High-refractive-index 1.67 resin lens monomer and preparation process thereof
By using components such as triethylene glycol diacrylate, modified styrene and thiol acrylate, a resin lens monomer with a refractive index of 1.67 was prepared, which solved the problems of heavy and discomfort in traditional resin lenses, and achieved the goal of achieving the The high refractive index and weather resistance are improved to meet the visual needs of users of high-level numbers.
Patent Information
- Application Number
- CN202411072142.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
Due to its thickness and discomfort, traditional 1.50 refractive index resin lenses are difficult to meet the visual comfort and aesthetic needs of users of heights, and lack high refractive index materials to replace them.
Using triethylene glycol diacrylate, modified styrene, thiol acrylate and benzoyl peroxide, a resin lens monomer with a refractive index of 1.67 is prepared through a specific preparation process to improve the material. optical density, weather resistance and chemical stability.
The preparation of high-refractive index resin lenses is realized, reducing the thickness and weight of the lenses, improving the comfort and aesthetics of wear, and improving mechanical strength and thermal stability.
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of a resin lens monomer, and more specifically to a resin lens monomer with a high refractive index of 1.67 and a preparation process thereof. Background Art
[0002] In the field of modern optics, the selection of lens materials is crucial for vision correction and visual comfort. With the improvement of people's living standards and the increase in the demand for visual quality, high-refractive-index resin lenses have gradually become the mainstream products in the market due to their superior optical performance and physical properties. In particular, resin lenses with a refractive index of 1.67 are favored by the majority of users because of their advantages in reducing the thickness and weight of lenses.
[0003] Traditional resin lenses are mainly made of materials such as CR-39, and their refractive index is generally around 1.50. Although this material has good light transmittance and impact resistance, for users with high degrees of vision, the lenses will appear too thick and heavy, affecting the comfort and aesthetics of wearing. Therefore, the development of high-refractive-index resin materials has become a major research direction in the field of eyeglasses. Summary of the invention
[0004] In order to solve the problems existing in the prior art, a high refractive index 1.67 resin lens monomer and its preparation process are provided. The specific scheme is as follows:
[0005] A high refractive index 1.67 resin lens monomer, the resin lens monomer comprising the following components in percentage by weight:
[0006] Triethylene glycol diacrylate 70-80wt%;
[0007] Modified styrene; 10-15wt%;
[0008] Thiol acrylate 5-10wt%;
[0009] Ultraviolet absorber 0.5-1wt%;
[0010] Benzoyl peroxide 0.5-1wt%.
[0011] Furthermore, the preparation method of the modified styrene comprises the following steps:
[0012] S1: Add THF to the reactor, add anthracene and stir until completely dissolved;
[0013] S2: Slowly add aluminum chloride to the solution and stir for 30 minutes to ensure that the catalyst is fully dissolved and activated;
[0014] S3: Slowly add styrene dropwise under stirring;
[0015] S4: After the reaction is completed, slowly add titanium trichloride as a reducing agent and continue stirring;
[0016] S5: Finally, evaporation, precipitation, washing and drying are performed to obtain modified styrene.
[0017] Furthermore, in S3, the reaction temperature is controlled to be 25° C. and the reaction time is controlled to be 2 h.
[0018] Further, the styrene was dried in a vacuum drying oven at 50° C. for 12 hours to obtain modified styrene.
[0019] A preparation process of a resin lens monomer with a high refractive index of 1.67, comprising the following steps:
[0020] S1: Add all monomers into the reactor according to the ratio;
[0021] S2: react at 70-80°C for 2 hours to ensure that the monomers are fully mixed; slowly add initiator benzoyl peroxide and continue to react for 3 hours to ensure that the monomers are completely polymerized;
[0022] S3: After the reaction is completed, pour the reaction liquid into a mold; dry it at 60° C. for 24 hours to obtain a resin lens monomer.
[0023] Furthermore, the temperature in the reactor in S1 is controlled at 70-80°C; and the stirring speed is maintained at 100-200 rpm.
[0024] Further, the polymerization reaction steps of the resin lens monomer are as follows:
[0025] S1: injecting resin monomer liquid into the mold;
[0026] S2: Place the mold into a polymerization reactor, set the temperature to 100°C, and the reaction time to 4 hours, during which the temperature is maintained constant and stirred appropriately;
[0027] S3: After the polymerization reaction is completed, the mold is taken out and cooled to room temperature.
[0028] Beneficial effects:
[0029] The present invention provides a high refractive index 1.67 resin lens monomer and a preparation process thereof, which specifically include the following advantages:
[0030] Triethylene glycol diacrylate is used as a base monomer in the formula. Due to its high optical transparency and good chemical stability, it effectively improves the refractive index of the resin lens. Modified styrene increases the density of the benzene ring through the special design of the molecular structure, enhances the optical density of the material, and further improves the refractive index. Compared with traditional styrene, modified styrene not only improves the refractive index, but also improves the weather resistance and chemical stability of the material. The use of thiol acrylate as a cross-linking agent not only improves the mechanical strength of the lens, but also improves the thermal stability and chemical resistance of the material through moderate cross-linking. DETAILED DESCRIPTION
[0031] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0032] Embodiment 1:
[0033] Step 1: Prepare the ingredients
[0034] Triethylene glycol diacrylate: 75wt%
[0035] Modified styrene: 12wt%
[0036] Thiol acrylate: 8wt%
[0037] UV absorber: 0.75wt%
[0038] Benzoyl peroxide: 0.75wt%
[0039] Step 2: Preparation of modified styrene
[0040] 1. Add 100 ml of THF into the reactor, add 1 g of anthracene and stir until completely dissolved.
[0041] 2. Slowly add 3g of aluminum chloride to the solution and stir for 30 minutes to ensure that the catalyst is fully dissolved and activated.
[0042] 3. Under stirring conditions, slowly add 10g of styrene, the reaction temperature is controlled at 25°C, and the reaction time is 2 hours.
[0043] 4. After the reaction is completed, slowly add 1g of titanium trichloride as a reducing agent and continue stirring for 30 minutes.
[0044] 5. The modified styrene was obtained by evaporation, precipitation, washing and drying in a vacuum oven at 50°C for 12 hours.
[0045] Step 3: Preparation of resin lens monomer
[0046] 1. Add triethylene glycol diacrylate, modified styrene, mercaptan acrylate, ultraviolet absorber and benzoyl peroxide into the reactor according to the proportion.
[0047] 2. React at 70-80°C for 2 hours to ensure that the monomers are fully mixed; slowly add initiator benzoyl peroxide and continue to react for 3 hours to ensure that the monomers are completely polymerized.
[0048] 3. After the reaction is completed, pour the reaction liquid into a mold; dry it at 60°C for 24 hours to obtain a resin lens monomer.
[0049] Embodiment 2:
[0050] Step 1: Prepare the ingredients
[0051] Triethylene glycol diacrylate: 78wt%
[0052] Modified styrene: 10wt%
[0053] Thiol acrylate: 8wt%
[0054] UV absorber: 0.6wt%
[0055] Benzoyl peroxide: 0.4wt%
[0056] Step 2: Preparation of modified styrene
[0057] 1. Add 200 ml of THF into the reactor, add 2 g of anthracene and stir until completely dissolved.
[0058] 2. Slowly add 6 g of aluminum chloride to the solution and stir for 30 minutes to ensure that the catalyst is fully dissolved and activated.
[0059] 3. Under stirring conditions, slowly add 20g of styrene, the reaction temperature is controlled at 25°C, and the reaction time is 2 hours.
[0060] 4. After the reaction is completed, slowly add 2 g of titanium trichloride as a reducing agent and continue stirring for 30 minutes.
[0061] 5. The modified styrene was obtained by evaporation, precipitation, washing and drying in a vacuum oven at 50°C for 12 hours.
[0062] Step 3: Preparation of resin lens monomer
[0063] 1. Add triethylene glycol diacrylate, modified styrene, mercaptan acrylate, ultraviolet absorber and benzoyl peroxide into the reactor according to the proportion.
[0064] 2. React at 75°C for 2 hours to ensure that the monomers are fully mixed; slowly add initiator benzoyl peroxide and continue to react for 3 hours to ensure that the monomers are completely polymerized.
[0065] 3. After the reaction is completed, pour the reaction liquid into a mold; dry it at 60°C for 24 hours to obtain a resin lens monomer.
[0066] Example 3
[0067] Step 1: Prepare the ingredients
[0068] Triethylene glycol diacrylate: 70wt%
[0069] Modified styrene: 15wt%
[0070] Thiol acrylate: 10wt%
[0071] UV absorber: 1wt%
[0072] Benzoyl peroxide: 1wt%
[0073] Step 2: Preparation of modified styrene
[0074] 1. Add 150 ml of THF into the reactor, add 1.5 g of anthracene and stir until completely dissolved.
[0075] 2. Slowly add 4.5 g of aluminum chloride to the solution and stir for 30 minutes to ensure that the catalyst is fully dissolved and activated.
[0076] 3. Under stirring conditions, slowly add 15 g of styrene, the reaction temperature is controlled at 25°C, and the reaction time is 2 hours.
[0077] 4. After the reaction is completed, slowly add 1.5 g of titanium trichloride as a reducing agent and continue stirring for 30 minutes.
[0078] 5. The modified styrene was obtained by evaporation, precipitation, washing and drying in a vacuum oven at 50°C for 12 hours.
[0079] Step 3: Preparation of resin lens monomer
[0080] 1. Add triethylene glycol diacrylate, modified styrene, mercaptan acrylate, ultraviolet absorber and benzoyl peroxide into the reactor according to the proportion.
[0081] 2. React at 80°C for 2 hours to ensure that the monomers are fully mixed; slowly add initiator benzoyl peroxide and continue to react for 3 hours to ensure that the monomers are completely polymerized.
[0082] 3. After the reaction is completed, pour the reaction liquid into a mold; dry it at 60°C for 24 hours to obtain a resin lens monomer.
[0083] After testing, the refractive index of the lens prepared from the resin lens monomers of Examples 1 to 3 was 1.67.
[0084] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high refractive index 1.67 resin lens monomer, It is characterized in that The resin lens monomer comprises the following components in percentage by weight: Triethylene glycol diacrylate 70-80wt%; Modified styrene; 10-15wt%; Thiol acrylate 5-10wt%; Ultraviolet absorber 0.5-1wt%; Benzoyl peroxide 0.5-1wt%.
2. A high refractive index 1.67 resin lens monomer according to claim 1, It is characterized in that The preparation method of the modified styrene comprises the following steps: S1: Add THF to the reactor, add anthracene and stir until completely dissolved; S2: Slowly add aluminum chloride to the solution and stir for 30 minutes to ensure that the catalyst is fully dissolved and activated; S3: Slowly add styrene dropwise under stirring; S4: After the reaction is completed, slowly add titanium trichloride as a reducing agent and continue stirring; S5: Finally, evaporation, precipitation, washing and drying are performed to obtain modified styrene.
3. A high refractive index 1.67 resin lens monomer according to claim 2, It is characterized in that In S3, the reaction temperature is controlled at 25°C and the reaction time is 2h.
4. The high refractive index 1.67 resin lens monomer according to claim 2, It is characterized in that Styrene was dried in a vacuum drying oven at 50°C for 12 hours to obtain modified styrene.
5. A process for preparing a high refractive index 1.67 resin lens monomer as claimed in any one of claims 1 to 4, It is characterized in that The following steps are involved: S1: Add all monomers into the reactor according to the ratio; S2: react at 70-80°C for 2 hours to ensure that the monomers are fully mixed; slowly add initiator benzoyl peroxide and continue to react for 3 hours to ensure that the monomers are completely polymerized; S3: After the reaction is completed, pour the reaction liquid into a mold; dry it at 60° C. for 24 hours to obtain a resin lens monomer.
6. The process for preparing a high refractive index 1.67 resin lens monomer according to claim 5, It is characterized in that The temperature in the reactor in S1 is controlled at 70-80°C; the stirring speed is maintained at 100-200 rpm.
7. The process for preparing a high refractive index 1.67 resin lens monomer according to claim 5, It is characterized in that The polymerization reaction steps of resin lens monomer are as follows: S1: injecting resin monomer liquid into the mold; S2: Place the mold into a polymerization reactor, set the temperature to 100°C, and the reaction time to 4 hours, during which the temperature is maintained constant and stirred appropriately; S3: After the polymerization reaction is completed, the mold is taken out and cooled to room temperature.