Production method of transition material for reducing chromium polyethylene to produce metallocene polyethylene
By adjusting the state of the chromium-based polyethylene reactor and converting the transition material into metallocene polyethylene rotomolding or PE-RT pipe products, the problem of excessive transition material in the process of converting chromium-based polyethylene to metallocene polyethylene is solved, and production is reduced Cost and workload improve production conversion efficiency.
Patent Information
- Application Number
- CN202411489358.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the process of converting chromium polyethylene to metallocene polyethylene, excessive transition materials are produced, resulting in loss of enterprise benefits. The existing methods require emptying the bed powder, cleaning and replacing the metallocene polyethylene seed bed, which is costly and processed complex.
By adjusting the chromium-based polyethylene gas-phase reactor to the production state, injecting the terminator and pretreatment agent, the transition material is converted into metallocene polyethylene rotomolding products or PE-RT pipe products that have no requirements for fish eyes, and through blending and blowing Plastics evaluate fisheye content, adjust production parameters to complete the conversion of metallocene polyethylene, avoid emptying of beds and replacement steps.
It reduces the demand and replacement cost of seed beds, reduces workload and inspection and maintenance costs, effectively reduces the production of transition materials, and improves production efficiency and enterprise benefits.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of petrochemical industry and relates to a production method of a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene. Background Art
[0002] Metallocene polyethylene is a polyethylene resin polymerized by a catalyst consisting of metallocene organic compounds and co-catalysts. At present, foreign companies mainly use gas phase and loop slurry production processes, and the comonomer is mostly 1-hexene, and some use 1-octene. The metallocene catalysts used are all independently developed, and the products have become serialized. Domestic metallocene (mPE) manufacturers mainly use gas phase production technology, and the comonomer is 1-hexene. The catalyst mainly uses Univation's metallocene catalyst, and a few companies use GRACE and Xinsu Chemical Metallocene TH-5 series catalysts.
[0003] Metallocene catalysts have a single active center and extremely high catalytic activity. They are very different from traditional Ziegler-Natta catalysts and chromium-based catalyst systems. They are more sensitive to impurity components in the raw materials. At the same time, their responses to hydrogen and comonomers are also very different. Therefore, in the current gas-phase polymerization process for producing metallocene polyethylene, the domestic industry mainly uses existing metallocene polyethylene as a seed bed for production. However, this production method has the following disadvantages: ① As the domestic metallocene polyethylene production technology is in its initial stage, the metallocene polyethylene products used in large-scale industrial applications are mainly used for film products such as heavy coating and greenhouse film, which have high requirements for product fisheyes; ② As the domestic metallocene polyethylene production technology is in its initial stage and the technology is not yet mature, there are only a few manufacturers that can achieve stable production; therefore, some companies that are preparing to develop the production of metallocene polyethylene must purchase foreign metallocene polyethylene powder as a seed bed during the initial production process to support the development of metallocene polyethylene; ③ For gas phase polyethylene production equipment, the production grades are mainly titanium and chromium polyethylene, and the corresponding titanium seed bed and chromium seed bed must be used during production; after the metallocene polyethylene products are produced, the metallocene polyethylene seed bed must be used, and a silo dedicated to storing metallocene polyethylene powder must be built to hold the metallocene polyethylene seed bed, which has high construction and maintenance costs (some enterprises without silos must transform their equipment and add metallocene polyethylene seed silos); ④ In the process of converting between the products of chromium catalyst system and metallocene polyethylene grades, a series of steps must be experienced, such as reactor deactivation, emptying of bed powder, qualified replacement of reaction loop, cleaning, reloading, replacement again, filling of metallocene polyethylene seed bed, qualified replacement, etc., before metallocene polyethylene can be started. The replacement cycle is long, the inspection and maintenance cost is high, and a lot of manpower and material resources are consumed; ⑤ The recently developed process of converting chromium polyethylene to metallocene polyethylene. For example, CN 117567675A discloses a production method of converting chromium polyethylene to metallocene polyethylene, which includes: adjusting the gas phase reactor of the chromium polyethylene to be converted to the conversion state, and then injecting a terminator; replacing the gas phase reactor of the chromium polyethylene to be converted, and then injecting a pretreatment agent; re-establishing the gas phase component concentration according to the initiation conditions of the metallocene polyethylene, and then injecting a metallocene catalyst to initiate the reaction and complete the conversion. Although this method reduces the steps of emptying the bed powder, cleaning, reloading, replacing again, and filling the metallocene polyethylene seed bed, the chromium polyethylene powder in the bed is mixed with the newly generated metallocene polyethylene during the conversion process, which makes the bed replacement more difficult, resulting in a slow reduction in the fisheye content in the metallocene polyethylene product and excessive production of transition materials. Summary of the invention
[0004] In view of this, the present invention provides a production method for reducing transition materials in converting chromium-based polyethylene to metallocene polyethylene. On the basis of the existing production method for converting chromium-based polyethylene to metallocene polyethylene, the problem of excessive transition materials in the conversion process is solved while ensuring that the fisheye of the metallocene polyethylene used for membrane materials is at a reasonable level.
[0005] In a first aspect, the present invention provides a method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene, comprising the following steps: 1) Adjust the gas phase reactor of the chromium polyethylene to be converted to the conversion state, and then inject the terminator; 2) replacing the gas phase reactor of the chromium polyethylene to be converted, and then injecting a pretreatment agent; 3) Convert the transition material generated during the conversion process into metallocene polyethylene rotational molding products or PE-RT pipe products that do not require fisheyes; 4) evaluating the fisheye content of the metallocene polyethylene rotational molding product or PE-RT pipe product obtained in step 3); 5) When the fisheye content in the metallocene polyethylene rotational molding product or the PE-RT pipe product meets the requirements, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for the membrane material to convert the production of the metallocene polyethylene.
[0006] In the above production method, as an optional embodiment, in step 1), adjusting the gas phase reactor of the chromium polyethylene to be converted to a conversion state comprises the following steps: Adjust the gas phase reactor of the chromium polyethylene to be converted from condensed production mode to dry operation mode; In the dry operation mode, the discharge frequency of the gas phase reactor discharge system of the chromium polyethylene to be converted is reduced to accumulate the bed weight to the quality required for the start-up of the metallocene; Gradually reduce the catalyst injection amount to zero to allow the residual catalyst to be naturally consumed and the reaction load to be reduced, thus completing the adjustment of the production conversion status.
[0007] In the above production method, as an optional implementation, in step 1), the terminator includes at least one of CO2 and O2.
[0008] In the above production method, as an optional implementation, in step 2), the amount of the pretreatment agent added is 15 ppm to 25 ppm of the bed weight of the gas phase reactor of the chromium-based polyethylene to be converted.
[0009] As an optional embodiment, the pretreatment agent is circulated in the gas phase reactor of the chromium-based polyethylene to be converted for 1 h to 2 h.
[0010] In the above production method, as an optional implementation, in step 2), the pretreatment agent includes an antistatic agent.
[0011] As an optional embodiment, the antistatic agent includes at least one of CA-200 and CA-300.
[0012] In the present invention, CA-200 and CA-300 are common antistatic agents in the art. Among them, CA-200 is mainly composed of aluminum stearate, oil-soluble alkyl alcohol amine and mineral oil solvent, with a ratio of 10% to 30%: 15% to 25%: 65% to 90%; CA-300 is mainly composed of aluminum stearate, oil-soluble alkanolamide, mineral oil solvent, stearate, with a ratio of 10% to 30%: 15% to 25%: 65% to 90%: 1% to 3%).
[0013] In the above production method, as an optional implementation, in step 2), the replacement adopts a pressure increase and decrease method.
[0014] In the above production method, as an optional implementation, the low pressure of the boost-and-drop pressure method is 600 kPa to 900 kPa, and the high pressure of the boost-and-drop pressure method is 1100 kPa to 1400 kPa.
[0015] In the above production method, as an optional implementation, in step 2), the completion of the replacement is based on O2 < 8 ppm and CO2 < 8 ppm in the gas phase reactor of the chromium-based polyethylene to be converted.
[0016] In the above production method, as an optional implementation, in step 3), the transition material refers to a mixed product of the chromium polyethylene product and the metallocene polyethylene product produced in the process of replacing the chromium polyethylene bed layer, and a product whose quality does not meet the factory specifications.
[0017] During the process of replacing the chromium polyethylene bed layer, not only the chromium polyethylene product is replaced as transition material when discharging, but also a part of the newly generated metallocene polyethylene product is replaced as transition material. This transition material cannot be sold as a qualified product, thus causing loss of corporate benefits.
[0018] In the above production method, as an optional implementation, in step 3), the transition material generated in the conversion process is converted into a metallocene polyethylene rotational molding product or a PE-RT pipe product with no fisheye requirement, and the following steps are also included: According to the initiation conditions of metallocene polyethylene, the concentration of gas phase components is re-established, and then the metallocene catalyst is injected to produce metallocene polyethylene rotational molding products or PE-RT pipe products with no requirements for fisheyes.
[0019] In the prior art, in the process of converting chromium-based polyethylene to metallocene polyethylene, since the chromium-based polyethylene product generated before the conversion and the metallocene polyethylene product generated after the conversion are not compatible with each other, the mixture of the two products during the conversion causes the fisheye of the metallocene polyethylene product obtained from the conversion to be unqualified and cannot be used as a raw material for producing qualified polyethylene film materials. Therefore, the mixture of the chromium-based polyethylene product and the metallocene polyethylene product can only be replaced during the conversion process as a transition material, and the transition material cannot be sold as a qualified product, thereby causing a loss of corporate benefits.
[0020] The present invention uses a metallocene catalyst to first produce a metallocene polyethylene rotomolding product or a PE-RT pipe product after injecting a metallocene catalyst during the process of converting chromium polyethylene to metallocene polyethylene. These products have no requirements for fisheyes, so the chromium polyethylene product produced before the conversion is mixed with the metallocene polyethylene rotomolding product or the PE-RT pipe product, and the chromium polyethylene product produced before the conversion (i.e., transition material) is discharged so that the chromium polyethylene product produced before the conversion (i.e., transition material) is gradually removed from the conversion reaction system. When the chromium polyethylene product no longer exists in the metallocene polyethylene rotomolding product or the PE-RT pipe product in the reaction system or when the chromium polyethylene product has no obvious effect on the fisheye of the metallocene polyethylene film material product, the metallocene polyethylene is produced again, thereby completing the conversion of the metallocene polyethylene and converting the transition material produced in the conversion into the metallocene polyethylene rotomolding product or the PE-RT pipe product without causing a waste of resources.
[0021] In the above production method, as an optional embodiment, in step 3), when producing metallocene polyethylene rotational molding products or PE-RT pipe materials, the corresponding gas phase components include at least one of N2, isopentane, ethylene, H2 and hexene-1.
[0022] In the above production method, as an optional implementation, in the step 3), when producing metallocene polyethylene rotational molding products or PE-RT pipe materials, the ethylene concentration is maintained at 60% to 75% and the catalyst activity is maintained at 4500 kg / kg to 6000 kg / kg.
[0023] In the above production method, as an optional embodiment, in the step 3), the melt index of the metallocene polyethylene rotomolding product is 3 g / 10 min to 6 g / 10 min, and the density is 0.935 g / cm 3 Up to 0.945 g / cm 3 .
[0024] In the above production method, as an optional embodiment, in the step 3), the melt index of the metallocene polyethylene PE-RT pipe material is 1 g / 10 min to 2 g / 10 min, and the density is 0.935 g / cm 3 Up to 0.945 g / cm 3 .
[0025] In the above production method, as an optional implementation, the metallocene catalyst used in the production of metallocene polyethylene rotational molding products or metallocene polyethylene PE-RT pipe materials is a supported metallocene catalyst.
[0026] In the above production method, as an optional embodiment, the supported metallocene catalyst comprises methylaluminoxane (MAO) and carrier silica gel, wherein the content of methylaluminoxane (MAO) is 15% to 20%, and the specific surface area of the carrier silica gel is 250 m 2 / g to 300 m 2 / g.
[0027] In the above production method, as an optional implementation, in step 4), the fisheye content of the metallocene polyethylene rotational molded product or PE-RT pipe product obtained in step 3) is evaluated by blow molding or casting after blending.
[0028] Since metallocene polyethylene rotomolding products or PE-RT pipe products cannot be used to produce film materials, it is impossible to directly obtain the fisheye information of metallocene polyethylene rotomolding products or PE-RT pipe products. The present invention obtains a polyethylene film by mixing the metallocene polyethylene rotomolding products or PE-RT pipe products with a finished metallocene polyethylene film material (metallocene polyethylene used to prepare film materials) and then blow-molding or casting the mixture to obtain a polyethylene film, and then using the polyethylene film to evaluate the fisheye content information of the metallocene polyethylene rotomolding products or PE-RT pipe products.
[0029] In the above production method, as an optional implementation, in step 4), the evaluation includes: mixing the metallocene polyethylene rotational molding product or PE-RT pipe material into the qualified metallocene polyethylene for preparing the membrane material at 10% to 50%, and making the polyethylene film product by blow molding or casting, observing the reduction of fish eyes, until there are no fish eyes or only a small number of small fish eyes, it is determined to be qualified, and then the next step of production conversion is started.
[0030] In the above production method, as an optional embodiment, in step 4), as the fisheyes of the polyethylene film product in the evaluation decrease, the mixing ratio of the metallocene polyethylene rotational molding product or PE-RT pipe material and the qualified metallocene polyethylene for preparing the film material increases.
[0031] In the above production method, as an optional implementation, in step 5), adjusting the production parameters includes adjusting the gas phase components, and the gas phase components include at least one of N2, isopentane, ethylene, H2 and hexene-1.
[0032] In the above production method, as an optional embodiment, in step 5), the melt index of the metallocene polyethylene used for the film material produced is 0.2 g / 10 min to 4 g / 10 min, and the density is 0.915 g / cm 3 Up to 0.945 g / cm 3 .
[0033] In the above production method, as an optional embodiment, in step 5), the fisheye of the polyethylene film product is evaluated according to GB / T 11115, and the product index of the polyethylene film product requires that the fisheye (0.4 mm) is ≤ 15 / 1520 cm 2 , fisheye (0.8 mm) ≤ 6 / 1520 cm 2 .
[0034] In the above production method, as an optional implementation, in step 5), adjusting the production parameters includes adjusting the process parameters of ethylene, H2 and hexene-1.
[0035] In the above production method, as an optional embodiment, in step 5), the ethylene concentration is maintained at 60% to 75%, and the catalyst activity is maintained at 4500 kg / kg to 6000 kg / kg; the H2 partial pressure in the reactor is reduced to 0.3 kPa to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 kPa to 12 kPa.
[0036] In the above production method, as an optional implementation, the metallocene polyethylene rotational molding product with no fisheye requirement includes mHD3605UA.
[0037] In the above production method, as an optional implementation, the PE-RT pipe product with no fisheye requirement includes mHD3702.
[0038] The present invention provides a production method for reducing chromium-based polyethylene to produce metallocene polyethylene transition material. Without emptying the bed powder and cleaning the reactor, an antistatic agent is added after qualified replacement to eliminate the influence of residual components in the bed on the metallocene catalyst, and then a gas phase is established, and the metallocene catalyst is injected to initiate the reaction; according to demand, the metallocene catalyst is used to produce metallocene polyethylene rotational molding products or PE-RT pipe products with no requirements for fisheyes. In this process, the fisheye content of the product is evaluated by sample preparation methods such as blending blow molding and casting. After the fisheye content in the product meets the requirements for metallocene polyethylene, the production parameters are adjusted to complete the production conversion.
[0039] In the present invention, the above technical features can be freely combined to form a new technical solution without conflicting with each other.
[0040] Compared with the prior art, the above technical solution provided by the present invention has the following beneficial effects: (1) According to the production method of the present invention, the metallocene polyethylene production can be completed without using a metallocene polyethylene seed bed during the entire conversion process, which not only reduces the cost of extracting and filling the seed bed to the greatest extent, but also avoids the construction cost of adding a metallocene polyethylene seed silo for enterprises without a metallocene polyethylene seed bed; (2) The production method of the present invention utilizes metallocene polyethylene rotational molding products or PE-RT pipe products that have no requirements for fisheyes, thereby solving the problem that the metallocene polyethylene products produced during the replacement of the chromium polyethylene bed layer during the start-up of the metallocene polyethylene have fisheyes for a long time and produce a large amount of transition materials; (3) The technical solution of the present invention eliminates the need to extract the chromium seed bed and load the metallocene polyethylene seed bed, thereby significantly reducing the workload and working time, lowering the inspection and maintenance costs of the device, and further reducing the economic benefit losses caused by the production of transition materials. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0042] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0043] Some embodiments of the present invention provide a method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene, comprising the following steps: 1) Adjust the gas phase reactor of the chromium polyethylene to be converted to the conversion state, and then inject the terminator; 2) replacing the gas phase reactor of the chromium polyethylene to be converted, and then injecting a pretreatment agent; 3) Convert the transition material generated during the conversion process into metallocene polyethylene rotational molding products or PE-RT pipe products that do not require fisheyes; 4) evaluating the fisheye content of the metallocene polyethylene rotational molding product or PE-RT pipe product obtained in step 3); 5) When the fisheye content in the metallocene polyethylene rotational molding product or the PE-RT pipe product meets the requirements, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for the membrane material to convert the production of the metallocene polyethylene.
[0044] In some embodiments, in step 1), adjusting the gas phase reactor of the chromium polyethylene to be converted to a conversion state comprises the following steps: Adjust the gas phase reactor of the chromium polyethylene to be converted from condensed production mode to dry operation mode; In the dry operation mode, the discharge frequency of the gas phase reactor discharge system of the chromium polyethylene to be converted is reduced to accumulate the bed weight to the quality required for the start-up of the metallocene; Gradually reduce the catalyst injection amount to zero to allow the residual catalyst to be naturally consumed and the reaction load to be reduced, thus completing the adjustment of the production conversion status.
[0045] In some embodiments, in step 1), the terminator includes at least one of CO2 and O2.
[0046] In some embodiments, in step 2), the pretreatment agent includes an antistatic agent, the amount of the pretreatment agent added is 15 ppm to 25 ppm of the bed weight of the gas phase reactor of the chromium-based polyethylene to be converted, and the pretreatment agent circulates in the gas phase reactor of the chromium-based polyethylene to be converted for 1 h to 2 h.
[0047] In some embodiments, the antistatic agent includes at least one of CA-200 and CA-300.
[0048] In some embodiments, in step 2), the replacement is performed by a step-up and step-down pressure method, wherein the low pressure of the step-up and step-down pressure method is 600 kPa to 900 kPa, and the high pressure is 1100 kPa to 1400 kPa.
[0049] In some embodiments, in step 3), converting the transition material produced in the conversion process into a metallocene polyethylene rotational molding product or a PE-RT pipe product specifically comprises the following steps: According to the initiation conditions of metallocene polyethylene, the concentration of gas phase components is re-established, and then the metallocene catalyst is injected to produce metallocene polyethylene rotational molding products or PE-RT pipe products with no requirements for fisheyes.
[0050] In some embodiments, in step 3), when producing the metallocene polyethylene rotational molding product or the PE-RT pipe material, the corresponding gas phase components include at least one of N2, isopentane, ethylene, H2 and hexene-1.
[0051] In some embodiments, in step 3), when producing metallocene polyethylene rotational molding products or PE-RT pipe materials, the ethylene concentration is maintained at 60% to 75% and the catalyst activity is maintained at 4500 kg / kg to 6000 kg / kg.
[0052] In some embodiments, in step 3), the metallocene polyethylene rotational molding product with no fisheye requirement includes mHD3605UA; the PE-RT pipe product with no fisheye requirement includes mHD3702.
[0053] In some embodiments, in step 3), the melt index of the metallocene polyethylene rotomolding product is 3 to 6 g / 10 min, and the density is 0.935 to 0.945 g / cm 3 Or the melt index of the metallocene polyethylene PE-RT pipe material is 1 to 2g / 10 min, and the density is 0.935 to 0.945 g / cm 3 .
[0054] In some embodiments, the metallocene catalyst used in the production of metallocene polyethylene rotational molding products or metallocene polyethylene PE-RT pipe materials is a supported metallocene catalyst; the supported metallocene catalyst includes methylaluminoxane (MAO) and carrier silica gel, wherein the content of methylaluminoxane (MAO) is 15% to 20%, and the specific surface area of the carrier silica gel is 250 to 300 m 2 / g.
[0055] In some embodiments, in step 4), the fisheye content of the metallocene polyethylene rotational molded product or PE-RT pipe product obtained in step 3) is evaluated by blow molding or casting after blending.
[0056] In some embodiments, in step 4), the evaluation includes: blending the metallocene polyethylene rotational molding product or PE-RT pipe material into qualified metallocene polyethylene for preparing membrane materials at a rate of 10% to 50%, producing a polyethylene film product by blow molding or casting, observing the reduction of fish eyes until there are no fish eyes or only a small number of small fish eyes, and determining that it is qualified, and the next step of production conversion can be started.
[0057] In some embodiments, in step 4), as the fisheyes of the polyethylene film product in the evaluation decrease, the blending ratio of the metallocene polyethylene rotational molding product or PE-RT pipe material and the qualified metallocene polyethylene for preparing the film material increases.
[0058] In some embodiments, in step 5), adjusting the production parameters includes adjusting a gas phase component, wherein the gas phase component includes at least one of N2, isopentane, ethylene, H2, and hexene-1.
[0059] In some embodiments, in step 5), the H2 partial pressure in the reactor is reduced to 0.3 to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 to 12 kPa.
[0060] In some embodiments, in step 5), the melt index of the metallocene polyethylene used for the film material produced is 0.2 to 4 g / 10 min, and the density is 0.915 to 0.945 g / cm 3According to GB / T 11115, the fisheye of polyethylene film products is evaluated. The product index of polyethylene film products requires that the fisheye (0.4 mm) should be ≤ 8 / 1520 cm 2 , fisheye (0.8 mm) ≤ 1 / 1520 cm 2 .
[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0062] In addition, since the detection of the fisheye content of the metallocene polyethylene rotomolding product is carried out by taking samples of the metallocene polyethylene rotomolding product during the production process, for the convenience of description, the following embodiment incorporates the technical features of the above step 4) into step 3) to form a new step S3.
[0063] Example 1 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: Convert the transition material produced in the conversion process into a metallocene polyethylene rotomolding product with no fisheye requirement; specifically, according to the initiation conditions of metallocene polyethylene, re-establish the concentration of gas phase components, maintain the ethylene concentration at 60% to 75%, and the catalyst activity at 4500 kg / kg to 6000 kg / kg; then inject the metallocene catalyst to produce a metallocene polyethylene rotomolding product with no fisheye requirement; evaluate the fisheye content of the metallocene polyethylene rotomolding product obtained in the production process; specifically, blend the metallocene polyethylene rotomolding product into the qualified metallocene polyethylene film material at 10%, 20%, 30%, 40% and 50% respectively, obtain polyethylene products by blow molding, observe the reduction of fisheyes, and judge it as qualified after there is no fisheye or only a small amount of small fisheyes, and the production time of the metallocene polyethylene rotomolding product is greater than 150 hours; S4: After the fisheye content in the metallocene polyethylene rotational molded product is judged to be qualified, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, the H2 partial pressure in the reactor is reduced to 0.3 to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 to 12 kPa, and the production of the metallocene polyethylene used for membrane materials is started to complete the conversion.
[0064] In step S4 of this embodiment, after 2.5 times of BTO (replacement cycle), the fisheye (0.4 mm) of the metallocene polyethylene produced for membrane material is 8 / 1520cm 2 , fisheye (0.8 mm) is 1 / 1520 cm 2 The melt index of the metallocene polyethylene rotomolded product obtained in step S3 is 5.0 g / 10 min and the density is 0.938 g / cm 3 The metallocene polyethylene (for membrane material) obtained in step S4 has a melt index of 2.2 g / 10 min and a density of 0.920 g / cm 3 .
[0065] Example 2 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: Convert the transition material produced in the conversion process into metallocene polyethylene PE-RT pipe products with no fisheye requirements; specifically, according to the initiation conditions of metallocene polyethylene, re-establish the gas phase component concentration, maintain the ethylene concentration at 60% to 75%, and the catalyst activity at 6000 kg / kg to 7500 kg / kg; then inject the metallocene catalyst to produce PE-RT pipe products with no fisheye requirements; evaluate the fisheye content of the metallocene polyethylene rotational molded products or PE-RT pipe products obtained in the production process; specifically, blend the metallocene polyethylene rotational molded products into qualified metallocene polyethylene film materials at 10%, 20%, 30%, 40% and 50% respectively, and make polyethylene products by blow molding, observe the reduction of fisheyes, and judge it as qualified after there are no fisheyes or only a small number of small fisheyes, and the production time of metallocene polyethylene PR-RT pipe products is greater than 150 hours; S4: After the fisheye content in the metallocene polyethylene rotational molding product or the PE-RT pipe product is determined to be qualified, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, by reducing the H2 partial pressure in the reactor to 0.3 to 0.8 kPa and increasing the hexene-1 partial pressure in the reactor to 8 to 12 kPa, the production of the metallocene polyethylene used for membrane materials is started to complete the conversion.
[0066] In step S4 of this embodiment, after 2.5 times of BTO, the fisheye (0.4 mm) of the metallocene polyethylene produced for membrane material is 6 / 1520cm 2, fisheye (0.8 mm) is 2 / 1520 cm 2 The metallocene polyethylene PE-RT pipe product obtained in step S3 has a melt index of 1.5 g / 10 min and a density of 0.938 g / cm 3 The metallocene polyethylene (for membrane material) obtained in step S4 has a melt index of 2.0 g / 10 min and a density of 0.918 g / cm 3 .
[0067] Example 3 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: Convert the transition material produced in the conversion process into a metallocene polyethylene rotomolding product with no fisheye requirement; specifically, according to the initiation conditions of metallocene polyethylene, re-establish the gas phase component concentration, maintain the ethylene concentration at 60% to 75%, and the catalyst activity at 4500 kg / kg to 6000 kg / kg; then inject the metallocene catalyst to produce a metallocene polyethylene rotomolding product with no fisheye requirement; evaluate the fisheye content of the metallocene polyethylene rotomolding product obtained in the production process; specifically, blend the metallocene polyethylene rotomolding product into the qualified metallocene polyethylene film material at 10%, 20%, 30%, 40%, and 50%, respectively, and obtain polyethylene products by casting, observe the reduction of fisheyes, and judge it as qualified after there is no fisheye or only a small amount of small fisheyes, and the production time of the metallocene polyethylene rotomolding product is greater than 150 hours; S4: After the fisheye content in the metallocene polyethylene rotational molded product is judged to be qualified, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, the H2 partial pressure in the reactor is reduced to 0.3 to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 to 12 kPa, and the production of the metallocene polyethylene used for membrane materials is started to complete the conversion.
[0068] In step S4 of this embodiment, after 2.5 times of BTO, the metallocene polyethylene produced for membrane material has 9 fisheyes (0.4 mm) / 1520cm 2 , fisheye (0.8 mm) 2 / 1520 cm 2 The melt index of the metallocene polyethylene rotomolded product obtained in step S3 is 5.2 g / 10 min and the density is 0.939 g / cm 3The metallocene polyethylene (for membrane material) obtained in step S4 has a melt index of 2.1 g / 10 min and a density of 0.921 g / cm 3 .
[0069] Example 4 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: Convert the transition material produced during the conversion process into metallocene polyethylene PE-RT pipe products with no fisheye requirements; specifically, according to the initiation conditions of metallocene polyethylene, re-establish the gas phase component concentration, maintain the ethylene concentration at 60% to 75%, and the catalyst activity at 6000 kg / kg to 7500 kg / kg; then inject the metallocene catalyst to produce PE-RT pipe products with no fisheye requirements; evaluate the fisheye content of the PE-RT pipe products obtained during the production process; specifically, mix the metallocene polyethylene rotational molding products into qualified metallocene polyethylene film materials at 10%, 20%, 30%, 40%, and 50%, respectively, and make polyethylene products by casting, observe the reduction of fisheyes, and judge it as qualified after there are no fisheyes or only a small number of small fisheyes, and the production time of metallocene polyethylene PR-RT pipe products is greater than 150 hours; S4: After the fisheye content in the PE-RT pipe product is determined to be qualified, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, the H2 partial pressure in the reactor is reduced to 0.3 to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 to 12 kPa, and the production of the metallocene polyethylene used for membrane materials is started to complete the conversion.
[0070] In step S4 of this embodiment, after 2.5 times of BTO, the fisheye (0.4 mm) of the metallocene polyethylene produced for membrane material is 8 / 1520cm 2 , fisheye (0.8 mm) is 1 / 1520 cm 2 The metallocene polyethylene PE-RT pipe product obtained in step S3 has a melt index of 1.4 g / 10 min and a density of 0.936 g / cm 3 The metallocene polyethylene (for membrane material) obtained in step S4 has a melt index of 1.9 g / 10 min and a density of 0.919 g / cm 3 .
[0071] Comparative Example 1 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: converting the transition material produced in the conversion process into a metallocene polyethylene rotomolding product with no fisheye requirement; specifically, re-establishing the gas phase component concentration according to the initiation conditions of the metallocene polyethylene, maintaining the ethylene concentration at 60% to 75%, and the catalyst activity at 4500 kg / kg to 6000 kg / kg; then injecting the metallocene catalyst to produce the metallocene polyethylene rotomolding product with no fisheye requirement for 100 hours; S4: Adjust the production parameters according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, by reducing the H2 partial pressure in the reactor to 0.3 to 0.8 kPa and increasing the hexene-1 partial pressure in the reactor to 8 to 12 kPa, start the production of the metallocene polyethylene used for membrane materials to complete the conversion.
[0072] In step S4 of this comparative example, after 3 times of BTO, the fisheye (0.4 mm) of the produced metallocene polyethylene (used for membrane material) is 45 / 1520 cm 2 , fisheye (0.8 mm) is 18 / 1520 cm 2 The metallocene polyethylene (used as membrane material) obtained in step S4 has a melt index of 1.8 g / 10 min and a density of 0.923 g / cm 3 .
[0073] Comparative Example 2 A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene comprises the following steps: S1: Adjust the gas phase reactor of the chromium-based polyethylene to be converted to the conversion state, and then inject the terminator; S2: replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; S3: Convert the transition material produced during the conversion process into metallocene polyethylene PE-RT pipe products with no fisheye requirements; specifically, according to the initiation conditions of metallocene polyethylene, re-establish the gas phase component concentration, maintain the ethylene concentration at 60% to 75%, and the catalyst activity at 6000 kg / kg to 7500 kg / kg; then inject the metallocene catalyst to produce PE-RT pipe products with no fisheye requirements for 80 hours; S4: Adjust the production parameters according to the production parameters of the metallocene polyethylene used for membrane materials to complete the conversion of the metallocene polyethylene; specifically, reduce the H2 partial pressure in the reactor to 0.3 to 0.8 kPa, increase the hexene-1 partial pressure in the reactor to 8 to 12 kPa, and start the production of the metallocene polyethylene used for membrane materials to complete the conversion.
[0074] In step S4 of this comparative example, after 3 times of BTO, the fisheye (0.4 mm) of the produced metallocene polyethylene (used for membrane material) is 55 / 1520cm 2 , fisheye (0.8 mm) is 12 / 1520 cm 2 The melt index of the metallocene polyethylene film material obtained in step S4 is 1.9 g / 10 min and the density is 0.921 g / cm 3 .
[0075] Comparative Example 3 A production method for reducing chromium-based polyethylene to produce metallocene polyethylene transition material, comprising the following steps: 1) Adjust the gas phase reactor of the chromium polyethylene to be converted to the conversion state, and then inject the terminator; 2) replacing the gas phase reactor of the chromium-based polyethylene to be converted, and then injecting a pretreatment agent; 3) According to the initiation conditions of metallocene polyethylene, the concentration of gas phase components is re-established by adjusting the amount of H2 and hexene-1 added to the reactor, and then the metallocene catalyst is injected and its catalytic activity is ensured to be 6000 kg / kg to initiate the reaction and start the production of metallocene polyethylene film.
[0076] In step S3 of this comparative example, after 15 times of BTO, the fisheye (0.4 mm) of the produced metallocene polyethylene (used for membrane material) is 88 / 1520cm 2 , fisheye (0.8 mm) is 32 / 1520 cm 2 , see Table 1. The metallocene polyethylene (for membrane material) obtained in step S3 has a melt index of 1.9 g / 10 min and a density of 0.917 g / cm 3 .
[0077] Table 1 shows the fisheye levels of the metallocene polyethylenes used for film materials obtained in the Examples and Comparative Examples.
[0078] As shown in Table 1, the fisheye index of the metallocene polyethylene (for membrane material) prepared by the production method provided in Examples 1 to 4 of the present invention in a shorter bed replacement cycle can meet the requirements, and the fisheye (0.8 mm) is ≤ 6 / 1520cm 2, fisheye (0.4 mm) ≤ 15 / 1520 cm 2 The production methods provided in Comparative Examples 1, 2 and 3, in which the fisheyes (0.4 mm) of the metallocene polyethylene prepared in a longer bed replacement cycle are all greater than 10 / 1520cm 2 , fisheyes (0.8 mm) are greater than 40 / 1520 cm 2 , which is obviously inferior to Examples 1 to 4.
[0079] Therefore, by comparing each embodiment with each comparative example, it can be known that each embodiment of the present invention evaluates the fisheye of the metallocene polyethylene rotomolding material or PE-RT pipe product by adopting the method of blowing film or casting after blending, and then generates the metallocene polyethylene for the film material after the fisheye meets the requirements. The fisheye level of the polyethylene film prepared by using the obtained metallocene polyethylene is qualified, indicating that this method can be used to correctly evaluate the fisheye level of the metallocene polyethylene rotomolding material or PE-RT pipe product, and then prompt the reasonable time to produce the metallocene polyethylene for the film material. In comparative examples 1 and 2, since the fisheye of the metallocene polyethylene rotomolding material or PE-RT pipe product is evaluated, it is impossible to accurately obtain the reasonable time to produce the metallocene polyethylene for the film material, resulting in the fisheye level of the metallocene polyethylene film material finally obtained being unqualified. In comparative example 3, since the metallocene polyethylene film material is directly produced in the conversion, the fisheye level of the metal polyethylene film material produced after 15 times BTO is still high. Since comparative example 3 has undergone more BTO, more transition materials are produced, and the transition materials cannot be sold as qualified products, thus causing the loss of corporate benefits.
[0080] Table 1 .
Claims
1. A method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene, characterized in that: The production method comprises the following steps: 1) Adjust the gas phase reactor of the chromium polyethylene to be converted to the conversion state, and then inject the terminator; 2) replacing the gas phase reactor of the chromium polyethylene to be converted, and then injecting a pretreatment agent; 3) Convert the transition material generated during the conversion process into metallocene polyethylene rotational molding products or PE-RT pipe products that do not require fisheyes; 4) evaluating the fisheye content of the metallocene polyethylene rotational molding product or PE-RT pipe product obtained in step 3); 5) When the fisheye content in the metallocene polyethylene rotational molding product or the PE-RT pipe product meets the requirements, the production parameters are adjusted according to the production parameters of the metallocene polyethylene used for the membrane material to convert the production of the metallocene polyethylene.
2. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 1, characterized in that: In step 1), adjusting the gas phase reactor of the chromium-based polyethylene to be converted to a conversion state comprises the following steps: Adjust the gas phase reactor of the chromium polyethylene to be converted from condensed production mode to dry operation mode; In the dry operation mode, the discharge frequency of the gas phase reactor discharge system of the chromium polyethylene to be converted is reduced to accumulate the bed weight to the quality required for the start-up of the metallocene; Reduce the catalyst injection amount to zero to allow the residual catalyst to be naturally consumed, reduce the reaction load, and complete the adjustment of the production conversion status.
3. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 2, characterized in that: In step 1), the terminator comprises at least one of CO2 and O2; or / and In step 2), the amount of the pretreatment agent added is 15 ppm to 25 ppm of the bed weight of the gas phase reactor of the chromium-based polyethylene to be converted.
4. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 3, characterized in that: In step 2), the pretreatment agent is circulated in the gas phase reactor of the chromium-based polyethylene to be converted for 1 h to 2 h.
5. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 1, characterized in that: In step 2), the pretreatment agent includes an antistatic agent, and the antistatic agent includes at least one of CA-300 and CA-200.
6. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 1, characterized in that: In step 2), the replacement adopts a boost pressure method, the low pressure of the boost pressure method is 600 kPa to 900 kPa; the high pressure of the boost pressure method is 1100 kPa to 1400 kPa; or / and The replacement is terminated when O2<8 ppm and CO2<8 ppm in the gas phase reactor of the chromium polyethylene to be converted; or In step 3), the transition material refers to a mixed product of the chromium-based polyethylene product and the metallocene polyethylene product produced in the process of replacing the chromium-based polyethylene bed layer, and a product whose quality does not meet the factory specifications.
7. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to any one of claims 1 to 6, characterized in that: In step 3), the conversion of the transition material produced in the conversion process into a metallocene polyethylene rotational molding product or a PE-RT pipe product comprises the following steps: According to the initiation conditions of metallocene polyethylene, the gas phase component concentration is re-established, and then the metallocene catalyst is injected to produce metallocene polyethylene rotational molding products or PE-RT pipe products with no requirements for fisheyes; among them, When producing metallocene polyethylene rotational molding products or PE-RT pipe materials, the corresponding gas phase components include at least one of N2, isopentane, ethylene, H2 and hexene-1.
8. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 7, characterized in that: In the step 3), when producing metallocene polyethylene rotational molding products or PE-RT pipe materials, the ethylene concentration is maintained at 60% to 75% and the catalyst activity is maintained at 4500 kg / kg to 6000 kg / kg; or / and In step 3), the melt index of the metallocene polyethylene rotomolding product is 3 to 6 g / 10 min, and the density is 0.935 g / cm 3 Up to 0.945 g / cm 3 Or, the melt index of the metallocene polyethylene PE-RT pipe material is 1g / 10 min to 2g / 10 min, and the density is 0.935g / cm 3 Up to 0.945 g / cm 3 .
9. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 7, characterized in that: Metallocene polyethylene rotomolding products that do not require fisheyes include mHD3605UA; or PE-RT pipe products that have no requirements for fisheyes include mHD3702.
10. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 7, characterized in that: The metallocene catalyst used in the production of metallocene polyethylene rotational molding products or metallocene polyethylene PE-RT pipe materials is a supported metallocene catalyst; the supported metallocene catalyst comprises methylaluminoxane and carrier silica gel, wherein the content of methylaluminoxane is 15% to 20%, and the specific surface area of the carrier silica gel is 250m 2 / g to 300 m 2 / g.
11. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to any one of claims 1 to 6, characterized in that: In step 4), the fisheye content of the metallocene polyethylene rotational molded product or PE-RT pipe product obtained in step 3) is evaluated by blow molding or casting after blending.
12. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 11, characterized in that: In step 4), the evaluation includes: blending the metallocene polyethylene rotational molding product or PE-RT pipe material into qualified metallocene polyethylene for preparing membrane materials at a rate of 10% to 50%, preparing polyethylene film products by blow molding or casting, observing the reduction of fish eyes, and judging the products as qualified after there are no fish eyes or only a few small fish eyes.
13. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 12, characterized in that: In step 4), as the fisheyes of the polyethylene film product in the evaluation decrease, the blending ratio of the metallocene polyethylene rotomolding product or PE-RT pipe material and the qualified metallocene polyethylene for preparing the film material increases.
14. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to any one of claims 1 to 6, characterized in that: In step 5), adjusting the production parameters includes adjusting the gas phase components, and the gas phase components include at least one of N2, isopentane, ethylene, H2 and hexene-1.
15. The method for producing a transition material for reducing chromium-based polyethylene to produce metallocene polyethylene according to claim 14, characterized in that: In the step 5), the H2 partial pressure in the reactor is reduced to 0.3 kPa to 0.8 kPa, and the hexene-1 partial pressure in the reactor is increased to 8 kPa to 12 kPa.
Citation Information
Patent Citations
Converting method of polyvinyl acetate with different polymerization degrees
CN102863572A
Production conversion method of polyethylene
CN117343224A
Method for converting low-melt-flow-rate polyethylene into high-melt-flow-rate polyethylene
CN117343225A
Method for continuously converting chromium-based hollow material into chromium-based film material polyethylene
CN117534785A
Production method for converting chromium polyethylene into metallocene polyethylene
CN117567675A