Modified polymer, preparation method thereof, gel particles and application

The gel particles are prepared by modifying the modified polymer formed by graphene oxide and alcoholamine compounds, and the problem of insufficient temperature and salt resistance in existing water-regulating agents in high-temperature and high-mineralization reservoirs is solved, and the problem of insufficient temperature and salt resistance in high-temperature and high-mineralization reservoirs is achieved. Efficient deep blockage adjustment and improved oil well recovery rate.

CN118994502AActive Publication Date: 2024-11-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310556843.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

The existing water regulating agents have insufficient temperature and salt resistance in high-temperature and high-mineralization reservoirs, resulting in unsatisfactory deep regulating and blocking effect.

Method used

Using a modified polymer formed by modified graphene oxide and alcohol amine compounds, a coagulant with excellent temperature resistance, salt resistance and expansion properties is prepared by reacting in the presence of initiator, crosslinking agent and water. Glue particles.

Benefits of technology

The gel particles exhibit high expansion ratio and elasticity under high temperature and mineralization environment, which can effectively block large pores and significantly improve the recovery rate of the oil well.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994502A_ABST
    Figure CN118994502A_ABST
Patent Text Reader

Abstract

The invention relates to the field of oilfield chemistry, and discloses a modified polymer, a preparation method thereof, gel particles and application. The modified polymer contains a structural unit A as shown in a formula (I) # imgabs 0 # and a structural unit B as shown in a formula (II) # imgabs 1 #; wherein the weight ratio of the structural unit A to the structural unit B is 1: (0.1-2); wherein R1 and R2 are respectively and independently-H or alkyl of C1-C5; r3 and R4 are respectively and independently-H or alkyl of C1-C3; r5 is an alkylene group having 1 to 15 carbon atoms; z is H, Na or K; q represents graphene oxide partially modified by an alcohol amine compound. The modified polymer has excellent temperature resistance, salt resistance and expansion performance, and has good elasticity and toughness after expansion. The gel particles prepared from the modified polymer are used as a profile control and water plugging agent, are high in temperature resistance and salt tolerance and high in plugging strength for large pore channels, can effectively reduce the permeability of a water phase, and well meet the deep profile control and water plugging effect requirements of high-salinity oil reservoirs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of oil field development and recovery, and in particular to a modified polymer and a preparation method thereof, gel particles and applications. Background Art

[0002] With the continuous development of old oil fields, high-permeability seepage channels have been formed in the reservoirs, resulting in ineffective circulation of injected fluids, which greatly reduces the benefits of oil field development. In order to change the seepage state of formation water, plug the high-permeability water flow channels of oil wells, and increase oil well production, it is necessary to treat oil and water wells with profile control and water plugging agents. For high-temperature and high-mineralization oil reservoirs, taking the Zhongyuan Oilfield as an example, the ground temperature is as high as 90°C and the mineralization is as high as 10×10 4 -30×10 4 mg / L, most conventional plugging agents have poor tolerance to high temperature and high mineralization environment, resulting in unsatisfactory actual plugging effect.

[0003] At present, the profile control and water plugging agents used in the field can be divided into jelly plugging agents, gel plugging agents, granular plugging agents and other plugging agents. Among them, granular plugging agents include inorganic granules (such as clay), ultrafine cement, bulky granules and other plugging agents. In order to achieve the purpose of deep plugging, bulky granular plugging agents have been used more and more in recent years. However, the adaptability of existing bulky granular plugging agents to high temperature and high mineralization still needs to be improved.

[0004] Therefore, improving the temperature resistance and salt resistance of profile control and water plugging agents is of great significance for effectively reducing the seepage capacity of high seepage channels and achieving effective deep plugging and regulation. Summary of the invention

[0005] The purpose of the present invention is to provide a modified polymer and its preparation method, gel particles and application to address the problems that the prior art profile control and water plugging agents have insufficient temperature and salt resistance and low large pore plugging strength, resulting in unsatisfactory deep plugging effect.

[0006] In order to achieve the above object, the first aspect of the present invention provides a modified polymer, wherein the modified polymer comprises a structural unit A represented by formula (I) and a structural unit B represented by formula (II); wherein the weight ratio of the structural unit A to the structural unit B is 1:(0.1-2);

[0007]

[0008] Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; Z is H, Na or K;

[0009] Q represents graphene oxide partially modified by an amine compound.

[0010] The second aspect of the present invention provides a method for preparing a modified polymer, comprising: reacting monomer A', monomer B' and modified graphene in the presence of an initiator, a crosslinking agent and water to obtain a modified polymer;

[0011] Wherein, the weight ratio of the monomer A', the monomer B' and the modified graphene is 100:(1-200):(1-10);

[0012] The modified graphene is graphene oxide partially modified by an alcoholamine compound;

[0013] The monomer A' is a monomer having a structure represented by formula (IV), and the monomer B' is a monomer having a structure represented by formula (V).

[0014]

[0015] Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; and Z is H, Na or K.

[0016] The third aspect of the present invention provides a modified polymer obtained by the method described in the second aspect.

[0017] A fourth aspect of the present invention provides a gel particle, wherein the gel particle is obtained by sequentially granulating, drying, pulverizing and screening a polymer;

[0018] Wherein, the polymer is the modified polymer described in the first aspect or the third aspect.

[0019] The fifth aspect of the present invention provides the use of the gel particles described in the fourth aspect as a profile control and water plugging agent in oil production.

[0020] The present invention adopts specific modified graphene oxide and The structural unit from The structural units together form a modified polymer containing graphene, and the modified polymer has excellent temperature resistance, salt resistance and expansion performance, and has good elasticity and toughness after expansion. The gel particles prepared from the modified polymer have high temperature and high mineralization tolerance. Under the condition of 60-120°C, the expansion multiple in salt water with a mineralization of 30000-300000 mg / L is 10-50, and the elasticity of the particles after expansion is 600-2000Pa. As a profile control and water plugging agent, the gel particles have strong temperature resistance and salt resistance, high plugging strength for large pores, can effectively reduce the permeability of the water phase, and well meet the requirements of deep profile control and water plugging effects in high-mineralization oil reservoirs. The gel particles are used in combination with a polymer solution for oil displacement, which can increase the recovery rate by more than 10% compared with water displacement. DETAILED DESCRIPTION

[0021] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0023] In a first aspect, the present invention provides a modified polymer, wherein the modified polymer comprises a structural unit A represented by formula (I) and a structural unit B represented by formula (II); wherein the weight ratio of the structural unit A to the structural unit B is 1:(0.1-2);

[0024]

[0025] Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; Z is H, Na or K;

[0026] Q represents graphene oxide partially modified by an amine compound.

[0027] According to the present invention, on the basis of satisfying the above structure and composition, preferably, in the modified polymer, the weight ratio of the structural unit A: structural unit B is 1: (0.5-1);

[0028] Preferably, in the structural unit A represented by formula (I) and the structural unit B represented by formula (II), R1 and R2 are each independently -H or a C1-C2 alkyl group; R3 and R4 are each independently -H or a C1-C2 alkyl group; and R5 is a C1-C10 alkylene group.

[0029] According to the present invention, more preferably, in the structural unit A represented by formula (I) and the structural unit B represented by formula (II), R1 and R2 are each independently -H or -CH3; R3 and R4 are each independently -H or -CH3; and R5 is a C1-C6 alkylene group.

[0030] According to the present invention, in the structural unit A shown in formula (I), Q represents graphene oxide partially modified by an olamine compound. By introducing this specific modified graphene into the polymer structure, the temperature resistance, salt resistance and expansion performance of the polymer can be significantly improved, thereby making the polymer more suitable for deep profile control operations in high-mineralization oil reservoirs.

[0031] According to the present invention, the alcoholamine compound has a structure shown in formula (III),

[0032]

[0033] Wherein, R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl.

[0034] Preferably, in formula (III), R6 and R7 are each independently selected from at least one of -H and C1-C3 alkyl.

[0035] More preferably, the alcoholamine compound is at least one selected from 2-hydroxyethylamine, N,N-diethylethanolamine and N,N-di-n-propylethanolamine.

[0036] According to the present invention, the modified graphene represented by Q is prepared by the joint reaction of graphene oxide and the alcoholamine compound shown in the above formula (III). In the present invention, the graphene oxide is a graphene oxide that can be obtained through conventional commercial channels or preparation methods known in the prior art, and has abundant hydroxyl and carboxyl groups distributed on its surface. The hydroxyl groups in the alcoholamine compound shown in the above formula (III) can undergo an esterification reaction with some of the surface carboxyl groups in the graphene oxide to achieve partial modification of the graphene oxide. In addition, the graphene oxide can undergo a dehydration condensation reaction with the amino groups in the amide molecules through the surface hydroxyl groups contained therein to achieve connection with the amide molecules. Specifically, in the structural unit A shown in formula (I), the graphene oxide partially modified by the alcoholamine compound represented by Q has a structure as shown in formula (VI),

[0037]

[0038] in, represents graphene oxide matrix; represents the surface hydroxyl groups of graphene oxide; represents the surface carboxyl group of graphene oxide; * represents the connection position between the graphene oxide partially modified by the alcoholamine compound and N in formula (I); R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl. The surface of the graphene oxide matrix has a plurality of surface hydroxyl groups, surface carboxyl groups and modified groups from alcoholamine compounds.

[0039] In the present invention, the conditions for preparing the modified graphene by reacting the graphene oxide with the alcohol amine compound include: the pH of the reaction system is 1-2, the reaction temperature is 55-65° C., and the reaction time is 1-2 h.

[0040] In the above preparation process, preferably, the weight ratio of the graphene oxide:alcoholamine compound is 1:(0.5-1.5).

[0041] According to the present invention, the modified polymer satisfies the above-mentioned structure and composition, and thus has the characteristics of strong tolerance to high temperature and high mineralization environment. The modified polymer has excellent temperature resistance, salt resistance and expansion performance. Under the condition of 60-120°C, the expansion multiple of the modified polymer in salt water with a mineralization of 30000-300000 mg / L is 10-50, which can well adapt to the performance requirements of deep profile control operations in high-mineralization oil reservoirs for profile control and water plugging materials.

[0042] In the present invention, the mineralization degree can be expressed by the total amount of salt (mg / L) contained in 1L of water. Specifically in oil fields, it can usually be expressed by the total amount of NaCl, CaCl2, and MgCl2 contained in 1L of water.

[0043] According to the present invention, the viscosity average molecular weight of the modified polymer is (1.5-3)×10 7 g / mol.

[0044] According to a preferred embodiment of the present invention, in the structural unit A shown in formula (I), R1 is -H, Q is a modified graphene obtained by the reaction of graphene oxide and N, N-diethylethanolamine (wherein the weight ratio of graphene oxide: N, N-diethylethanolamine is 1:0.8-1.2); in the structural unit B shown in formula (II), R2 is -H, R3 is -CH3, R4 is -CH3, R5 is -CH2-, and Z is H, Na or K; the weight ratio of structural unit A: structural unit B is 1:(0.6-0.8). The modified polymer having this specific structure and composition has better temperature resistance, salt resistance and expansion performance.

[0045] The second aspect of the present invention provides a method for preparing a modified polymer, comprising: reacting monomer A', monomer B' and modified graphene in the presence of an initiator, a crosslinking agent and water to obtain a modified polymer;

[0046] Wherein, the weight ratio of the monomer A', the monomer B' and the modified graphene is 100:(1-200):(1-10);

[0047] The modified graphene is graphene oxide partially modified by an alcoholamine compound;

[0048] The monomer A' is a monomer having a structure represented by formula (IV), and the monomer B' is a monomer having a structure represented by formula (V).

[0049]

[0050] Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; and Z is H, Na or K.

[0051] According to the present invention, in the method for preparing the modified polymer, preferably, the weight ratio of the monomer A', the monomer B' and the modified graphene is 100:(10-100):(1-5).

[0052] According to the present invention, in the preparation method of the modified polymer, preferably, in the monomer A' having a structure represented by formula (IV) and the monomer B' having a structure represented by formula (V), R1 and R2 are each independently -H or a C1-C2 alkyl group; R3 and R4 are each independently -H or a C1-C2 alkyl group; and R5 is a C1-C10 alkylene group.

[0053] According to the present invention, more preferably, in monomer A' having a structure represented by formula (IV) and monomer B' having a structure represented by formula (V), R1 and R2 are each independently -H or -CH3; R3 and R4 are each independently -H or -CH3; and R5 is a C1-C6 alkylene group.

[0054] According to the present invention, in the preparation method of the modified polymer, the modified graphene is graphene oxide partially modified by an alcoholamine compound, which can be prepared by reacting graphene oxide with an alcoholamine compound. By using this specific modified graphene and introducing it into a polymer containing structural units provided by the monomer A' and the monomer B', the temperature resistance, salt resistance and expansion performance of the polymer can be significantly improved, thereby making the polymer more suitable for deep profile control operations in high-mineralization oil reservoirs.

[0055] According to the present invention, in the preparation method of the modified polymer, the definition of the alcoholamine compound is the same as the definition of the alcoholamine compound involved in the first aspect. Specifically, the alcoholamine compound has a structure shown in formula (III),

[0056]

[0057] Wherein, R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl.

[0058] Preferably, in formula (III), R6 and R7 are each independently selected from at least one of -H and C1-C3 alkyl.

[0059] More preferably, the alcoholamine compound is at least one selected from 2-hydroxyethylamine, N,N-diethylethanolamine and N,N-di-n-propylethanolamine.

[0060] According to the present invention, in the preparation method of the modified polymer, the graphene oxide is a graphene oxide that can be obtained through conventional commercial channels or a preparation method known in the prior art, and has abundant hydroxyl and carboxyl groups distributed on its surface. The hydroxyl groups in the alcoholamine compound shown in the above formula (III) can undergo an esterification reaction with some surface carboxyl groups in the graphene oxide (the ester groups generated by the esterification reaction can be determined by infrared spectroscopy testing), thereby achieving partial modification of the graphene oxide. In addition, the graphene oxide can undergo a dehydration condensation reaction with the amino groups in the amide molecules through the surface hydroxyl groups contained therein, thereby achieving connection with the amide molecules.

[0061] According to the present invention, in the preparation method of the modified polymer, the conditions for preparing the modified graphene by reacting the graphene oxide with an alcoholamine compound include: the pH of the reaction system is 1-2, the reaction temperature is 55-65° C., and the reaction time is 1-2h.

[0062] In the above preparation process, preferably, the weight ratio of the graphene oxide:alcoholamine compound is 1:(0.5-1.5).

[0063] According to the present invention, the modified graphene has a structure as shown in formula (VII),

[0064]

[0065] in, represents graphene oxide matrix; represents the surface hydroxyl groups of graphene oxide; represents the surface carboxyl group of graphene oxide; R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl. The surface of the graphene oxide matrix has a plurality of surface hydroxyl groups, surface carboxyl groups and modified groups from alcoholamine compounds.

[0066] According to the present invention, in the preparation method of the modified polymer, based on 100 parts by weight of the monomer A', the initiator is 1-10 parts by weight, the crosslinking agent is 0.2-5 parts by weight, and water is 1500-3000 parts by weight.

[0067] According to the present invention, in the method for preparing the modified polymer, the cross-linking agent is selected from N,N-methylenebisacrylamide and / or aluminum citrate.

[0068] According to the present invention, in the preparation method of the modified polymer, the initiator consists of an oxidant and a reducing agent; wherein the weight ratio of the oxidant:reducing agent is (0.5-1.5):1.

[0069] In the present invention, in the initiator, the oxidant can be selected from at least one of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, sodium hypochlorite, potassium permanganate, potassium perborate and sodium perborate; the reducing agent can be selected from at least one of sodium bisulfite, potassium sulfite, sodium thiosulfate, potassium thiosulfate, sodium sulfide and hydrogen sulfide.

[0070] According to the present invention, in the preparation method of the modified polymer, preferably, the monomer A', the monomer B', the modified graphene and water can be mixed to obtain a mixed solution, a protective gas is introduced to deoxygenate, and then a crosslinking agent and an initiator are added to initiate the reaction, and a polymer colloid is obtained after the reaction is completed, and the modified polymer is obtained by drying. Wherein, the reaction conditions include: a temperature of 45-80°C, preferably 55-65°C; a time of 0.5-5h, preferably 1-2h.

[0071] According to the present invention, in the method for preparing the modified polymer, the protective gas may preferably be nitrogen.

[0072] The third aspect of the present invention provides a modified polymer obtained by the method described in the second aspect.

[0073] According to the present invention, the structure, composition and properties of the modified polymer prepared by the method described in the second aspect are the same as those of the modified polymer described in the first aspect of the present invention, and will not be described in detail herein.

[0074] A fourth aspect of the present invention provides a gel particle, wherein the gel particle is obtained by sequentially granulating, drying, pulverizing and screening a polymer;

[0075] Wherein, the polymer is the modified polymer described in the first aspect or the third aspect.

[0076] According to the present invention, the granulation, drying, crushing and screening can all adopt conventional processes and conditions used in preparing gel particles used as profile control and water plugging agents in the oil field, and the present invention has no particular limitation thereto.

[0077] According to the present invention, the average particle size of the gel particles is 0.05-2 mm.

[0078] According to the present invention, the gel particles have excellent temperature resistance, salt resistance and expansion performance. At 60-120°C, the expansion multiple of the gel particles in salt water with a mineralization of 30,000-300,000 mg / L is 10-50.

[0079] According to the present invention, the gel particles also have good elasticity. At 60-120° C., the elasticity of the gel particles after swelling in saline with a mineralization of 30,000-300,000 mg / L is 600-2000 Pa.

[0080] The gel particles provided by the present invention are used as profile control and water plugging agents for oil fields. They have strong heat and salt resistance, high plugging strength for large pores, and can effectively reduce the permeability of the water phase, thus well meeting the requirements for deep profile control and water plugging effects in high-mineralization oil reservoirs. The gel particles are used in combination with a polymer solution for oil flooding, which can increase the recovery rate by more than 10% compared with water flooding.

[0081] The fifth aspect of the present invention provides the use of the gel particles described in the fourth aspect as a profile control and water plugging agent in oil production.

[0082] The present invention will be described in detail below by way of examples. In the following examples and comparative examples, unless otherwise specified, all are conventional methods; the reagents and materials, unless otherwise specified, can be obtained from commercial sources.

[0083] Graphene oxide: brand INFAN, purchased from Ningbo Fengcheng Nanotechnology Co., Ltd.

[0084] Q1: Modified graphene-I, the preparation process is: graphene oxide and The mixture was mixed in a weight ratio of 1:1 to obtain a mixed system; hydrochloric acid was added to adjust the pH value of the mixed system to 1.5; and then the mixture was reacted at 60° C. for 1.5 hours to obtain modified graphene-I.

[0085] Q2: Modified graphene-II, the preparation process is: graphene oxide and The mixture was mixed at a weight ratio of 1:1.5 to obtain a mixed system; hydrochloric acid was added to adjust the pH value of the mixed system to 1.5; and then the mixture was reacted at 65° C. for 1.5 hours to obtain modified graphene-II.

[0086] Q3: Modified graphene-III, the preparation process is: graphene oxide and The mixture was mixed in a weight ratio of 1:1 to obtain a mixed system; sulfuric acid was added to adjust the pH value of the mixed system to 1.5; and then the mixture was reacted at 65° C. for 2 hours to obtain modified graphene-III.

[0087] In the following examples, the weight ratio of the structural units contained in the prepared polymer is calculated based on the feed amount of the raw materials.

[0088] Example 1

[0089] (1) Monomer A' Monomer B' Modified graphene-I is added into a reaction bottle, and then water is added and mixed thoroughly to obtain a mixed solution;

[0090] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1:1) were added to the above mixed solution to initiate the reaction at a temperature of 60°C for 1.5 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as P1);

[0091] Wherein, the weight ratio of monomer A':monomer B':modified graphene-I:N,N-methylenebisacrylamide:initiator:water is 100:80:2:0.3:2:1800;

[0092] The viscosity average molecular weight of P1 is 2.9×10 7 g / mol; in P1, structural unit A Structural unit B The weight ratio is 1:0.8.

[0093] P1 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S1).

[0094] Example 2

[0095] (1) Monomer A' Monomer B' Modified graphene-I is added into a reaction bottle, and then water is added and mixed thoroughly to obtain a mixed solution;

[0096] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1.2:1) were added to the above mixed solution to initiate the reaction at a temperature of 65°C and a reaction time of 1.5 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as P2);

[0097] Wherein, the weight ratio of monomer A':monomer B':modified graphene-I:N,N-methylenebisacrylamide:initiator:water is 100:51:1.5:0.5:2:1800;

[0098] The viscosity average molecular weight of P2 is 2.7×10 7 g / mol; in P2, structural unit A Structural unit B The weight ratio is 1:0.5.

[0099] P2 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S2).

[0100] Example 3

[0101] (1) Monomer A' Monomer B' Modified graphene-I is added into a reaction bottle, and then water is added and mixed thoroughly to obtain a mixed solution;

[0102] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1.2:1) were added to the above mixed solution to initiate the reaction at a temperature of 55°C for 2 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as P3);

[0103] Wherein, the weight ratio of monomer A':monomer B':modified graphene-I:N,N-methylenebisacrylamide:initiator:water is 100:102:1.5:0.3:2:2000;

[0104] The viscosity average molecular weight of P3 is 2.5×10 7 g / mol; in P3, structural unit A Structural unit B The weight ratio is 1:1.

[0105] P3 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S3).

[0106] Example 4

[0107] (1) Monomer A' Monomer B' Modified graphene-I is added into a reaction bottle, and then water is added and mixed thoroughly to obtain a mixed solution;

[0108] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1.5:1) were added to the above mixed solution to initiate the reaction at a temperature of 70°C for 1 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as P4);

[0109] Wherein, the weight ratio of monomer A':monomer B':modified graphene-I:N,N-methylenebisacrylamide:initiator:water is 100:155:3:0.5:2:2000;

[0110] The viscosity average molecular weight of P4 is 2.3×10 7 g / mol; in P4, structural unit A Structural unit B The weight ratio is 1:1.5.

[0111] P4 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S4).

[0112] Example 5

[0113] (1) Monomer A' Monomer B' Modified graphene-I is added into a reaction bottle, and then water is added and mixed thoroughly to obtain a mixed solution;

[0114] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1.5:1) were added to the above mixed solution to initiate the reaction at a temperature of 70°C for 1 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as P5);

[0115] Wherein, the weight ratio of monomer A':monomer B':modified graphene-I:N,N-methylenebisacrylamide:initiator:water is 100:155:3:0.5:2:2000;

[0116] The viscosity average molecular weight of P5 is 2.2×10 7 g / mol; in P5, structural unit A Structural unit B The weight ratio is 1:1.5.

[0117] P5 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S5).

[0118] Example 6

[0119] The method of Example 5 is followed, except that the modified graphene-I is replaced by an equal weight of modified graphene-II. Other conditions are the same as those of Example 5. A modified polymer (denoted as P6) is obtained;

[0120] The viscosity average molecular weight of P6 is 2.1×10 7 g / mol; in P6, structural unit A Structural unit B The weight ratio is 1:1.5.

[0121] P6 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S6).

[0122] Example 7

[0123] The method of Example 5 is followed, except that the modified graphene-I is replaced by an equal weight of modified graphene-III. Other conditions are the same as those of Example 5. A modified polymer (denoted as P7) is obtained;

[0124] The viscosity average molecular weight of P7 is 1.9×10 7 g / mol; in P7, structural unit A Structural unit B The weight ratio is 1:1.5.

[0125] P7 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as S7).

[0126] Comparative Example 1

[0127] (1) Monomer A' Monomer B' Add to the reaction bottle, then add water, mix thoroughly to obtain a mixed solution;

[0128] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1:1) were added to the above mixed solution to initiate the reaction at a temperature of 60°C for 1.5 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as DP1);

[0129] The weight ratio of monomer A':monomer B':N,N-methylenebisacrylamide:initiator:water is 100:80:0.3:2:1800.

[0130] DP1 was granulated, dried at 105°C to constant weight, crushed, and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as DS1).

[0131] Comparative Example 2

[0132] (1) Monomer A' Monomer B' Graphene oxide (brand INFAN, purchased from Ningbo Fengcheng Nanotechnology Co., Ltd.) was added to the reaction bottle, and then water was added and mixed thoroughly to obtain a mixed solution;

[0133] (2) nitrogen was introduced to deoxygenate for 30 min, and then N,N-methylenebisacrylamide and an initiator (ammonium persulfate: sodium bisulfite weight ratio of 1:1) were added to the above mixed solution to initiate the reaction at a temperature of 60°C for 1.5 h. After the reaction, a polymer colloid was obtained, which was dried to obtain a modified polymer (denoted as DP2);

[0134] Wherein, the weight ratio of monomer A':monomer B':graphene oxide:N,N-methylenebisacrylamide:initiator:water is 100:80:2:0.3:2:1800.

[0135] DP2 was granulated, dried at 105°C to constant weight, crushed and sieved to obtain gel particles with an average particle size of 0.2 mm (denoted as DS2).

[0136] Test Case

[0137] The gel particles S1-S7 and DS1-DS2 prepared in Examples 1-7 and Comparative Examples 1-2 were respectively tested for temperature and salt resistance, large pore plugging strength and enhanced crude oil recovery.

[0138] 1. Temperature and salt resistance test

[0139] 0.2 mm gel particles S1-S7 and DS1-DS2 were added to saline with a mineralization of 30000 mg / L (30000 mg of NaCl was added to 1L of water), and the expansion multiple and elasticity of the gel particles were tested at 60°C and 120°C. The results are shown in Table 1-1.

[0140] 0.2 mm gel particles S1-S7 and DS1-DS2 were added to saline with a mineralization of 300000 mg / L (300000 mg of NaCl was added to 1 L of water), and the expansion multiple and elasticity of the gel particles were tested at 60°C and 120°C. The results are shown in Table 1-2.

[0141] Gel particle expansion multiple test: weigh the gel particle sample (recorded as m); pour the weighed gel particles into the filter bag, seal it and completely place it in the above-mentioned saline solution with the above-mentioned mineralization degree, then place the above-mentioned gel particles and saline solution in a container, seal the container, pressurize it, and place the above-mentioned sealed high-pressure container in an oven at 60°C and 120°C for heating, take out the filter bag after 24 hours and hang it to drip water for 10 minutes, then weigh the whole thing (recorded as m0); at the same time, measure the weight blank value of the unused empty filter bag (recorded as m1). The expansion multiple of the gel particles is calculated by the following formula,

[0142]

[0143] Where c is the expansion multiple of the gel particles.

[0144] Elasticity test of gel particles: The expanded gel particles were made into cylindrical models with a diameter of 5 cm and a height of 2.5 cm. The elastic modulus of the cylindrical models was tested using a universal material testing machine. The elasticity of the gel particles was characterized by the size of the elastic modulus.

[0145] Table 1-1

[0146]

[0147]

[0148] Note: Table 1-1 shows the test data of gel particles in salt water with a mineralization of 30,000 mg / L

[0149] Table 1-2

[0150]

[0151] Note: Table 1-2 shows the test data of gel particles in salt water with a mineralization of 300,000 mg / L

[0152] As can be seen from Table 1-1 and Table 1-2, the gel particles S1-S7 prepared by the modified polymers P1-P7 provided by the present invention have an expansion multiple greater than 19, up to 50, and an elasticity greater than 600Pa, up to 1760Pa, in brine at temperatures of 60°C and 120°C and a salinity of 30000mg / L; in brine at temperatures of 60°C and 120°C and a salinity of 300000mg / L, the expansion multiple is greater than 10, up to 42, and the elasticity greater than 630Pa, up to 2000Pa, and have high expansion multiples and high elasticity in high temperature and high salinity environments, showing excellent temperature and salt resistance. The gel particles DS1-DS2 prepared by the polymers DP1-DP2 provided in Comparative Example 1-2 have significantly worse expansion performance and elasticity than S1-S7 under the same conditions.

[0153] 2. Large channel plugging strength test

[0154] The plugging rate of gel particles S1-S7 and DS1-DS2 was tested according to the method specified in "SY / T 6379-1998 Performance Evaluation Method of Granular Profile Control Agents". The results are shown in Table 2.

[0155] Table 2

[0156] Test subjects Blockage rate (%) S1 98.5 S2 97.8 S3 97.3 S4 97.1 S5 96.8 S6 96.6 S7 96.5 DS1 89.1 DS2 89.0

[0157] As can be seen from Table 2, the gel particles S1-S7 prepared by the modified polymers P1-P7 provided by the present invention exhibit excellent plugging performance. In the above-mentioned plugging test, the plugging rate is greater than 96%, and the plugging strength for large pores is high, thereby being able to effectively reduce the permeability of the water phase, and having significantly better profile control and water plugging effects than DS1-DS2.

[0158] 3. Enhanced oil recovery test

[0159] In a constant temperature box at 80℃, an oil displacement experiment was conducted using interlayer heterogeneous cores. The process is as follows:

[0160] The core was saturated with 100,000 mg / L salt water after vacuuming; the water in the core was displaced by simulated oil until no water flowed out of the outlet, and the oil saturation was calculated; the simulated oil under bound water conditions in the core was displaced by injected salt water at a constant rate until the outlet water content reached 98%, and the water drive recovery was calculated;

[0161] Gel particles S1-S7 and DS1-DS2 were added to 2000 mg / L polyacrylamide aqueous solution (the concentration of gel particles in the polyacrylamide aqueous solution was 1000 mg / L) to obtain a composite flooding system. The composite flooding system of 0.5 PV was injected at the same rate as the above water flooding, and then subsequent water flooding was performed until the outlet water content reached 98%. The percentage increase in the recovery factor of the composite flooding system compared with the water flooding was calculated, and the results are shown in Table 3.

[0162] Table 3

[0163] Test subjects Improved oil recovery (%) S1 13.4 S2 12.9 S3 12.5 S4 12.3 S5 11.5 S6 11.3 S7 10.7 DS1 6.5 DS2 6.3

[0164] As can be seen from Table 3, in the above oil displacement experiment, the composite flooding system consisting of the gel particles S1-S7 prepared by the modified polymers P1-P7 provided by the present invention and the polymer solution showed excellent oil displacement effect, and compared with water flooding, the recovery rate can be increased by more than 10%.

[0165] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A modified polymer, characterized in that The modified polymer contains a structural unit A represented by formula (I) and a structural unit B represented by formula (II); wherein the weight ratio of the structural unit A to the structural unit B is 1:(0.1-2); Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; Z is H, Na or K; Q represents graphene oxide partially modified by an amine compound.

2. The modified polymer according to claim 1, wherein The weight ratio of the structural unit A: structural unit B is 1: (0.5-1); Preferably, R1 and R2 are each independently -H or a C1-C2 alkyl group; R3 and R4 are each independently -H or a C1-C2 alkyl group; and R5 is a C1-C10 alkylene group.

3. The modified polymer according to claim 1 or 2, wherein The alcoholamine compound has a structure shown in formula (III), Wherein, R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl; Preferably, R6 and R7 are each independently selected from at least one of -H and C1-C3 alkyl.

4. The modified polymer according to any one of claims 1 to 3, wherein At 60-120° C., the expansion multiple of the modified polymer in saline water with a salinity of 30,000-300,000 mg / L is 10-50; The viscosity average molecular weight of the modified polymer is (1.5-3)×10 7 g / mol.

5. A method for preparing a modified polymer, comprising: In the presence of an initiator, a cross-linking agent and water, monomer A', monomer B' and modified graphene are reacted to obtain a modified polymer; Wherein, the weight ratio of the monomer A', the monomer B' and the modified graphene is 100:(1-200):(1-10); The modified graphene is graphene oxide partially modified by an alcoholamine compound; The monomer A' is a monomer having a structure represented by formula (IV), and the monomer B' is a monomer having a structure represented by formula (V). Wherein, R1 and R2 are each independently -H or a C1-C5 alkyl group; R3 and R4 are each independently -H or a C1-C3 alkyl group; R5 is a C1-C15 alkylene group; and Z is H, Na or K.

6. The method according to claim 5, wherein: The alcoholamine compound has a structure shown in formula (III), Wherein, R6 and R7 are each independently selected from at least one of -H and C1-C5 alkyl; Preferably, R6 and R7 are each independently selected from at least one of -H and C1-C3 alkyl.

7. The method according to claim 5 or 6, wherein: Based on 100 parts by weight of the monomer A', the initiator is 1-10 parts by weight, the crosslinking agent is 0.2-5 parts by weight, and water is 1500-3000 parts by weight.

8. The method according to any one of claims 5 to 7, wherein: The cross-linking agent is selected from N,N-methylenebisacrylamide and / or aluminum citrate; And / or, the initiator is composed of an oxidant and a reductant; wherein the weight ratio of the oxidant:reductant is (0.5-1.5):

1.

9. The method according to any one of claims 5 to 8, wherein: The reaction conditions include: temperature of 45-80°C, preferably 55-65°C; time of 0.5-5h, preferably 1-2h.

10. A modified polymer obtained by the method according to any one of claims 5 to 9.

11. A gel particle, characterized in that: The gel particles are prepared by sequentially granulating, drying, crushing and screening the polymer; Wherein, the polymer is the modified polymer described in any one of claims 1-4 and 10.

12. The gel particles according to claim 11, wherein The average particle size of the gel particles is 0.05-2 mm.

13. The gel particles according to claim 11 or 12, wherein At 60-120° C., the gel particles expand by a multiple of 10-50 in saline water with a mineralization of 30,000-300,000 mg / L; And / or, at 60-120° C., the elasticity of the gel particles after swelling in saline with a mineralization degree of 30,000-300,000 mg / L is 600-2000 Pa.

14. Use of the gel particles according to any one of claims 11 to 13 as a profile control and water plugging agent in oil production.

Citation Information

Patent Citations

  • Functional magnetic oxidized graphene catalyst material of hydramine-containing compound and its preparation method and application

    CN107252685A

  • Strong-suppression strong-sealing water-based drilling fluid suitable for shale formations, and preparation method thereof

    CN109837072A

  • Polymer and preparation method thereof and oil displacement agent

    CN111548466A

  • Synthesis of graphene oxide nano hydrogel blocking agent and water-based drilling fluid

    CN114605675A

  • Polysulfonic acid silane composite graphene oxide plugging agent and oil-based drilling fluid

    CN114605976A