask, stir and react at 145°C for 4.5 hours to obtain an intermediate product solution, cool to room temperature, slowly add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 dropwise under ice-water bath conditions, and complete the addition in about 2 hours. After the addition is completed, stir and react for 8 hours, then raise the temperature to 40°C and stir and react for 3 hours. The product is distilled under reduced pressure, washed, filtered and dried to obtain the final product P2, as shown in formula (6).

[0183]

[0184] Preparation Example 3: Phosphorus-containing compound P3

[0185] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0186] S2. Under nitrogen protection, add 30.8 g (0.1 mol) of DABPA, 46.8 g (0.2 mol) of diphenyl phosphonate and 50 ml of xylene to another 1000 ml three-necked flask, stir and react at 150°C for 4 hours to obtain an intermediate product solution, cool to room temperature, slowly add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 dropwise under ice-water bath conditions, and complete the addition in about 2 hours. After the addition is completed, stir and react for 8 hours, then raise the temperature to 45°C and stir and react for 3 hours. The product is distilled under reduced pressure, washed, filtered and dried to obtain the final product P3, as shown in formula (7).

[0187]

[0188] Preparation Example 4: Phosphorus-containing compound P4

[0189] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0190] S2. Under nitrogen protection, add 30.8 g (0.1 mol) of DABPA, 58.1 g (0.2 mol) of bis(2,6-dimethylphenyl)phosphonate and 50 ml of xylene to another 1000 ml three-necked flask, stir and react at 150°C for 4 hours to obtain an intermediate product solution, cool to room temperature, slowly dropwise add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 under ice-water bath conditions, and complete the dropwise addition in about 2 hours. After the dropwise addition is completed, stir and react for 10 hours, then raise the temperature to 55°C and stir and react for 3 hours. The product is subjected to reduced pressure distillation, washing, filtering and drying to obtain the final product P4, as shown in formula (8).

[0191]

[0192] Preparation Example 5: Phosphorus-containing compound P5

[0193] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0194] S2. Under nitrogen protection, add 26.6 g (0.1 mol) of 5',5-diallyl-2,2'-biphenol, 40.4 g (0.2 mol) of DPO and 50 ml of xylene to another 1000 ml three-necked flask, stir and react at 140°C for 4.5 hours to obtain an intermediate product solution, cool to room temperature, and slowly dropwise add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 under ice-water bath conditions. The addition takes about 2 hours. After the addition is completed, stir and react for 10 hours, then raise the temperature to 50°C and stir and react for 4 hours. The product is distilled under reduced pressure, washed, filtered and dried to obtain the final product P5, as shown in formula (9).

[0195]

[0196] Preparation Example 6: Prepolymer Y1

[0197] Add 100 parts by weight of SA9000, 15 parts by weight of P1 and 110 parts by weight of toluene to a Schlenk reaction bottle, add 1 part by weight of hardening accelerator 25B after uniform dissolution, evacuate under liquid nitrogen environment, pass nitrogen, repeat the above steps three times to discharge oxygen in the system, heat to 120°C, react for 2 hours, cool down, filter and purify to obtain a homemade prepolymer Y1 with a solid content of 100%, and the conversion rate of the homemade prepolymer Y1 is between 10% and 99%.

[0198] Preparation Example 7: Prepolymer Y2

[0199] To a Schlenk reaction flask, 60 parts by weight of SA9000, 10 parts by weight of OPE-2st 1200, 30 parts by weight of OPE-2st2200, 20 parts by weight of P1, 10 parts by weight of P2, 10 parts by weight of P3, 10 parts by weight of P4 and 110 parts by weight of toluene were added, and after uniform dissolution, 0.1 parts by weight of hardening accelerator 25B was added. Vacuum was evacuated under a liquid nitrogen environment, and nitrogen was passed through. The above steps were repeated three times to discharge oxygen in the system. The temperature was raised to 120° C., and the reaction was carried out for 2 hours. After cooling, filtration and purification were performed, a self-made prepolymer Y2 was obtained, and the solid content was 100%. The conversion rate of the self-made prepolymer Y2 was between 10% and 99%.

[0200] Preparation Example 8: Prepolymer Y3

[0201] Add 100 parts by weight of SA9000, 90 parts by weight of P1 and 110 parts by weight of toluene to a Schlenk reaction bottle, add 3 parts by weight of hardening accelerator 25B after uniform dissolution, evacuate under liquid nitrogen environment, pass nitrogen, repeat the above steps three times to discharge oxygen in the system, heat to 120°C, react for 2 hours, cool down, filter and purify to obtain a self-made prepolymer Y3 with a solid content of 100%, and the conversion rate of the self-made prepolymer Y3 is between 10% and 99%.

[0202] Preparation Example 9: Compound V1

[0203] S1. Under nitrogen protection, add 6 g (0.25 mol) of magnesium powder, 500 ml of anhydrous tetrahydrofuran and 0.1 g of elemental iodine into a 1000 ml three-necked flask, add 36.6 g (0.2 mol) of 4-bromobenzocyclobutene dropwise while slowly stirring, heat to 80°C, reflux and stir for 2 hours to obtain 4-bromobenzocyclobutene Grignard reagent.

[0204] S2. Under nitrogen protection, add 30.8 g (0.1 mol) of DABPA to another 1000 ml three-necked flask, and slowly dropwise add the 4-bromobenzocyclobutene Grignard reagent prepared in step 1 under ice-water bath conditions. The addition takes about 2 hours. After the addition is completed, stir and react for 8 hours, then raise the temperature to 40°C and stir and react for 2 hours. The product is distilled under reduced pressure, washed, filtered and dried to obtain the final product V1.

[0205]

[0206] The resin composition compositions of the embodiments and comparative examples (all in parts by weight) and the test results of the sample properties are shown in Tables 1 to 3:

[0207] Table 1 Composition of the resin composition of Examples E1 to E7 (unit: parts by weight) and test results of properties of their products

[0208]

[0209] Table 2 Composition of the resin composition of Examples E8 to E13 (unit: parts by weight) and test results of properties of their products

[0210]

[0211] Table 3 Compositions of the resin compositions of Comparative Examples C1 to C7 (unit: parts by weight) and test results of properties of their products

[0212]

[0213] From Table 1 to Table 3, we can see that:

[0214] 1. Examples E1 to E10 use a phosphorus-containing compound having a structure of formula (1), and E11 to E13 use a prepolymer of the present application. Compared with Comparative Example C1 which does not contain a phosphorus-containing compound having a structure of formula (1) or a prepolymer of the present application, the following properties are significantly improved: Tg, Dk, Df, flame retardancy, Z-PTE and PCT. Among them, the Tg of the comparative example C1 sample is 205°C, while the Tg of the samples of embodiments E1 to E13 are all greater than or equal to 240°C; the Dk of the comparative example C1 sample is 3.30, while the Dk of the samples of embodiments E1 to E13 are all less than or equal to 3.20; the Df of the comparative example C1 sample is 0.0023, while the Df of the samples of embodiments E1 to E13 are all less than or equal to 0.0020; the flame retardancy of the comparative example C1 sample is V2, while the flame retardancy of the samples of embodiments E1 to E13 are all V0; the Z-PTE of the comparative example C1 sample is 1.8%, while the Z-PTE of the samples of embodiments E1 to E13 are all less than or equal to 1.5%; the PCT of the comparative example C1 sample exploded, while the PCT of the samples of embodiments E1 to E13 did not explode.

[0215] 2. Examples E1 to E10 use a phosphorus-containing compound having the structure of formula (1), and E11 to E13 use the prepolymer of the present application. Compared with the mixture of V1 and DPO (Comparative Example C2) and the mixture of DABPA, 4-bromobenzocyclobutene and DPO (Comparative Example C3), the following properties are significantly improved: Tg, Dk, Df, Z-PTE and PCT. Among them, the Tg of the comparative examples C2 and C3 samples is less than 240°C, while the Tg of the samples of embodiments E1 to E13 is greater than or equal to 240°C; the Dk of the comparative examples C2 and C3 samples is greater than 3.20, while the Dk of the samples of embodiments E1 to E13 is less than or equal to 3.20; the Df of the comparative examples C2 and C3 samples is greater than 0.0020, while the Df of the samples of embodiments E1 to E13 is less than or equal to 0.0020; the Z-PTE of the comparative examples C2 and C3 samples is greater than 1.5%, while the Z-PTE of the samples of embodiments E1 to E13 is less than or equal to 1.5%; the PCT of the comparative examples C2 and C3 samples exploded, while the PCT of the samples of embodiments E1 to E13 did not explode.

[0216] 3. Examples E1 to E10 use phosphorus-containing compounds having the structure of formula (1), and E11 to E13 use the prepolymer of the present application. Compared with the use of phosphorus-containing compounds with other structures (Comparative Examples C4 to C7), the following properties are significantly improved: Tg, Dk, Df, Z-PTE and PCT. Among them, the Tg of the samples of comparative examples C4 to C7 is less than 240°C, while the Tg of the samples of embodiments E1 to E13 is greater than or equal to 240°C; the Dk of the samples of comparative examples C4 to C7 is greater than 3.20, while the Dk of the samples of embodiments E1 to E13 is less than or equal to 3.20; the Df of the samples of comparative examples C4 to C7 is greater than 0.0020, while the Df of the samples of embodiments E1 to E13 is less than or equal to 0.0020; the Z-PTE of the samples of comparative examples C4 to C7 is greater than 1.5%, while the Z-PTE of the samples of embodiments E1 to E13 is less than or equal to 1.5%; the PCT of the samples of comparative examples C4 to C7 has different degrees of bursting, while the PCT of the samples of embodiments E1 to E13 has no bursting.

[0217] The above embodiments are essentially only for auxiliary explanation and are not intended to limit the embodiments of the present application or the application or use of these embodiments. In the present application, words similar to "example" represent "as an example, example or illustration". Any illustrative embodiment herein is not necessarily interpreted as being preferred or more advantageous relative to other embodiments, unless otherwise specified.

[0218] In addition, although at least one exemplary embodiment or comparative example has been proposed in the aforementioned embodiments, it should be understood that there are still a large number of variations in the present application. It should also be understood that the embodiments described herein are not intended to limit the scope, use or configuration of the requested technical solution in any way. On the contrary, the aforementioned embodiments will provide a simple guide for those skilled in the art to implement one or more of the embodiments and their equivalents. Furthermore, the claims include known equivalents and all foreseeable equivalents when the present patent application is filed.

Claims

1. A phosphorus-containing compound, the structure of which is shown in formula (1): In the structural formula (1), X is a covalent bond or a C1-C3 alkyl group, R is independently a group represented by formula (2), formula (3) or formula (4), in, R1~R 28 Each is independently a hydrogen atom or a C1-C3 alkyl group.

2. The phosphorus-containing compound according to claim 1, characterized in that The phosphorus-containing compound is any one of the phosphorus-containing compounds represented by the structures of formula (5) to formula (9), 3. A method for producing the phosphorus-containing compound according to claim 1, comprising the following steps: Step (1): preparing a halogen benzocyclobutene Grignard reagent in a reaction vessel; Step (2): In another reaction vessel, diallyl bisphenol is reacted with one or more compounds RH to obtain an intermediate product 1, wherein H in the compound RH represents a hydrogen atom, and R is a group represented by formula (2), formula (3) or formula (4). Among them, R1~R 28 Each is independently a hydrogen atom or a C1-C3 alkyl group; Step (3): reacting the halogen benzocyclobutene Grignard reagent obtained in step (1) with the intermediate 1 to obtain a phosphorus-containing compound represented by formula (1).

4. The method for producing a phosphorus-containing compound according to claim 3, characterized in that: The reaction temperature of step (1) is 0°C to 100°C, and the reaction time of step (1) is 1 to 10 hours. In step (2), the RH is diphenylphosphine oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, diphenyl phosphonate or bis(2,6-dimethylphenyl)phosphonate, and the molar ratio of the RH to the diallyl bisphenol is 2:1 to 3:

1. The reaction temperature of step (2) is 80° C. to 160° C., and the reaction time of step (2) is 1 to 6 hours. The reaction temperature of step (3) is -20°C to 120°C, and the reaction time of step (3) is 3 to 30 hours.

5. A resin composition comprising the following components or prepolymers thereof, (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; (B) 15 to 90 parts by weight of the phosphorus-containing compound of claim 1; in, The prepolymer is obtained by prepolymerizing a mixture, and the mixture contains at least the component (A) and the component (B).

6. The resin composition according to claim 5, characterized in that The component (A) includes any one of (meth)acryl polyphenylene ether resin, vinylbenzyl polyphenylene ether resin, and vinyl polyphenylene ether resin, or a combination of two or more thereof.

7. The resin composition according to claim 5, characterized in that The phosphorus-containing compound includes any one or a combination of two or more of the phosphorus-containing compounds represented by formula (5) to formula (9), 8. The resin composition according to claim 5, characterized in that The prepolymer is formed by a prepolymerization reaction between the component (A) and the component (B), and the conversion rate of the prepolymerization reaction is between 10% and 99%.

9. The resin composition according to claim 5, characterized in that The resin composition further comprises any one or a combination of two or more of a cross-linking agent containing unsaturated carbon-carbon double bonds, a silicone resin, a benzoxazine resin, an epoxy resin, a polyester resin, a phenolic resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, and a maleimide triazine resin.

10. The resin composition according to claim 5, characterized in that The resin composition further comprises any one or a combination of two or more of a hardening accelerator, a polymerization inhibitor, an inorganic filler, a surface treatment agent, a dye, and a solvent.

11. A product, characterized in that The product is made of the resin composition according to any one of claims 5 to 10, wherein the product includes a prepreg, a resin film, a laminate or a printed circuit board.

12. The product according to claim 11, characterized in that The product has one, more or all of the following characteristics: The glass transition temperature measured by the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 240oC, The dielectric constant Dk measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 3.20, The dielectric loss Df measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.0020, The flame retardancy measured according to the method described in UL94 is V0. The Z-axis thermal expansion rate measured by the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.5%, The products were tested for moisture absorption and heat resistance according to the methods of IPC-TM-650 2.6.16.1 and IPC-TM-650 2.4.23, and no board explosion occurred. The copper foil tensile force measured in accordance with IPC-TM-650 2.4.8 is greater than or equal to 3.2 lb / in.

Citation Information

Cited By

  • Resin composition and article made therefrom

    TWI946345B