Contact lens and silicone glue contact lens

By using silicone monomers and polyacrylic acid or sodium polyacrylate formulas in silicone water glue contact lenses, the problems of low oxygen permeability and high production cost of soft contact lenses are solved, and high oxygen permeability and low cost are achieved. Silicone hydroglue contact lens, suitable for long-term wear.

CN118994496APending Publication Date: 2024-11-22VIZIONFOCUS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311375129.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-16
Filing Date
2023-10-23
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing soft contact lens materials have low oxygen permeability, which leads to hypoxia of the cornea during long-term wear, causing discomfort. The traditional surface treatment process is complex or costly, limiting the efficient and low-cost silicone hydroglue contact lens production.

Method used

Using a silicone water glue contact lens formula containing at least one silicone monomer and polyacrylic acid or sodium polyacrylate, the high molecular weight of polyacrylic acid or sodium polyacrylate is combined with the high molecular weight of polyacrylic acid or sodium polyacrylate to improve the visibility of the lens by combining specific monomers and crosslinking agents. Water-based and durable, reducing production costs.

Benefits of technology

It achieves high oxygen permeability and suitable for long-term wear, which reduces production costs, improves the hydrophilicity and durability of the lenses, and reduces the discomfort of wearing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994496A_ABST
    Figure CN118994496A_ABST
Patent Text Reader

Abstract

A contact lens contains at least one silicon-containing monomer, the surface of the contact lens contains polyacrylic acid and / or sodium polyacrylate, and the molecular weight of the polyacrylic acid and / or sodium polyacrylate is greater than 100 kDa. The invention also provides a silicon hydrogel contact lens. The contact lens and the silicone hydrogel contact lens provided by the invention have the advantages of good hydrophilicity and suitability for long-time wearing of consumers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a contact lens and a silicone hydrogel contact lens, in particular to a surface-treated contact lens and a silicone hydrogel contact lens. Background Art

[0002] Soft contact lens materials were introduced in the 1960s. The softness of the material solved the discomfort often experienced by hard contact lenses (RGP lenses) when worn. Users who were not used to hard contact lenses could switch to soft contact lenses, making them the main choice for contact lens users today.

[0003] However, the materials traditionally used for soft contact lenses (mainly composed of HEMA, generally referred to as hydrogel materials) have low oxygen permeability, with a general Dk (oxygen permeability) of only 8-20. This causes consumers (or users; contact lens users) to often experience bloodshot eyes and corresponding discomfort at the end of a day's wear (wearing for more than 10 hours) due to lack of oxygen. Therefore, the research and development of contact lens materials has shifted to seeking high oxygen permeability materials. Around 2000, soft contact lens products containing silicon components began to appear on the market, that is, contact lens products made of silicone hydrogel materials, generally referred to as silicone hydrogel contact lenses. Compared with traditional hydrogel materials, silicone hydrogel materials have higher oxygen permeability and can solve problems such as corneal hypoxia.

[0004] The main technical threshold of silicone hydrogel contact lenses is how to make the lenses sufficiently hydrophilic to avoid discomfort caused by the hydrophobicity of the silicone component. The industry generally uses the contact angle to judge the hydrophilicity of the lens surface. The industry first developed plasma technology to treat the surface of lenses, such as patent documents US20030039748 and US5760100. However, this technology requires a complicated process and the lens production cost is relatively high. In addition, polyvinylpyrrolidone (PVP) is added to the formula as an internal wetting agent, such as patent documents US6367929, US6943203, US7052131, US7249848, US7473738, US7473738, and US7691916. This method avoids the complicated process of plasma surface treatment, but there are many limitations in the lens formula. In addition to the above two technologies, some researchers have also developed formulation technologies that do not require plasma surface treatment and do not require the additional addition of PVP as an internal wetting agent, such as patent documents US7750079, US8129442, US8231218, US8476337, and EP195584. This type of formulation technology requires a specific silicon-containing monomer, a specific hydrophilic monomer, and a specific filler (diluents) combination to achieve the desired lens properties, and usually requires a specific mold material for contact lens production. These limitations limit the optimization of product production costs.

[0005] Therefore, it is necessary to design a set of contact lenses that can meet consumer needs, be suitable for long-term wear, and be convenient for large quantities, high quality, and cost-competitive. Summary of the invention

[0006] The present invention provides a contact lens which is suitable for consumers to wear for a long time and is convenient for mass production.

[0007] The present invention further provides a silicone hydrogel contact lens which is suitable for consumers to wear for a long time and is easy to mass produce.

[0008] To achieve the above advantages, one embodiment of the present invention provides a contact lens comprising at least one silicon-containing monomer, and the surface of the contact lens comprises polyacrylic acid and / or sodium polyacrylate, wherein the molecular weight of the polyacrylic acid and / or sodium polyacrylate is preferably greater than 100 kDa, more preferably greater than 200 kDa, and more preferably greater than 450 kDa.

[0009] To achieve the above advantages, another embodiment of the present invention provides a silicone hydrogel contact lens, comprising a first silicon-containing monomer, a second silicon-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer, and a silicon-containing crosslinking agent. The surface of the silicone hydrogel contact lens comprises polyacrylic acid and / or sodium polyacrylate. The molecular weight of the polyacrylic acid and / or sodium polyacrylate is preferably greater than 100 kDa, more preferably greater than 200 kDa, and more preferably greater than 450 kDa.

[0010] The first silicon-containing monomer mentioned above has the following structure;

[0011]

[0012] Where A is the following structure:

[0013]

[0014] or the following structure:

[0015]

[0016] Wherein R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structure or a combination thereof:

[0017] (CH2) n1 , (C m1 H 2m1 O m2 ) m3 or

[0018] Where n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.

[0019] The second silicon-containing monomer contains the first structure or the second structure;

[0020] The first structure mentioned above:

[0021]

[0022] Wherein a is 0-20; R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:

[0023] (CH2) n6 , (C m7 H 2m7 O m8 ) m9 , or (CH2) n7NHCO(O m13 C m14 H 2m14 ) m15

[0024] Among them, n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4;

[0025] The second structure mentioned above:

[0026]

[0027] Where c is 0-20; where R 10 is H or CH3 or C2H5, R 11 is H or CH3 or OSi(CH3)3, R 12 is H or CH3 or OSi(CH3)3, L5 is the following structure or a combination thereof: O or NH;

[0028] L6 is the following structure or a combination thereof:

[0029] (CH2) n20 , (C m34 H 2m34 O m35 ) m36 or

[0030] Among them n20 is 1-5, m34 is 1-4, m35 is 0-1, m36 is 1-4, m37 is 0-1, m38 is 1-4, and m39 is 1-4.

[0031] The first hydrophilic monomer is a hydrophilic monomer containing an N-vinyl group, and the second hydrophilic monomer is different from the first hydrophilic monomer.

[0032] The first silicon-containing monomer includes at least one of methacryloxypropyl tris(trimethylsiloxy)silane, 3-(3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxane)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.

[0033] The second silicon-containing monomer comprises at least one of monomethacryloxypropyl terminated polydimethylsiloxane, monomethacryloxypropyl terminated urethane polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropoxy)propyl terminated monobutyl terminated polydimethylsiloxane. The molecular weight of the second silicon-containing monomer is 350-2500, preferably 500-1500.

[0034] The silicone hydrogel contact lens further comprises a filler, and the total content of the first silicon-containing monomer and the second silicon-containing monomer accounts for 15%-60% of the weight of the silicone hydrogel contact lens after deducting the filler, and more preferably 25%-45%.

[0035] The first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide.

[0036] The silicone hydrogel contact lens further comprises a filler, and the content of the first hydrophilic monomer accounts for 30%-65% by weight of the silicone hydrogel contact lens after deducting the filler, and more preferably 35%-55%.

[0037] The second hydrophilic monomer includes hydroxyethyl methacrylate.

[0038] The above-mentioned silicon-containing crosslinking agent comprises the following structure:

[0039]

[0040] Wherein b is 0-20; R6 is H or CH3 or C2H5, R7 is H or CH3 or OSi(CH3)3, and L3 is the following structure or a combination thereof:

[0041] (CH2) n12 , (C m16 H 2m16 O m17 ) m18 , or (CH2) n13 NHCO(O m22 C m23 H 2m23 ) m24

[0042] Among them, n12 is 1-5, n13 is 1-5, m16 is 1-4, m17 is 0-1, m18 is 1-4, m19 is 0-1, m20 is 1-4, m21 is 1-4, m22 is 0-1, m23 is 1-4, and m24 is 1-4;

[0043] R8 is the following structure or a combination thereof:

[0044]

[0045] Wherein R9 is H or CH3 or C2H5, L4 is the following structure or a combination thereof:

[0046] (CH2) n18 , (C m25 H 2m25 O m26 ) m27 , or (CH2) n19 NHCO(O m31 C m32 H 2m32 ) m33

[0047] Where n18 is 1-5, n19 is 1-5, m25 is 1-4, m26 is 0-1, m27 is 1-4, m28 is 0-1, m29 is 1-4, m30 is 1-4, m31 is 0-1, m32 is 1-4, and m33 is 1-4.

[0048] The above-mentioned silicon-containing crosslinking agent comprises the following structure:

[0049]

[0050] Wherein d is 0-20; R13 is H or CH3 or C2H5, R14 is H or CH3 or C2H5, L7 is the following structure or a combination thereof: O or NH;

[0051] L8 is the following structure or a combination thereof:

[0052] (CH2) n25 , (C m40 H 2m40 O m41 ) m42 or

[0053] Among them, n25 is 1-5, m40 is 1-4, m41 is 0-1, m42 is 1-4, m43 is 0-1, m44 is 1-4, and m45 is 1-4;

[0054] R 15 Is the following structure or a combination of them:

[0055]

[0056] Wherein R16 is H or CH3 or C2H5, L9 is the following structure or a combination thereof:

[0057] (CH2) n31 , (C m46 H 2m46 O m47 ) m48 or

[0058] Among them n31 is 1-5, m46 is 1-4, m47 is 0-1, m48 is 1-4, m49 is 0-1, m50 is 1-4, and m51 is 1-4.

[0059] The silicon-containing crosslinking agent includes at least one of methacryloxypropyl terminated polydimethylsiloxane, methacryloxypropyl terminated urethane polydimethylsiloxane, methacryloxypropyl terminated polydimethylsiloxane modified with polyethylene glycol, 1,3-bis[4-vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropoxypropyl polydimethylsiloxane. The molecular weight of the silicon-containing crosslinking agent is between 500 and 3000.

[0060] The silicone hydrogel contact lens further comprises at least one non-silicon-containing crosslinking agent, wherein the at least one non-silicon-containing crosslinking agent comprises at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and trimethylolpropane trimethacrylate.

[0061] The above-mentioned contact lens is a silicone hydrogel contact lens, whose contact angle (Contact Angle) is less than or equal to 60°, and the water breaking time (WBUT) is greater than or equal to 20 seconds, and after being worn for about 8 to 10 hours, the tear film breakup time can still be greater than about 15 seconds.

[0062] The contact lens and silicone hydrogel contact lens of the embodiments of the present invention have at least one silicon-containing monomer, and the surface of the contact lens and silicone hydrogel contact lens includes polyacrylic acid and / or sodium polyacrylate, wherein the molecular weight of polyacrylic acid and / or sodium polyacrylate is greater than 100 kDa. Therefore, the prepared contact lens and silicone hydrogel contact lens have the advantages of good hydrophilicity and are suitable for consumers to wear for a long time.

[0063] In order to make the above and other purposes, features and advantages of the present invention more clearly understood, embodiments are given below with reference to the accompanying drawings for detailed description as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 FIG. 4 is a schematic cross-sectional view of a contact lens according to an embodiment of the present invention.

[0065] Figure 2 The figure is a schematic flow chart of a method for manufacturing a contact lens according to an embodiment of the present invention. DETAILED DESCRIPTION

[0066] An embodiment of the present invention provides a contact lens 100 . The contact lens 100 includes a lens body 110 . The lens body 110 contains at least one silicon-containing monomer. The surface of the contact lens 100 includes polyacrylic acid and / or sodium polyacrylate 120 . Figure 1 FIG. 1 is a cross-sectional schematic diagram of a contact lens according to an embodiment of the present invention. Figure 1 Specifically, polyacrylic acid and / or sodium polyacrylate 120 is a thin film covering the lens body 110, and this thin film is the surface of the contact lens 100. The surface of the contact lens 100 may include a convex surface, a concave surface or a combination thereof. Since polyacrylic acid and sodium polyacrylate 120 are hydrophilic, when used as the surface of the contact lens 100, the hydrophilicity of the contact lens 100 can be increased. In addition, the surface of the contact lens 100, for example, does not contain a polymer other than polyacrylic acid or sodium polyacrylate 120 and having an opposite charge to that of polyacrylic acid or sodium polyacrylate. In other words, the contact lens 100 of this embodiment, for example, only has the thin film formed by polyacrylic acid and / or sodium polyacrylate 120 covering the lens body 110. The molecular weight of polyacrylic acid and / or sodium polyacrylate 120 is preferably greater than about 100 kDa, more preferably greater than about 200 kDa, and more preferably greater than about 450 kDa. Specifically, the contact lens 100 is, for example, a silicone hydrogel contact lens, wherein the lens body 110 of the contact lens 100 may include a first silicon-containing monomer, a second silicon-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer and a silicon-containing crosslinking agent.

[0067] The first silicon-containing monomer has the following structure:

[0068]

[0069] Where A is the following structure:

[0070]

[0071] or the following structure:

[0072]

[0073] Wherein R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structure or a combination thereof:

[0074] (CH2) n1 , (C m1 H 2m1 O m2 ) m3 or

[0075] Where n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.

[0076] The second silicon-containing monomer contains the following first structure or second structure:

[0077] The first structure is:

[0078]

[0079] Wherein a is 0-20; R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:

[0080] (CH2) n6 , (C m7 H 2m7 O m8 ) m9 , or (CH2) n7 NHCO(O m13 C m14 H 2m14 ) m15

[0081] Among them, n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4;

[0082] The second structure is:

[0083]

[0084] Where c is 0-20; where R 10 is H or CH3 or C2H5, R 11 is H or CH3 or OSi(CH3)3, R 12 is H or CH3 or OSi(CH3)3, L5 is the following structure or a combination thereof: O or NH;

[0085] L6 is the following structure or a combination thereof:

[0086] (CH2) n20 , (C m34 H 2m34 O m35 ) m36 or

[0087] Among them, n20 is 1-5, m34 is 1-4, m35 is 0-1, m36 is 1-4, m37 is 0-1, m38 is 1-4, and m39 is 1-4;

[0088] The first hydrophilic monomer contains N-vinyl. The second hydrophilic monomer is different from the first hydrophilic monomer. The second hydrophilic monomer preferably contains hydroxyethyl methacrylate (HEMA).

[0089] The contact angle (Contact Angle) of the contact lens is less than or equal to 60°, and the water breaking time (WBUT) is greater than or equal to 20 seconds, and after being worn for about 8 to 10 hours, the tear film breakup time can still be greater than about 15 seconds.

[0090] Herein, contact lenses may refer to hydrated contact lenses or hydrated and sterilized contact lenses. Herein, lenses may be interchangeable with contact lenses in some contexts, and lenses may refer to lens bodies or dry lenses (dry lenses) that have not been hydrated in some contexts. In addition, the lens formulation (referred to as formulation) herein refers to a formulation consisting of monomers, crosslinking agents, and initiators, and may also contain fillers if necessary. "Monomer" is used to refer to a lens formulation that can be polymerized in the curing process through free radical polymerization to further form a polymer. Monomers generally have double bonds that can accept free radicals in their chemical structure.

[0091] "Silicone monomer" refers to a monomer that has at least one chemical structure of silicon-oxygen bonding (-Si-O-). Examples of the silicon-containing monomers that can be used in this embodiment include: 3-[Tris(trimethylsiloxy)silyl]propylmethacrylate, TRIS for short; and monomethacryloxypropylterminatedpolydimethylsiloxane (MPDMS for short). The CAS No. of the commonly used monomethacryloxypropylterminatedpolydimethylsiloxane is 146632-07-7. Other silicon-containing monomers that can be used in this embodiment include, but are not limited to: 2-(Trimethylsilyloxy)ethylmethacrylate (2-(Trimethylsilyloxy)ethyl methacrylate), 3-(3-Methacryloxy-2-hydroxypropoxy)propylbis(trimethylsiloxy)methylsilane (SiGMA), (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane, Methacryloxymethylphenethyltris(trimethylsiloxy)silane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate, 3-[Tris(trimethylsiloxy)silyl]propyl vinylcarbamate The silicon-containing monomers can be purchased from suppliers such as Sigma-Aldrich, Gelest, JNC, Shin-Etsu, Pharnocia, and Bimax.The silicon-containing monomer that can be used in this embodiment is also, for example, mono-(3-methacryloxy-2-hydroxypropyloxy)propyl terminated, mono-butylterminated polydimethylsiloxane, which can be synthesized by referring to the method in U.S. Patent No. 20030162862A1. Silicon-containing monomers that can be used in this embodiment include, for example, urethane esters of monoCarbinol terminated polydimethylsiloxane (CAS No: 207308-30-3, MOHPMDS) and 2-isocyanatoethylmethacrylate (IEM). The synthesis reaction of urethane esters can use 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) as a catalyst.

[0092] The first silicon-containing monomer may contain the following structure;

[0093]

[0094] Where A is the following structure:

[0095]

[0096] or the following structure:

[0097]

[0098] Wherein R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structure or a combination thereof:

[0099] (CH2) n1 , (C m1 H 2m1 O m2 ) m3 or

[0100] Where n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4.

[0101] In the present embodiment, the first silicon-containing monomer includes, for example, at least one of methacryloxypropyl tris(trimethylsiloxy)silane, 3-(3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxane)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.

[0102] The second silicon-containing monomer includes, for example, at least one of monomethacryloxypropyl terminated polydimethylsiloxane, monomethacryloxypropyl terminated urethane polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropoxy)propyl terminated monobutyl terminated polydimethylsiloxane. In addition, the molecular weight of the second silicon-containing monomer may be 350-2500, preferably 500-1500.

[0103] The second silicon-containing monomer contains a first structure or a second structure;

[0104] The first structure is:

[0105]

[0106] Wherein a is 0-20; R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof:

[0107] (CH2) n6 , (C m7 H 2m7 O m8 ) m9 , or (CH2) n7 NHCO(O m13 C m14 H 2m14 ) m15

[0108] Among them, n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4;

[0109] The second structure is:

[0110]

[0111] Where c is 0-20; where R 10 is H or CH3 or C2H5, R 11is H or CH3 or OSi(CH3)3, R 12 is H or CH3 or OSi(CH3)3, L5 is the following structure or a combination thereof: O or NH;

[0112] L6 is the following structure or a combination thereof:

[0113] (CH2) n20 , (C m34 H 2m34 O m35 ) m36 or

[0114] Among them, n20 is 1-5, m34 is 1-4, m35 is 0-1, m36 is 1-4, m37 is 0-1, m38 is 1-4, and m39 is 1-4;

[0115] The first hydrophilic monomer is a hydrophilic monomer containing an N-vinyl group, such as N-vinylpyrrolidone and N-methyl-N-vinylacetamide.

[0116] The total content of the first silicon-containing monomer and the second silicon-containing monomer is, for example, 15%-60% by weight of the contact lens after deducting the filler, preferably 25%-45%.

[0117] “Hydrophilic monomer” refers to a monomer that has a relatively hydrophilic chemical structure. The hydrophilic monomers that can be used in this embodiment include, but are not limited to: N-vinylpyrrolidone (NVP), N-methyl-N-vinylacetamide (MVA), N,N-dimethylacrylamide (DMA), N,N-diethylacrylamide, N-(Hydroxymethyl)acrylamide, N-hydroxyethylacrylamide, 2-Hydroxyethylmethacrylate (HEMA), ethylene glycol vinyl ether (EGVE), 1,4-butanediol vinyl ether (BVE), di(ethylene glycol)vinyl ether, hydroxypropyl ...1,4-butanediol vinyl ether (BVE), di(ethylene glycol)vinyl ether, hydroxypropyl methacrylate (HEMA), 1,4-butanediol vinyl ether (BVE), di(ethylene glycol)vinyl ether, hydroxypropyl methacrylate (HEMA), 1,4- methacrylate and / or Hydroxyisopropyl methacrylate), 2-methyl-2-acrylic acid-2-hydroxybutyl ester (Hydroxybutylmethacrylate, referred to as HOBMA), Poly(propylene ethylene glycol)methacrylate), Poly(ethpropylene glycol)acrylate, 2-methyl-2-acrylic acid-2,3-Dihydroxypropyl (Glyceryl methacrylate), Glycidyl methacrylate, 2-Hydroxyethyl acrylate, Hydroxypropyl acrylate and / or Hydroxyisopropyl acrylate, 4-Hydroxybutyl acrylate, Glyceryl acrylate, N-[Tris(hydroxymethyl)methyl]acrylamide, Methacrylamide, 2-Hydroxypropyl methacrylamide, N-Isopropylacrylamide, N,N-Diethylacrylamide, N-Ethylacrylamide, 2-Ethoxyethyl Methacrylate In this embodiment, the preferred hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA). A better choice is a combination of N-vinylpyrrolidone (NVP) and hydroxyethyl methacrylate (HEMA), or a combination of N-methyl-N-vinylacetamide (MVA) and hydroxyethyl methacrylate (HEMA). The above hydrophilic monomers can generally be purchased from suppliers such as Sigma-Aldrich, TCI, Alfa Aesar, etc. In addition to "hydrophilic monomers", "hydrophobic monomers" can also be selectively added to the formula, which are usually used to adjust the mechanical properties of the lens, such as adding methyl methacrylate (MMA) in some embodiments of the present invention. ,

[0118] In one embodiment of the present invention, the first hydrophilic monomer is, for example, N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA). In addition, the first hydrophilic monomer accounts for 30%-65% of the weight of the contact lens after deducting the filler.

[0119] In one embodiment of the present invention, the first hydrophilic monomer is, for example, N-vinylpyrrolidone or N-methyl-N-vinylacetamide (MVA). In addition, the first hydrophilic monomer accounts for 35%-55% of the weight of the contact lens after deducting the filler.

[0120] In one embodiment of the present invention, the second hydrophilic monomer includes at least one of hydroxyethyl methacrylate (HEMA), ethylene glycol vinyl ether, and 1,4-butanediol vinyl ether. Among them, hydroxyethyl methacrylate (HEMA) has the best effect. Although there is no detailed theoretical framework explanation at present, and the inventor does not want to limit the invention to certain theoretical frameworks, the unexpected discovery of the present invention may be that the hydroxyl group in the structure of hydroxyethyl methacrylate (HEMA) and the silicon-containing polymer structure formed by the first hydrophilic monomer containing N-vinyl can form appropriate hydrogen bonds or van der Waals forces with polyacrylic acid and / or sodium polyacrylate, thereby helping polyacrylic acid and / or sodium polyacrylate to be more stably adsorbed on the lens surface, or to form entanglement with the polymer structure on the lens surface after being adsorbed on the lens surface, so that polyacrylic acid and / or sodium polyacrylate can stay on the lens surface more stably, making the contact lens better and more suitable for wearing.

[0121] "UV Blocker" refers to a component added to the lens to block UV wavelength light. The UV blocker generally used for contact lenses also has a double bond that can accept free radicals in the chemical structure, so it also belongs to the category of monomers. The UV blockers that can be used in this embodiment include, but are not limited to: 2-[3-(2H-Benzotriazol-2-yl)-4-hydroxyphenyl]ethyl methacrylate (2-[3-(2H-Benzotriazol-2-yl)-4-hydroxyphenyl]ethyl methacrylate, referred to as HMEPB), 2-(4-Benzoyl-3-hydroxyphenoxy)ethyl acrylate. The above-mentioned UV blockers can generally be purchased from suppliers such as Sigma-Aldrich, TCI, Alfa Aesar, etc.

[0122] In this embodiment, the contact lens may further include at least one non-silicon-containing crosslinking agent.

[0123] "Crosslinking agent" refers to a crosslinking agent that can cause monomers to undergo crosslinking reactions during polymerization reactions, and can provide the polymer produced by the polymerization reaction with the desired crosslinking density, so that two polymer chains react and bond to form a network polymer. The crosslinking agent can be divided into non-silicon-containing crosslinking agents and silicon-containing crosslinking agents based on whether it has a chemical structure of silicon-oxygen bonding (-Si-O-). The non-silicon-containing crosslinking agents that can be used in this embodiment include, but are not limited to: ethylene glycol dimethacrylate (EGDMA), diethylene glycol dimethacrylate (Di(ethylene glycol) dimethacrylate), triethylene glycol dimethacrylate (Triethylene glycol dimethacrylate), tetraethylene glycol dimethacrylate (TEGDMA), ethylene glycol diacrylate (Ethylene glycol diacrylate), diethylene glycol diacrylate (Di(ethylene glycol) diacrylate), triethylene glycol diacrylate, tetraethylene glycol diacrylate (Tetraethylene glycol diacrylate) glycoldiacrylate), N,N'-methylenebisacrylamide (N,N'-Methylenebis(acrylamide)), N,N'-ethylenebisacrylamide (N,N'-Ethylenebis(acrylamide)), dihydroxyethylene (N,N'-(1,2-Dihydroxyethylene)bisacrylamide), trimethylolpropanetrimethacrylate (Trimethylolpropanetrimethacrylate, referred to as TEPTMA), N,N'-hexamethylenebis(methacrylamide) (N,N'-Hexamethylenebis(methacrylamide), Glycerol trimethacrylate, Polyethylene glycol dimethacrylate, Polyethylene glycol diacrylate, (Z)-2-butenedioic acid-2-[(2-methyl-1-oxo-2-propenyl)oxy]ethyl monoester (mono-2-(Methacryloyloxy)ethyl maleate), Diurethanedimethacrylate, 3-Isopropenyl-α,α-dimethylbenzylisocyanate, Diethylene glycol monovinyl ether (DEGVE), Tri(ethylene glycol)divinyl ether (TEGDVE), etc. The above non-silicon-containing crosslinking agents can generally be purchased from suppliers such as Sigma-Aldrich, TCI, Alfa Aesar, etc. ,

[0124] In the present embodiment, the at least one non-silicon-containing crosslinking agent includes, for example, at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and trimethylolpropane trimethacrylate.

[0125] "Silicone crosslinking agent" refers to a crosslinking agent that has at least one silicon-oxygen bonded chemical structure (-Si-O-). Silicone crosslinking agents that can be used in this embodiment include but are not limited to the following examples. For example: methacryloxypropyl terminated polydimethylsiloxane (DMPDMS for short). The CAS No of commonly used methacryloxypropyl terminated polydimethylsiloxane is 58130-03-3. Another example is polyethylene glycol functionalized methacryloxypropyl terminated polydimethylsiloxane, such as the following structure:

[0126]

[0127] Silicon-containing crosslinking agents can be used in combination with other crosslinking agents to form appropriate lens properties. In this embodiment, the silicon-containing crosslinking agent can be purchased from suppliers such as Sigma-Aldrich, Gelest, JNC, Shin-Etsu, Pharnocia, Bimax, etc. Silicon-containing crosslinking agents that can be used in this embodiment are also exemplified by 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, which can be synthesized by referring to the method in U.S. Pat. No. 5,070,215A. The silicon-containing crosslinking agent that can be used in the present embodiment is also, for example, bis-3-Methacryloxy-2-hydroxypropyloxypropylpolydimethylsiloxane, which can be synthesized by referring to the method in U.S. Pat. No. 20030162862A1, and the crosslinking agent can be obtained by replacing mono-(2,3-epoxy)propylether terminatedpolydimethylsiloxane with epoxypropoxypropyl terminated polydimethylsiloxane. The silicon-containing crosslinking agent that can be used in this embodiment is also, for example, a urethane ester of carbinol (hydroxyl) terminated polydimethylsiloxane (DOHPDMS; CAS No: 156327-07-0) and 2-isocyanaoethyl methacrylate (IEM). The synthesis reaction of the urethane ester can use 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) as a catalyst.

[0128] In one embodiment of the present invention, the silicon-containing crosslinking agent comprises, for example, the following structure:

[0129]

[0130] Wherein b is 0-20; R6 is H or CH3 or C2H5, R7 is H or CH3 or OSi(CH3)3, and L3 is the following structure or a combination thereof:

[0131] (CH2) n12 , (C m16 H 2m16 O m17 ) m18 , or (CH2) n13 NHCO(O m22 C m23 H 2m23 ) m24

[0132] Among them, n12 is 1-5, n13 is 1-5, m16 is 1-4, m17 is 0-1, m18 is 1-4, m19 is 0-1, m20 is 1-4, m21 is 1-4, m22 is 0-1, m23 is 1-4, and m24 is 1-4;

[0133] R8 is the following structure or a combination thereof:

[0134]

[0135] Wherein R9 is H or CH3 or C2H5, L4 is the following structure or a combination thereof:

[0136] (CH2) n18 , (C m25 H 2m25 O m26 ) m27 , or (CH2) n19 NHCO(O m31 C m32 H 2m32 ) m33

[0137] Where n18 is 1-5, n19 is 1-5, m25 is 1-4, m26 is 0-1, m27 is 1-4, m28 is 0-1, m29 is 1-4, m30 is 1-4, m31 is 0-1, m32 is 1-4, and m33 is 1-4.

[0138] In one embodiment of the present invention, the silicon-containing crosslinking agent comprises, for example, the following structure:

[0139]

[0140] Where d is 0-20; R 13 is H or CH3 or C2H5, R 14 is H or CH3 or C2H5, L7 is the following structure or a combination thereof: O or NH;

[0141] L8 is the following structure or a combination thereof:

[0142] (CH2) n25 , (C m40 H 2m40 O m41 )m42 or

[0143] Among them, n25 is 1-5, m40 is 1-4, m41 is 0-1, m42 is 1-4, m43 is 0-1, m44 is 1-4, and m45 is 1-4;

[0144] R 15 Is the following structure or a combination of them:

[0145]

[0146] Where R 16 is H or CH3 or C2H5, L9 is the following structure or a combination thereof:

[0147] (CH2) n31 , (C m46 H 2m46 O m47 ) m48 or

[0148] Among them n31 is 1-5, m46 is 1-4, m47 is 0-1, m48 is 1-4, m49 is 0-1, m50 is 1-4, and m51 is 1-4.

[0149] In one embodiment of the present invention, the silicon-containing crosslinking agent includes, for example, at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated urethane polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane modified with polyethylene glycol, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropoxypropyl polydimethylsiloxane.

[0150] In one embodiment of the present invention, it can be observed that the formula composition containing a silicon-containing crosslinking agent, after being treated with a hydrating liquid containing polyacrylic acid and / or sodium polyacrylate, has a lower degree of haze on the lens. This may be due to the fact that in the lens body containing a silicon-containing crosslinking agent, the degree of polymerization between silicon-containing monomers (such as the first silicon-containing monomer and the second silicon-containing monomer) is higher, while the degree of polymerization between silicon-free monomers is lower, and the overall lens structure formed will not allow polyacrylic acid and / or sodium polyacrylate to penetrate too deeply into the inner layer structure of the lens, but will only stay on the surface of the lens, thereby reducing the phenomenon of haze on the lens. Therefore, by combining the molecular weight of polyacrylic acid and / or sodium polyacrylate, the concentration of polyacrylic acid and / or sodium polyacrylate in the hydrating solution, and an appropriate silicon-containing cross-linking agent, and an appropriate molecular weight of the silicon-containing cross-linking agent, it is possible to effectively obtain a contact lens that meets the following conditions: a contact angle (Contact Angle) less than or equal to 60°, and a water breaking time (WBUT) greater than or equal to 20 seconds, and after being worn for about 8 to 10 hours, the tear film breakup time can still be greater than about 15 seconds, and the degree of fogging of the contact lens is acceptable.

[0151] The molecular weight of the silicon-containing crosslinking agent is preferably between 500-5000, more preferably between 700-3000, and even more preferably between 900-2000.

[0152] The content of the silicon-containing crosslinking agent is, for example, 0.1%-6.0% by weight of the contact lens minus the filler, preferably 0.1%-3.0%.

[0153] The role of the initiator is to generate free radicals required for free radical polymerization. Generally, according to the different ways in which free radicals can be generated, they can be divided into thermal initiators and photoinitiators. Initiators that can be thermally activated to generate free radicals are thermal initiators, and initiators that can be photoactivated to generate free radicals are photoinitiators. Photoinitiators that can be used in this embodiment include but are not limited to: 1173 (2-Hydroxy-2-methylpropiophenone), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, referred to as 819), and other embodiments, for example, (2,4,6-trimethylbenzoyl)diphenylphosphine oxide (Diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide) and benzoin dimethyl ether (2,2-Dimethoxy-2-phenylacetophenone) are used.Thermal initiators that can be used in this embodiment include, but are not limited to: azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), 1,1'-azo(cyclohexanecarbonitrile), 2,2'-azobisisobutylamidine dihydrochloride, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane]dihydrochloride, e}dihydrochloride), 2,2'-Azobis(1-imino-1-pyrrolidino-2-ethylpropane) dihydrochloride), 2,2'-Azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}), 2,2'-Azo(2-methyl-N-(2-hydroxyethyl)propionamide), 2,2'-Azobis(4-methoxy-2,4-dimethylvaleronitrile), The initiators mentioned above can generally be purchased from suppliers such as Sigma-Aldrich, TCI, Alfa Aesar, etc.

[0154] "Diluent" refers to an additional ingredient added to the lens formula that does not have a double bond that can accept free radicals to produce free radical polymerization, and therefore cannot be polymerized with monomers or cross-linking agents or initiators to further form a polymer chemical. Some fillers may also have the function of a chain transfer agent and involve a portion of the free radical polymerization process, but their chain transfer effect is generally much lower than that of a true chain transfer agent such as thiol. Therefore, the function of the filler as a chain transfer agent is not considered in this embodiment. Fillers are usually used to help the compatibility of the ingredients in the lens formula, and solvent compounds may be a choice of fillers.The filler that can be used in this embodiment includes, but is not limited to, alcohols such as ethanol, isopropyl alcohol (IPA), n-butanol, n-hexanol, and tert-Amyl alcohol; esters such as ethyl acetate, butyl acetate, and ethyl lacetate; organic acids such as oleic acid; alcohol ethers such as ethyl cellosolve, 2-propoxyethanol, ethylene glycol monobutyl ether, hexyl cellosolve, ethylene glycol monophenyl ether, propylene glycol monomethyl ether, and propylene glycol phenyl ether. The fillers include 2-(2-methoxyethoxy)ethanol, 2-(2-eth ...

[0155] There are several ways to measure the hydrophilicity of the contact lens surface: one is to measure the hydrophilicity of the contact lens surface by contact angle measurement. The contact angle can be measured by the sessile drop method or the captive bubble method. The contact angle in the embodiments listed in the present invention is measured by the sessile drop method.

[0156] Another way to measure the contact lens is to take the contact lens out of water, or an aqueous solution containing buffered salts, or an aqueous solution containing a surfactant (such as Poloxamer 407 or Tween-80), or an aqueous solution containing both buffered salts and surfactants (such as Poloxamer 407 or Tween-80), gently shake off the excess water on the lens surface, and observe and record how long it takes for the water layer on the lens surface to break. The time from the start of the test to the water layer on the lens surface breaking is called the Water Break-up Time (WBUT).

[0157] Another measurement method that is closer to the needs of contact lens users is to give sterilized contact lenses to subjects and have professionally qualified optometrists observe the eyes of subjects wearing contact lenses with a slit lamp to observe how long it takes for the tear layer to break after blinking. The time when the tear layer on the surface of the lens on the eye begins to break after blinking is called the tear break-up time (TBUT). Generally speaking, the lower the contact angle of the contact lens, the longer the water break-up time will correspond to, and the longer the tear film break-up time will correspond to, and the more hydrophilic the surface of the contact lens will be.

[0158] The present invention further provides a method for preparing a contact lens, which includes making a lens body (i.e., a dry lens) and treating the lens body with a hydrating liquid and then washing it with water, or an aqueous solution containing a buffer solution, or an aqueous solution containing a small amount of a surfactant, wherein the hydrating liquid is an organic solution containing polyacrylic acid and / or sodium polyacrylate, so that a contact lens formed by coating the lens body with polyacrylic acid and / or sodium polyacrylate can be obtained. The contact lens can be sterilized by autoclave, and the sterilized contact lens can be worn. The lens body is composed of a silicon-containing unit, a silicon-free unit, a crosslinking agent, and an initiator, and may also contain a filler if necessary. The preparation of the lens body includes providing a composition containing a silicon-containing unit, a silicon-free unit, a crosslinking agent, an initiator, etc., and may also contain a filler if necessary, mixing and stirring them to form a formula, injecting the formula into a mold for controlling the shape and size of the lens to form a formula-mold complex, and then polymerizing the polymerizable units of the formula by light curing or heat curing, crosslinking and curing to form the lens body.

[0159] Figure 2 FIG. 1 is a flow chart of a method for manufacturing a contact lens according to an embodiment of the present invention. Figure 2In one embodiment of the present invention, the manufacturing method of contact lenses includes step S100: providing a lens body; step S200: providing a hydrating liquid, the hydrating liquid is an organic solution including polyacrylic acid and / or sodium polyacrylate, wherein the polyacrylic acid and / or sodium polyacrylate account for 0.01-10wt% of the weight percentage of the hydrating liquid; step S300: soaking the lens body in the hydrating liquid for at least 30 minutes; and step S400: soaking the lens body in water or an aqueous solution for at least 15 minutes, wherein the aqueous solution includes buffer salts and / or a surfactant. It should be noted that the present embodiment does not specifically limit the order of performing step S100 and step S200. In another embodiment, step S100 and step S200 can also be performed simultaneously.

[0160] That is, the manufacturing method of contact lenses includes two parts: the first part uses a hydrating liquid containing polyacrylic acid and / or sodium polyacrylate, an organic solvent and water that have been uniformly mixed, and is used to soak the lens body, namely step S200 and step S300. The soaking temperature can be room temperature, wherein the room temperature is, for example, 20-30°C. Since the embodiment of the present invention can allow polyacrylic acid and / or sodium polyacrylate to have sufficient adsorption force (such as hydrogen bonding and van der Waals force) with the lens of the selected formula, and further select polyacrylic acid and / or sodium polyacrylate with a sufficiently large molecular weight, so that polyacrylic acid and / or sodium polyacrylate can stably form a stable entanglement with the cross-linked polymer structure on the surface of the lens, so that a sufficient and stable amount can be maintained on the surface of the lens, and will not be washed away in the subsequent production process. Therefore, it is not necessary to allow polyacrylic acid and / or sodium polyacrylate to react chemically with the lens body to form a covalent bond, so heating is not necessarily required in step S300. If the temperature needs to be controlled for other production purposes, the temperature of the hydrating liquid can be controlled at 10-80°C. Using an aqueous solution containing polyacrylic acid and / or sodium polyacrylate as a hydrating liquid can effectively reduce the hydrophobicity of the surface of the conventional silicon-containing lens body (reducing the contact angle, increasing the water breaking time (WBUT), and increasing the tear film breakup time when the contact lens is worn on the eye). Further, the hydration of the first part can help improve the lens surface hydrophobicity problem when the lens body changes from dry to wet. The soaking time ranges from, for example, half an hour to 12 hours, and there are corresponding different degrees of improvement in the hydrophobicity of the lens surface, which can significantly optimize the wearing feeling of the lens and solve the hydrophobicity problem of the lens surface.

[0161] The polymer may be selected from: polyacrylic acid (Poly (acrylic acid)) or sodium polyacrylate (Poly (acrylic acid sodium salt)) of different molecular weights, used alone or in combination. Generally speaking, the molecular weight can have better performance within a range, and the preferred molecular weight range is about 100 kDa or more, the more preferred range is about 200 kDa or more, and the more preferred range is about 450 kDa or more. As for the proportion of the polymer in the hydrating liquid, the preferred proportion range is 0.01-10 wt %, the more preferred proportion range is about 0.05-5 wt %, and the more preferred proportion range is about 0.1-1.5 wt %. The proportion of the polymer in the hydrating liquid can be determined based on the lens surface quality requirements (such as contact angle, water break-up time (WBUT), tear film break-up time when the contact lens is worn on the eye), the polymer molecular weight, and the units constituting the lens body.

[0162] In most embodiments of the present invention, whether the contact lenses are before or after sterilization, they are stained with Toluidine Blue O, which proves that the contact lenses and contact lens manufacturing methods of the embodiments of the present invention can retain polymers such as polyacrylic acid and / or sodium polyacrylate on the surface of the contact lenses, thereby improving the hydrophilicity of the lens surface.

[0163] In most embodiments of the present invention, when the molecular weight of polyacrylic acid and / or sodium polyacrylate used in the hydrating liquid is 200 kDa (inclusive) or above, it can be ensured that the TBUT of the subjects at the initial wearing (within 10 minutes after wearing the contact lens) and after wearing for more than 8-10 hours is more than 15 seconds. In some embodiments, when the molecular weight of polyacrylic acid and / or sodium polyacrylate used in the hydrating liquid is 25 kDa (inclusive) or below, even if the contact angle measured by the contact lens is less than 50 degrees, it is found that some subjects have a TBUT of less than 15 seconds at the initial wearing stage. In some embodiments, it is found that when the molecular weight of polyacrylic acid and / or sodium polyacrylate is about 100 kDa, even if the contact angle measured by the contact lens is less than 20-30 degrees, the TBUT of the subjects at the initial wearing can be greater than 15 seconds, but some subjects will have a TBUT of less than 15 seconds after wearing for more than 8-10 hours.

[0164] The organic solvent accounts for 1-90 wt % of the hydration liquid, and preferably, the organic solvent accounts for 20-60 wt % of the hydration liquid. The organic solvents include but are not limited to the following commonly used organic solvents: tripropylene glycol methyl ether, dipropylene glycol methyl ether, ethylene glycol n-butyl ether, ketones (eg, acetone, methylethyl ketone, etc.), diethylene glycol n-butyl ether, diethylene glycol methyl ether, ethylene glycol phenylether, propylene glycol methyl ether, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether, tripropylene glycol n-butylether, propylene glycol n-butyl ether), dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, propylene glycol phenyl ether, dipropylene glycol dimethyl ether, polyethylene glycols, polypropylene glycols, ethyl acetate, butyl acetate, amylacetate, methyl lactate, ethyl lactate, i-propyl lactate,Monohydroxy alcohols (eg, 1-butanol, 2-butanol, 1-propanol, 2-propanol, methanol, ethanol, cyclohexanol, cyclopentanol, (1R, 2R, 4S)-bicyclo[2.2.1]heptan-2-ol, 1-pentanol, 2-pentanol, 3-pentanol, 1-hexanol, 2-hexanol, 3-hexanol, 3-methylbutane-2-ol (3- methyl-2-butanol), 1-heptanol, 2-heptanol, 1-octanol, 2-octanol, 1-nonanol, 2-nonanol, 1-decanol, 2-decanol, 3-octanol, norborneol, tert-butanol, tert-amyl alcohol alcohol), 2-methyl-2-pentanol, 2,3-dimethyl-2-butanol, 3-methyl-3-pentanol, 1-methylcyclohexanol, 2-methyl-2-hexanol, 3,7-dimethyl-3-octanol, 1-chloro-2-methyl-2-propanol 2-propanol), 2-methyl-2-heptanol, 2-methyl-2-octanol, 2-methyl-2-nonanol, 2-methyl-2-decanol, 3-methyl-3-hexanol, 3-methyl-3-heptanol, 4-methyl-4-heptanol,3-methyl-3-octanol, 4-methyl-4-octanol, 3-methyl-3-nonanol, 4-methyl-4-nonanol, 3-methyl-3-octanol, 3-ethyl-3-hexanol 3-hexanol), 3-methyl-3-heptanol, 4-ethyl-4-heptanol, 4-propyl-4-heptanol, 4-isopropyl-4-heptanol, 2,4-dimethyl-2-pentanol, 1-methylcyclopentanol, 1-ethylcyclopentanol, 3-hydroxy-3-methyl-1-butene, 4-hydroxy-4-methyl-1-cyclopentanol, 2-phenyl-2-propanol, 2-methoxy-2-methyl-2-propanol hoxy-2-methyl-2-propanol), 2,3,4-trimethyl-3-pentanol, 3,7-dimethyl-3-octanol, 2-phenyl-2-butanol, 2-methyl-1-phenyl-2-propanol, 3-ethyl-3-pentanol, 1-ethoxy-2-propanol, 1-methyl-2-propanol, t-amyl alcohol, isopropanol), 1-methyl-2-pyrrolidone, N,N-dimethylpropionamide, dimethylformamide formamide), dimethyl acetamide,dimethyl propionamide, N-methylpyrrolidinone, 1,2-propylene glycol, polyethylene glycol having a molecular weight equal to or less than 200 Da, tetrahydrofuran, methylene chloride and mixtures thereof,

[0165] The second part of the contact lens manufacturing method is performed after the first part, that is, step S400: water (RO water or pure water) or an aqueous solution containing buffer salts or an aqueous solution containing a small amount of surfactant (such as Poloxamer 407 or Tween-80) or an aqueous solution containing both buffer salts and a small amount of surfactant is used. That is, after the lens body is immersed in the hydrating liquid for a certain period of time, it is replaced by immersion in water or an aqueous solution to wash away the organic solvent remaining on the surface and inner layer of the contact lens. The time for the lens body to be immersed in the water or aqueous solution is preferably at least 15-30 minutes to ensure the occurrence of cleaning and replacement. The immersion temperature can be constant temperature or can be carried out in a hot and cold alternating manner (or variable temperature). For example, a fixed temperature water or aqueous solution is selected within the temperature range from room temperature to 60°C to immerse the lens, or the lens is alternately immersed in water or aqueous solutions at two temperatures, which are relatively cold and relatively hot, and the temperature range will not have an improper effect on the material of the lens. The thermal expansion and contraction of the lens body caused by the temperature change can promote the washing out of the organic solvent. The choice of temperature and whether to perform the reaction at a constant temperature or at a variable temperature may be determined by the type of organic solvent.

[0166] Preferably, the water or aqueous solution containing buffer salts in the second part (i.e., step S400) may also contain a trace amount of surfactant, wherein the amount of surfactant used is adjusted in proportion to the number of lens bodies to be treated. For example, 5-100 mL of water / each lens, if 100 lens bodies are cleaned at one time, 500 mL to 10 L of water will be used. The more water used, the fewer times of cleaning can be done, and vice versa. During or after step S400, the residual organic solvent in the lens body can be checked by any known method. The soaking in step S400 can be performed multiple times, such as changing the water and then soaking again, and preferably includes at least one change of water and a total of two soakings. The number of soakings can also be adjusted according to the type of organic solvent and the residual organic solvent. For example, the amount of organic solvent measured from the water or aqueous solution after soaking is preferably less than 1 ppm. If it is much more than 1 ppm, the water or aqueous solution can be continued to be soaked.

[0167] The second step of the contact lens manufacturing method of immersing the lens body in water or aqueous solution can further change the expansion rate of the wet lens of the first part, that is, after the second part of the treatment, the diameter of the lens body changes again and reaches the preset diameter of the contact lens. The following further illustrates the conditions and results of the lens body manufacturing method through Examples 1-3. The compounds used in the following examples include

[0168]

[0169]

[0170]

[0171] The compounds used in the examples are described using their commonly used abbreviations.

[0172] Embodiment 1:

[0173] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 819 0.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage. 9.53% of Hexanol and 9.53% of ethyl acetate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0174] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0175] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0176] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0177] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 81.24 in the 5 experimental lenses in the embodiment.

[0178] Embodiment 2:

[0179] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0180] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0181] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0182] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0183] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 83.07 in the 5 experimental lenses in the embodiment.

[0184] Embodiment 3:

[0185] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0186] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0187] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0188] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0189] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 68.91 in the 5 experimental lenses in the embodiment.

[0190] Embodiment 4:

[0191] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0192] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0193] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0194] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0195] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 69.03 in the 5 experimental lenses in the embodiment.

[0196] Embodiment 5:

[0197] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0198] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0199] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank hydrating liquid 1 for 1 hour, and then soaked in the second tank hydrating liquid 1 for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0200] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0201] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 70.14 in the 5 experimental lenses in the embodiment.

[0202] Embodiment 6:

[0203] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0204] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0205] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0206] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0207] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 73.89 in the 5 experimental lenses in the embodiment.

[0208] Embodiment 7:

[0209] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0210] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0211] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0212] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0213] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 79.61 in the 5 experimental lenses in the embodiment.

[0214] Embodiment 8:

[0215] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0216] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0217] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0218] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0219] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 80.72 in the 5 experimental lenses in the embodiment.

[0220] Embodiment 9:

[0221] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0222] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0223] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0224] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0225] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 85.96 in the 5 experimental lenses in the embodiment.

[0226] Embodiment 10:

[0227] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0228] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 2 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0229] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0230] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0231] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 91.86 in the 5 experimental lenses in the embodiment.

[0232] Embodiment 11:

[0233] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0234] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0235] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0236] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0237] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 70.94 in the 5 experimental lenses in the embodiment.

[0238] Embodiment 12:

[0239] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0240] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0241] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0242] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0243] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 68.49 in the 5 experimental lenses in the embodiment.

[0244] Embodiment 13:

[0245] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0246] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0247] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0248] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0249] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 40.12 in the 5 experimental lenses in the embodiment.

[0250] Embodiment 14:

[0251] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0252] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0253] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0254] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0255] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 37.59 in the 5 experimental lenses in the embodiment.

[0256] Embodiment 15:

[0257] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0258] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0259] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0260] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0261] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 66.52 in the 5 experimental lenses in the embodiment.

[0262] Embodiment 16:

[0263] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 819 0.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0264] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0265] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0266] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0267] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 68.07 in the 5 experimental lenses in the embodiment.

[0268] Embodiment 17:

[0269] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0270] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0271] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0272] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0273] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 74.84 in the 5 experimental lenses in the embodiment.

[0274] Embodiment 18:

[0275] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0276] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0277] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0278] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0279] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 84.21 in the 5 experimental lenses in the embodiment.

[0280] Embodiment 19:

[0281] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0282] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0283] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0284] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0285] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 81.98 in the 5 experimental lenses in the embodiment.

[0286] Embodiment 20:

[0287] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0288] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 3-5 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0289] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0290] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0291] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 87.61 in the 5 experimental lenses in the embodiment.

[0292] Embodiment 21:

[0293] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0294] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0295] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0296] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0297] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 65.14 in the 5 experimental lenses in the embodiment.

[0298] Embodiment 22:

[0299] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0300] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0301] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0302] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0303] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 54.09 in the five experimental lenses in the embodiment.

[0304] Embodiment 23:

[0305] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0306] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0307] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0308] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0309] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 50.18 in the five experimental lenses in the embodiment.

[0310] Embodiment 24:

[0311] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0312] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0313] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0314] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0315] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 44.98 in the 5 experimental lenses in the embodiment.

[0316] Embodiment 25:

[0317] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0318] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0319] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0320] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0321] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 40.17 in the 5 experimental lenses in the embodiment.

[0322] Embodiment 26:

[0323] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 8190.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0324] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0325] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0326] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0327] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 46.49 in the 5 experimental lenses in the embodiment.

[0328] Embodiment 27:

[0329] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0330] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0331] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0332] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0333] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 69.66 in the 5 experimental lenses in the embodiment.

[0334] Embodiment 28:

[0335] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0336] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0337] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0338] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0339] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 81.07 in the 5 experimental lenses in the embodiment.

[0340] Embodiment 29:

[0341] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0342] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0343] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0344] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0345] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 80.93 in the 5 experimental lenses in the embodiment.

[0346] Embodiment 30:

[0347] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0348] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 25 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0349] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0350] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0351] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 92.02 in the 5 experimental lenses in the embodiment.

[0352] Embodiment 31:

[0353] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0354] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0355] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0356] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0357] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 50.21 in the five experimental lenses in the embodiment.

[0358] Embodiment 32:

[0359] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0360] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent, for example, accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA%. In this embodiment, a first tank and a second tank of hydration liquid are prepared for use.

[0361] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0362] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0363] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 49.89 in the 5 experimental lenses in the embodiment.

[0364] Embodiment 33:

[0365] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0366] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 0.5 wt% PAA with a molecular weight of 100 KDa and 99.5 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0367] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0368] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0369] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 20.02 in the 5 experimental lenses in the embodiment.

[0370] Embodiment 34:

[0371] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0372] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0373] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0374] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0375] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 18.12 in the 5 experimental lenses in the embodiment.

[0376] Embodiment 35:

[0377] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0378] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0379] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0380] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0381] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 16.89 in the 5 experimental lenses in the embodiment.

[0382] Embodiment 36:

[0383] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 8190.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0384] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0385] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0386] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0387] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 25.37 in the 5 experimental lenses in the embodiment.

[0388] Embodiment 37:

[0389] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0390] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0391] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0392] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0393] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 13.79 in the 5 experimental lenses in the embodiment.

[0394] Embodiment 38:

[0395] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0396] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0397] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0398] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0399] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 38.04 in the 5 experimental lenses in the embodiment.

[0400] Embodiment 39:

[0401] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0402] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0403] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0404] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0405] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 80.47 in the 5 experimental lenses in the embodiment.

[0406] Embodiment 40:

[0407] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0408] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 100 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0409] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0410] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0411] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 32.03 in the 5 experimental lenses in the embodiment.

[0412] Embodiment 41:

[0413] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0414] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0415] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0416] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0417] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 51.47 in the five experimental lenses in the embodiment.

[0418] Embodiment 42:

[0419] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0420] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0421] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0422] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0423] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 46.38 in the 5 experimental lenses in the embodiment.

[0424] Embodiment 43:

[0425] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0426] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0427] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0428] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0429] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 13.98 in the 5 experimental lenses in the embodiment.

[0430] Embodiment 44:

[0431] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0432] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0433] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0434] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0435] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 8.09 in the 5 experimental lenses in the embodiment.

[0436] Embodiment 45:

[0437] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0438] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0439] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0440] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0441] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 7.46 in the 5 experimental lenses in the embodiment.

[0442] Embodiment 46:

[0443] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 8190.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0444] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 1 wt% PAA with a molecular weight of 200 KDa and 99 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0445] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0446] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0447] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 13.55 in the 5 experimental lenses in the embodiment.

[0448] Embodiment 47:

[0449] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0450] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% of PAA with a molecular weight of 200 KDa and 97 wt% of an organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, dipropylene glycol butyl ether. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0451] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0452] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0453] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 16.01 in the 5 experimental lenses in the embodiment.

[0454] Embodiment 48:

[0455] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0456] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0457] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0458] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0459] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 42.96 in the 5 experimental lenses in the embodiment.

[0460] Embodiment 49:

[0461] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0462] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0463] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0464] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0465] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 69.77 in the 5 experimental lenses in the embodiment.

[0466] Embodiment 50:

[0467] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0468] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 200 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0469] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0470] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0471] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 41.48 in the 5 experimental lenses in the embodiment.

[0472] Embodiment 51:

[0473] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0474] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0475] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0476] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0477] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 48.15 in the 5 experimental lenses in the embodiment.

[0478] Embodiment 52:

[0479] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0480] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0481] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0482] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0483] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 47.09 in the 5 experimental lenses in the embodiment.

[0484] Embodiment 53:

[0485] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0486] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0487] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0488] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0489] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 15.72 in the 5 experimental lenses in the embodiment.

[0490] Embodiment 54:

[0491] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0492] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0493] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0494] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0495] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 7.98 in the 5 experimental lenses in the embodiment.

[0496] Embodiment 55:

[0497] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0498] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0499] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0500] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0501] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 6.5 in the 5 experimental lenses in the embodiment.

[0502] Embodiment 56:

[0503] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 8190.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0504] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0505] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0506] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0507] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 8.19 in the 5 experimental lenses in the embodiment.

[0508] Embodiment 57:

[0509] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0510] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0511] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0512] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0513] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 20.14 in the 5 experimental lenses in the embodiment.

[0514] Embodiment 58:

[0515] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0516] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0517] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0518] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0519] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 49.87 in the 5 experimental lenses in the embodiment.

[0520] Embodiment 59:

[0521] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 5.70%, 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 11.11%, MPDMS 12.00%, NVP34.58%, DMA 33.40%, DEGVE 1.38%, TEGDMA 1.15%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Butyl acetate and 11.33% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0522] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0523] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0524] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0525] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 72.06 in the 5 experimental lenses in the embodiment.

[0526] Embodiment 60:

[0527] Step S100: Provide a lens body. The lens body of this embodiment is the tenth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 13.15%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 10.25%, HEMA 10.25%, NVP32.06%, DMA 31.54%, BVE 1.21%, EGDMA 0.80%, TEGDVE 0.10%, 819 0.64%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.44% of Ethyl lactate and 12.44% of Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0528] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 450 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0529] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0530] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0531] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 36.74 in the 5 experimental lenses in the embodiment.

[0532] Example 61:

[0533] Step S100: Provide a lens body. The lens body of this embodiment is the first formula of the ten different formulas of the composition prepared in the embodiment. Different formulas differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 12.70%, MPDMS (molecular weight of about 1000) 15.61%, MMA 1.57%, NVP 65.67%, DMPDMS 1.35%, TEGDMA 1.95%, 8190.58%, HMEPB 0.57%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 9.53% of Hexanol and 9.53% of ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0534] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0535] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0536] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0537] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 50.27 in the five experimental lenses in the embodiment.

[0538] Embodiment 62:

[0539] Step S100: Provide a lens body. The lens body of this embodiment is the second formula of the ten different formulas of the composition preparation in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formula according to the following proportions: TRIS 15.17%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.25%, IBM 3.37%, NVP61.65%, TEGDMA 0.34%, 819 0.61%, HMEPB 0.61%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 10.17% Hexanol and 9.53% ethyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0540] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0541] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0542] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0543] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 52.07 in the five experimental lenses in the embodiment.

[0544] Embodiment 63:

[0545] Step S100: Provide a lens body. The lens body of this embodiment is the third formula among the ten different formulas of the composition prepared in the embodiment. There are differences between different formulas in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formula is prepared according to the following proportions: SIGMA 16.11%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 18.23%, HEMA 2.00%, NVP54.15%, IBM 5.33%, DMPDMS 2.50%, TEGDMA 1.00%, 819 0.68%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formula uses the above total amount as the denominator of the weight percentage, and additionally adds 11.33% of Hexanol and 11.33% of Propyl acetate. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0546] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0547] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0548] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0549] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 18.64 in the 5 experimental lenses in the embodiment.

[0550] Embodiment 64:

[0551] Step S100: Provide a lens body. The lens body of this embodiment is the fourth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: Methacryloxymethylphenethyltris(trimethylsiloxy)silane 24.59%, O-(methacryloxyethyl)-3-[bis(trimethylsiloxy)methylsilyl]propylcarbamate 15.39%, HEMA 4.00%, NVP 53.55%, EGDMA 0.89%, 819 0.60%, HMEPB 0.98%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of ethyl acetate and 10.00% of TPME. Stir the mixed formula for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. Inject the mixed formula into the female mold made by injection molding, and then press the male mold made by injection molding with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is photocured, maintaining the ambient temperature between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0552] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0553] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0554] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in 4 tanks, each tank for 15 minutes, for a total of 60 minutes.

[0555] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 13.28 in the 5 experimental lenses in the embodiment.

[0556] Embodiment 65:

[0557] Step S100: Provide a lens body. The lens body of this embodiment is the fifth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. This embodiment prepares the lens formulation according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 23.25%, (Methacryloxymethyl)bis(trimethylsiloxy)methylsilane 27.15%, HEMA 8.00%, EOEMA 1.00%, NVP 35.98%, polyethylene glycol functionalized methacryloxypropyl terminatedpolydimethylsiloxane 1.5%, PEGDMA 1.50%, 819 0.62%, HMEPB 1.00%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formula uses the aforementioned total amount as the denominator of the weight percentage, and 10.00% of ethyl acetate and 10.00% of ethyl lactate are additionally added. The mixed formula is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formula is completely mixed. The mixed formula is injected into a female mold made by injection molding, and then a male mold made by injection molding is pressed together with the female mold to form a formula-mold complex, and the liquid mixed formula exists in the space between the male mold and the female mold. The formula-mold complex is photocured, and the ambient temperature is maintained between 33°C and 38°C, and the irradiation time is 60 minutes. After the curing process, the formula-mold complex becomes a lens formula complex, and the lenses in the lens formula complex are dry lenses (lenses that have not been hydrated).

[0558] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0559] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0560] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0561] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 10.94 in the 5 experimental lenses in the embodiment.

[0562] Embodiment 66:

[0563] Step S100: Provide a lens body. The lens body of this embodiment is the sixth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: TRIS 14.40%, MPDMS 16.32%, HEMA 12.00%, NVP 54.24%, polyethylene glycol functionalizedmethacryloxypropyl terminated polydimethylsiloxane 0.58%, TEGDMA 1.26%, 8190.60%, HMEPB 0.60%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 10.00% of Hexanol and 10.00% of Propyl acetate. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0564] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0565] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0566] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0567] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 9.06 in the 5 experimental lenses in the embodiment.

[0568] Embodiment 67:

[0569] Step S100: Provide a lens body. The lens body of this embodiment is the seventh formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: 3-[Tris(trimethylsiloxy)silyl]propyl vinyl carbamate 17.26%, MPDMS 16.15%, HEMA16.00%, NVP 49.95%, TEGDMA 0.40%, 819 0.24%, the total amount of the above is 100%, including monomers, initiators, and crosslinking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 12.10% of Hexanol and 12.10% of tAA. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0570] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0571] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0572] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0573] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 22.71 in the 5 experimental lenses in the embodiment.

[0574] Embodiment 68:

[0575] Step S100: Provide a lens body. The lens body of this embodiment is the eighth formulation among the ten different formulations of the composition prepared in the embodiment. Different formulations differ in the content of silicon-containing units, the content of non-silicon-containing units, and the types of silicon-containing units and non-silicon-containing units. In this embodiment, the lens formulation is prepared according to the following proportions: SIGMA 17.25%, Methacryloxymethylphenethyltris(trimethylsiloxy)silane 13.52%, HEMA 20.00%, NVP 47.18%, EGDMA 1.36%, 819 0.69%, the total amount of the above is 100%, including monomers, initiators, and cross-linking agents. The lens formulation uses the above total amount as the denominator of the weight percentage, and additionally adds 11.44% IPA and 11.44% Hexanol. The mixed formulation is stirred for more than 4 hours under nitrogen conditions to ensure that the mixed formulation is completely mixed and uniform. The mixed formula is injected into the female mold made by injection molding, and then the male mold made by injection molding is pressed together with the female mold to form a formula mold complex. The liquid mixed formula exists in the space between the male mold and the female mold. The formula mold complex is light-cured, and the ambient temperature is maintained between 33°C and 38°C for 60 minutes. After the curing process, the formula mold complex becomes a lens formula complex. At this time, the lens in the lens formula complex is a dry lens (a lens that has not been hydrated).

[0576] Step S200: Prepare a hydration liquid. The hydration liquid (hydration liquid 1) of this embodiment is a complete mixture of 3 wt% PAA with a molecular weight of 1250 KDa and 97 wt% organic aqueous solution, and the organic solvent accounts for 30 wt% of the weight percentage of the hydration liquid, wherein the organic solvent is, for example, IPA. In this embodiment, the first tank and the second tank of hydration liquid are prepared for use.

[0577] Step S300: Soak the lens body in the hydrating liquid for at least 30 minutes. In this embodiment, the lens body is left to stand and soak in the first tank of hydrating liquid for 1 hour, and then soaked in the second tank of hydrating liquid for 1 hour, that is, the first part of the treatment is 2 hours in total. The lens body can also be soaked in the same tank for a sufficient time without changing the tank. The soaking temperature is room temperature.

[0578] Step S400: Soak the lens body in water or an aqueous solution for at least 60 minutes to form a contact lens. In this embodiment, four water tanks are prepared, and the lens body is sequentially soaked in the four water tanks for 1 hour, for a total of 4 hours. Stirring can also be used during soaking. This step can also increase or shorten the soaking time, and increase or decrease the number of tank changes, wherein the more tank changes are made, the shorter the total soaking time can be, for example, soaking in five water tanks sequentially for half an hour. The soaking temperature is room temperature. In another embodiment, the lens body is soaked in water or an aqueous solution for at least 60 minutes to form a contact lens, and the lens body can be sequentially soaked in four tanks, each tank for 15 minutes, for a total of 60 minutes.

[0579] Through observation, measurement and calculation, the contact angle of the contact lens prepared in this embodiment has an average value of 30.93 in the 5 experimental lenses in the embodiment.

[0580] Embodiment 69:

[0581] Step S100: Provide a lens body. The lens body of this embodiment is the ninth formulation a...

Claims

1. A contact lens, characterized in that: The contact lens contains at least one silicon-containing monomer, and the surface of the contact lens comprises polyacrylic acid and / or sodium polyacrylate, and the molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 100 kDa.

2. The contact lens according to claim 1, wherein The molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 200 kDa.

3. The contact lens according to claim 1, wherein: The molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 450 kDa.

4. The contact lens according to claim 1, wherein: The at least one silicon-containing monomer includes at least one of methacryloxypropyl tris(trimethylsiloxy)silane, 3-(3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxane)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.

5. The contact lens according to claim 4, wherein: The at least one silicon-containing monomer further comprises at least one of mono-methacryloxypropyl-terminated polydimethylsiloxane, mono-methacryloxypropyl-terminated urethane polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropoxy)propyl-terminated monobutyl-terminated polydimethylsiloxane.

6. The contact lens according to claim 1, wherein: The contact lens includes N-vinylpyrrolidone or N-methyl-N-vinylacetamide.

7. The contact lens according to claim 6, wherein: The contact lens further comprises a filler, and the content of the N-vinylpyrrolidone or the N-methyl-N-vinylacetamide accounts for 30%-65% of the weight percentage of the contact lens after deducting the filler.

8. The contact lens according to claim 6, wherein: The contact lens further comprises a filler, and the content of the N-vinylpyrrolidone or the N-methyl-N-vinylacetamide accounts for 35%-55% of the weight percentage of the contact lens after deducting the filler.

9. The contact lens according to claim 6, wherein: The contact lens comprises hydroxyethyl methacrylate.

10. The contact lens according to claim 5, wherein: The contact lens further includes at least one silicon-containing crosslinking agent.

11. The contact lens according to claim 10, wherein: The at least one silicon-containing crosslinking agent includes at least one of methacrylamide-terminated polydimethylsiloxane, methacrylamide-terminated urethane polydimethylsiloxane, methacrylamide-terminated polydimethylsiloxane modified with polyethylene glycol, 1,3-bis[4-(vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropoxypropyl polydimethylsiloxane.

12. The contact lens according to claim 10, wherein: The molecular weight of the at least one silicon-containing crosslinking agent is between 500-3000.

13. The contact lens according to claim 1, wherein: The contact lens further includes at least one non-silicon-containing crosslinking agent.

14. The contact lens according to claim 13, wherein The at least one non-silicon-containing crosslinking agent includes at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and trimethylolpropane trimethacrylate.

15. The contact lens of claim 1, wherein: The contact lens has a contact angle less than or equal to 60° and a water breaking time (WBUT) greater than or equal to 20 seconds.

16. A silicone hydrogel contact lens, characterized in that: It includes a first silicon-containing monomer, a second silicon-containing monomer, a first hydrophilic monomer, a second hydrophilic monomer, and a silicon-containing crosslinking agent, wherein: The first silicon-containing monomer contains the following structure; Where A is the following structure: or the following structure: ; Wherein R1 is H or CH3 or OSi(CH3)3, R2 is H or CH3 or OSi(CH3)3, and L1 is the following structure or a combination thereof: (CH2) n1 , (C m1 H 2m1 O m2 ) m3 or Among them, n1 is 1-5, m1 is 1-4, m2 is 0-1, m3 is 1-4, m4 is 0-1, m5 is 1-4, and m6 is 1-4; The second silicon-containing monomer contains a first structure or a second structure; The first structure is: Wherein a is 0-20; R3 is H or CH3 or C2H5, R4 is H or CH3 or OSi(CH3)3, R5 is H or CH3 or OSi(CH3)3, and L2 is the following structure or a combination thereof: (CH2) n6 , (C m7 H 2m7 O m8 ) m9 , or (CH2) n7 NHCO(O m13 C m14 H 2m14 ) m15 Among them, n6 is 1-5, n7 is 1-5, m7 is 1-4, m8 is 0-1, m9 is 1-4, m10 is 0-1, m11 is 1-4, m12 is 1-4, m13 is 0-1, m14 is 1-4, and m15 is 1-4; The second structure is: Where c is 0-20; where R 10 is H or CH3 or C2H5, R 11 is H or CH3 or OSi(CH3)3, R 12 is H or CH3 or OSi(CH3)3, L5 is the following structure or a combination thereof: O or NH; L6 is the following structure or a combination thereof: (CH2) n20 , (C m34 H 2m34 O m35 ) m36 or Among them, n20 is 1-5, m34 is 1-4, m35 is 0-1, m36 is 1-4, m37 is 0-1, m38 is 1-4, and m39 is 1-4; The first hydrophilic monomer is a hydrophilic monomer containing an N-vinyl group; The second hydrophilic monomer is different from the first hydrophilic monomer; The surface of the silicone hydrogel contact lens comprises polyacrylic acid and / or sodium polyacrylate, and the molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 100 kDa.

17. The silicone hydrogel contact lens according to claim 16, wherein: The first silicon-containing monomer includes at least one of methacryloxypropyl tris(trimethylsiloxy)silane, 3-(3-methacryloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methylsilane, O-(methacryloxyethyl)-3-[bis(trimethylsiloxane)methylsilyl]propyl carbamate, and 3-[tris(trimethylsiloxy)silyl]propyl vinyl carbamate.

18. The silicone hydrogel contact lens according to claim 16, wherein: The second silicon-containing monomer includes at least one of mono-methacryloxypropyl-terminated polydimethylsiloxane, mono-methacryloxypropyl-terminated urethane polydimethylsiloxane, and mono-(3-methacryloxy-2-hydroxypropoxy)propyl-terminated monobutyl-terminated polydimethylsiloxane.

19. The silicone hydrogel contact lens according to claim 18, wherein: The molecular weight of the second silicon-containing monomer is 350-2500.

20. The silicone hydrogel contact lens according to claim 18, wherein: The molecular weight of the second silicon-containing monomer is 500-1500.

21. The silicone hydrogel contact lens according to claim 16, wherein: The silicone hydrogel contact lens further comprises a filler, and the total content of the first silicon-containing monomer and the second silicon-containing monomer accounts for 15%-60% of the weight of the silicone hydrogel contact lens after deducting the filler.

22. The silicone hydrogel contact lens according to claim 16, wherein: The silicone hydrogel contact lens further comprises a filler, and the total content of the first silicon-containing monomer and the second silicon-containing monomer accounts for 25%-45% of the weight of the silicone hydrogel contact lens after deducting the filler.

23. The silicone hydrogel contact lens according to claim 16, wherein: The first hydrophilic monomer is N-vinylpyrrolidone or N-methyl-N-vinylacetamide.

24. The silicone hydrogel contact lens according to claim 23, wherein: The silicone hydrogel contact lens further comprises a filler, and the content of the first hydrophilic monomer accounts for 30%-65% of the weight percentage of the silicone hydrogel contact lens after deducting the filler.

25. The silicone hydrogel contact lens according to claim 23, wherein: The silicone hydrogel contact lens further comprises a filler, and the content of the first hydrophilic monomer accounts for 35%-55% of the weight percentage of the silicone hydrogel contact lens after deducting the filler.

26. The silicone hydrogel contact lens according to claim 16, wherein: The second hydrophilic monomer includes hydroxyethyl methacrylate.

27. The silicone hydrogel contact lens according to claim 16, wherein: The silicon-containing crosslinking agent comprises the following structure: Wherein b is 0-20; R6 is H or CH3 or C2H5, R7 is H or CH3 or OSi(CH3)3, and L3 is the following structure or a combination thereof: (CH2) n12 , (C m16 H 2m16 O m17 ) m18 , or (CH2)n 13 NHCO(O m22 C m23 H 2m23 ) m24 Among them, n12 is 1-5, n13 is 1-5, m16 is 1-4, m17 is 0-1, m18 is 1-4, m19 is 0-1, m20 is 1-4, m21 is 1-4, m22 is 0-1, m23 is 1-4, and m24 is 1-4; R8 is the following structure or a combination thereof: Wherein R9 is H or CH3 or C2H5, L4 is the following structure or a combination thereof: (CH2) n18 , (C m25 H 2m25 O m26 ) m27 , or (CH2) n19 NHCO(O m31 C m32 H 2m32 ) m33 Where n18 is 1-5, n19 is 1-5, m25 is 1-4, m26 is 0-1, m27 is 1-4, m28 is 0-1, m29 is 1-4, m30 is 1-4, m31 is 0-1, m32 is 1-4, and m33 is 1-4.

28. The silicone hydrogel contact lens according to claim 16, wherein: The silicon-containing crosslinking agent comprises the following structure: Where d is 0-20; R 13 is H or CH3 or C2H5, R 14 is H or CH3 or C2H5, L7 is the following structure or a combination thereof: O or NH; L8 is the following structure or a combination thereof: (CH2) n25 , (C m40 H 2m40 O m41 ) m42 or Among them, n25 is 1-5, m40 is 1-4, m41 is 0-1, m42 is 1-4, m43 is 0-1, m44 is 1-4, and m45 is 1-4; R 15 Is the following structure or a combination of them: Where R 16 is H or CH3 or C2H5, L9 is the following structure or a combination thereof: (CH2) n31 , (C m46 H 2m46 O m47 ) m48 or Among them n31 is 1-5, m46 is 1-4, m47 is 0-1, m48 is 1-4, m49 is 0-1, m50 is 1-4, and m51 is 1-4.

29. The silicone hydrogel contact lens according to claim 16, wherein: The silicon-containing crosslinking agent comprises at least one of methacryloxypropyl-terminated polydimethylsiloxane, methacryloxypropyl-terminated urethane polydimethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane modified with polyethylene glycol, 1,3-bis[4-vinyloxycarbonyloxy)butyl]tetramethyldisiloxane, and bis-3-methacryloxy-2-hydroxypropoxypropyl polydimethylsiloxane.

30. The silicone hydrogel contact lens according to claim 29, wherein: The molecular weight of the silicon-containing crosslinking agent is between 500-3000.

31. The silicone hydrogel contact lens according to claim 16, wherein: The silicone hydrogel contact lens further comprises at least one non-silicon-containing crosslinking agent.

32. The silicone hydrogel contact lens according to claim 31, wherein: The at least one non-silicon-containing crosslinking agent includes at least one of ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, and trimethylolpropane trimethacrylate.

33. The silicone hydrogel contact lens according to claim 16, wherein: The molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 200 kDa.

34. The silicone hydrogel contact lens according to claim 16, wherein: The molecular weight of the polyacrylic acid and / or the sodium polyacrylate is greater than 450 kDa.