Conjugated microporous polymer taking quinoxaline diol as recognition group as well as preparation method and application of conjugated microporous polymer

By using quinoxaline diol as the recognition group, the complex problem of silver ion and permanganate detection in the prior art is solved, and high selectivity and high sensitivity fluorescence sensing detection is achieved. A simple and low-cost on-site inspection method is used.

CN118994540AActive Publication Date: 2024-11-22GUANGXI NORMAL UNIV FOR NATITIES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411091767.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

The prior art is difficult to detect silver ions and permanganate quickly, efficiently and easily, and the detection method is complex and cannot be carried out on-site detection.

Method used

A conjugated microporous polymer with quinoxaline glycol as the recognition group was prepared by coupling reaction polymerization, and its high selectivity and sensitivity were used to detect silver ions and permanganate.

Benefits of technology

High selectivity and high sensitivity detection of silver ions and permanganate are achieved, and a simple and low-cost field detection method is provided, with a detection limit of 2.5×10-6 mol·L-1 and 7.4×10- 6 mol·L-1, suitable for detection in solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994540A_ABST
    Figure CN118994540A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of fluorescence sensors, and provides a conjugated microporous polymer taking quinoxaline diol as a recognition group, and a preparation method and application thereof. The preparation method comprises the following steps: reacting C6H6Br2N2S with sodium borohydride to obtain an intermediate compound 1, reacting the intermediate compound 1 with oxalic acid to obtain an intermediate compound 2, and carrying out coupling reaction on the intermediate compound 2 and 2, 4, 6-tri (4-ethynylphenyl)-1, 3, 5-triazine under the action of a catalyst to obtain the conjugated microporous polymer CMP. The prepared conjugated microporous polymer has high selectivity and high sensitivity to Ag < + > and MnO4 <->, the fluorescence intensity of a CMP solution at 450 nm is in linear relation with the concentration of Ag < + > / MnO4 <->, and the detection limits are 2.5 * 10 <-6 > mol.L <-1 > and 7.4 * 10 <-6 > mol.L <-1 > respectively. The prepared CMP is suitable for detecting Ag < + > or MnO4 <->.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorescent sensors, and in particular to a conjugated microporous polymer using quinoxaline diol as a recognition group, and a preparation method and application thereof. Background Art

[0002] Silver ion is a common cation that is widely used in catalysis, production of coins, batteries, photoelectric tubes, bearing parts, gels, professional bandages, implantable prostheses, ureters, and drinking water disinfection. About 2,500 tons of silver are discharged into the environment from industry each year, of which 150 tons are precipitates from wastewater. The negative impact of silver ions on the environment, especially organisms, has also attracted great attention. It is reported that silver ions can bind to amines, imidazoles, and adenylate groups of various metabolites, thereby inactivating them. Silver ions can replace Ca in hydroxyapatite in bones. 2+ and Zn 2+ Excessive exposure to silver in the human body may lead to blood silver (argyria) and urine silver excretion, heart dilatation, growth retardation and liver degenerative changes.

[0003] Due to its strong oxidizing property, permanganate also has a wide range of uses, for example: in the production of chemicals, it is used as an oxidant for making saccharin, vitamin C, isoniazid and benzoic acid; in medicine, it is used for cleaning, disinfection and fungal eradication; in water purification and wastewater treatment, it is used as a water treatment agent to oxidize hydrogen sulfide, phenol, iron, manganese and organic, inorganic and other pollutants, control odor and decolorize; in laboratories, it is often used as a color developer for the color development of thin layer chromatography strips. Permanganate is used in large quantities in these fields. After being discharged into the environment, it will quickly enter the biosphere and hydrosphere, posing a serious threat to organisms, ecosystems and human health and safety.

[0004] At present, the methods used to detect silver ions and permanganate mostly require expensive instruments and professional operators, and the operation steps are complicated and cannot be tested on site. Therefore, it is necessary to develop a fast, efficient, simple and on-site means to detect silver ions and permanganate.

[0005] Conjugated microporous polymers, also known as Conjugated Microporous Polymers (CMPs), are a new type of porous microporous material with a stable π-π conjugated nano-skeleton spatial network structure. Since its discovery in 2007, it has broad application prospects in catalysis, energy storage, fluorescence sensing, separation, etc. due to its flexible and designable structure, adjustable pore size properties, and adjustable optical properties. Some CMPs have fluorescent properties themselves, but they can be quenched under the action of ions to identify specific ions. This is also a method for detecting some elements. The document "Synthesis of Novel Porous Organic Polymers and Research on Their Fluorescence Sensing Properties" (Zhang Chao, Jilin University, 2024) discloses a new type of conjugated microporous organic polymer (TPA-Bp). Experiments have found that Fe 3+ and Fe 2+ will quench the fluorescence of TPA-Bp. 3+ The detection limit was 1.02×10 - 5 mol·L -1 , Fe 2+ The detection limit was 5.37×10 -6 mol·L -1 TPA-Bp is expected to be used as Fe 3+ and Fe 2+ Detection of fluorescence sensors.

[0006] At present, there is no report on the use of conjugated microporous polymers with quinoxaline diol as the recognition group for the detection of silver ions and permanganate. Summary of the invention

[0007] The purpose of the present invention is to provide a conjugated microporous polymer with quinoxaline diol as a recognition group, a preparation method and application thereof, and the polymer prepared by the present invention has good affinity for Ag. + and MnO4 - It has high selectivity and high sensitivity and can be used to detect silver ions or permanganate in solution.

[0008] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A conjugated microporous polymer with quinoxaline diol as a recognition group, the conjugated microporous polymer is denoted as CMP, and its structure is shown in formula (I):

[0010]

[0011] The present invention also provides a method for preparing a conjugated microporous polymer using quinoxaline diol as a recognition group, wherein 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine and 2,3-dihydroxy-5,8-dibromo-quinoxaline are used as monomers and polymerized through a coupling reaction to obtain a conjugated microporous polymer shown in formula (I).

[0012] In the present invention, preferably, the specific steps of the coupling reaction are as follows:

[0013] 2,3-dihydroxy-5,8-dibromo-quinoxaline and 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine are weighed in a molar ratio of 1 to 1.5:1 and placed in a reaction container, catalysts tetrakis(triphenylphosphine)palladium and cuprous iodide are added to the reaction container, and the reaction container is degassed with nitrogen; toluene is injected into the reaction container, and at the same time, the instrument is turned on for stirring to degas with nitrogen; triethylamine is then injected into the reaction container to degas with nitrogen; after the nitrogen degassing is completed, the reaction temperature is raised to 78 to 82°C, and a cover is used to avoid light while maintaining nitrogen protection, and the reaction is continued for 40 to 55 hours; after the reaction is completed, the reaction container is cooled to room temperature, washed, and then Soxhlet extraction is performed with methanol, and the product is dried to obtain the conjugated microporous polymer.

[0014] In the present invention, preferably, the 2,3-dihydroxy-5,8-dibromo-quinoxaline is prepared by the following method: oxalic acid and 1,4-dibromo-2,3-diaminobenzene are weighed in a molar ratio of 1:1 to 1.3, and are respectively dissolved with hydrochloric acid; the two solutions are mixed in a reaction container, heated under reflux for a period of time; after cooling to room temperature, the obtained precipitate is separated by filtration, washed with water and dried to obtain the final product 2,3-dihydroxy-5,8-dibromo-quinoxaline.

[0015] In the present invention, preferably, the 1,4-dibromo-2,3-diaminobenzene is prepared by the following method: 4,7-dibromobenzo[c]-1.2.5-thiadiazole and sodium borohydride are weighed in a molar ratio of 1:10-15, dissolved in anhydrous ethanol, and added to a reaction container of a reflux reaction device; then a small amount of cobalt chloride hexahydrate is added to perform a reflux reaction; after the reflux is completed, the reaction container is cooled to room temperature; after the solution is filtered and separated, the filtrate is spin-dried and water is added, and then dichloromethane is added for extraction, and the extract is collected in a conical flask; finally, anhydrous sodium carbonate is added, the upper opening is wrapped with a paper towel, and it is left for about 1 hour. After the solvent is evaporated, 1,4-dibromo-2,3-diaminobenzene is obtained.

[0016] In the present invention, preferably, the amounts of tetrakis(triphenylphosphine)palladium and cuprous iodide used are 1% and 0.4% of the mass of 2,3-dihydroxy-5,8-dibromo-quinoxaline, respectively.

[0017] In the present invention, preferably, the reflux reaction time is 2 to 3 hours.

[0018] The present invention also provides an application of the conjugated microporous polymer, specifically, using the conjugated microporous polymer as a fluorescent sensor for Ag in a solution. + or MnO4 - Detection.

[0019] In the present invention, preferably, the Ag + or MnO4 - The detection method used is:

[0020] (1) Prepare a CMP mother solution of a certain concentration using DMF as solvent and test its fluorescence intensity I0. + or MnO4 - The solution was added to the conjugated microporous polymer mother solution and mixed, the fluorescence intensity I was tested, and (I0-I) / I0 was calculated; Ag was continued to be added dropwise. + or MnO4 - Solution, test the fluorescence intensity I of the mixed solution, repeat several times, establish (I0-I) / I0 and Ag in the test solution + or MnO4 - The linear relationship between the concentration of

[0021] (2) Under the same conditions as step (1), add the sample solution to be tested to the CMP mother solution, detect the fluorescence intensity I of the mixed solution, and use the linear relationship obtained in step (1) to calculate the Ag content in the sample solution to be tested. + or MnO4 - concentration.

[0022] In the present invention, preferably, the fluorescence intensity is tested at 450 nm.

[0023] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0024] 1. The present invention adopts 4,7-dibromobenzo[c]-1.2.5-thiadiazole (C6H6Br2N2S) and sodium borohydride to react to obtain intermediate compound 1, and then the intermediate compound 1 reacts with oxalic acid to obtain intermediate compound 2, and the intermediate compound 2 is then coupled with 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine under the action of a palladium catalyst to obtain a conjugated microporous polymer CMP. The preparation method of the present invention has the advantages of simple operation, low cost, good synthesis effect and high yield.

[0025] 2. The conjugated microporous polymer CMP product prepared by the present invention is fluffy and is a special amorphous material. + and MnO4 -It has high selectivity and high sensitivity. The fluorescence intensity of CMP at 450nm is similar to that of Ag. + / MnO4 - The concentration is linearly related, y (Ag+) =0.00576x-0.00143, R 2 =0.994;y (MnO4 - )=0.037x-1.65,R 2 =0.996; Ag + The quenching constant K SV =1.5×10 4 , limit of detection (LOD) = 2.5 × 10 -6 mol·L -1 ; MnO4 - Ion quenching constant K SV =5.1×10 3 , limit of detection (LOD) = 7.4 × 10 -6 mol·L -1 The CMP prepared by the present invention is suitable for Ag + or MnO4 - Perform specific testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 FT-IR spectrum of the conjugated microporous polymer CMP synthesized in Example 1;

[0027] Figure 2 This is a physical shape diagram of the conjugated microporous polymer CMP synthesized in Example 1;

[0028] Figure 3 This is a scanning electron microscope image of the conjugated microporous polymer CMP synthesized in Example 1;

[0029] Figure 4 is the X-ray diffraction pattern of the conjugated microporous polymer CMP synthesized in Example 1;

[0030] Figure 5 This is the nuclear magnetic resonance spectrum of the intermediate compound 2 synthesized in Example 1;

[0031] Figure 6 is the nuclear magnetic resonance spectrum of the synthesized conjugated microporous polymer CMP;

[0032] Figure 7 This is a comparison of the fluorescence intensity after adding different metal cations to CMP;

[0033] Figure 8 This is a graph showing the change in fluorescence intensity after adding different concentrations of cations to CMP;

[0034] Fig. 9 is a bar graph showing the fluorescence quenching percentage of CMP after adding metal cations;

[0035] Fig.10 This is the result of the anti-interference experiment of Ag+;

[0036] Fig.11 Adding low concentration of Ag to CMP + The fluorescence change graph after that;

[0037] Fig.12 This is the fluorescence intensity change diagram of CMP at different pH;

[0038] Fig.13 This is a fluorescent photo of CMP after adding anions;

[0039] Fig.14 Changes in fluorescence intensity when different anions are added to CMP;

[0040] Fig.15 Adding MnO4 to CMP - The change diagram; where a is the actual change diagram, and b is the ultraviolet spectrum diagram.

[0041] Fig.16 is the fluorescence quenching percentage of CMP after adding anions;

[0042] Fig.17 This is the result of the CMP anti-interference experiment for different anions;

[0043] Fig.18 Adding low concentration MnO4 to CMP - The fluorescence change graph after that;

[0044] Fig.19 Ag + Results of anti-interference experiment (for anions);

[0045] Fig. 20 Several typical ions and Ag in CMP + / MnO4 - The relative intensity diagram of fluorescence quenching. DETAILED DESCRIPTION

[0046] The technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without paying creative labor are within the scope of protection of the present invention. In the present invention, unless otherwise specified, all raw material components are commercially available commodities well known to those skilled in the art.

[0047] The conjugated microporous polymer with quinoxaline diol as the recognition group is denoted as CMP, and its structure is shown in formula (I):

[0048]

[0049] In an embodiment of the present invention, the preparation method of CMP is: 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine and 2,3-dihydroxy-5,8-dibromo-quinoxaline are used as monomers and polymerized by coupling reaction to obtain a conjugated microporous polymer represented by formula (I). The preparation route is as follows:

[0050]

[0051] Among them, the synthesis route of intermediate compound 2 (2,3-dihydroxy-5,8-dibromo-quinoxaline) is as follows:

[0052]

[0053] First, 4,7-dibromobenzo[c]-1.2.5-thiadiazole and sodium borohydride are weighed in a molar ratio of 1:10-15, dissolved in anhydrous ethanol, and added to a reaction vessel of a reflux reaction device; then a small amount of cobalt chloride hexahydrate is added to perform a reflux reaction; after the reflux is completed, the reaction vessel is cooled to room temperature; after the solution is filtered and separated, the filtrate is dried and water is added, and then dichloromethane is added for extraction, and the extract is collected in a conical flask; finally, anhydrous sodium carbonate is added, the upper opening is wrapped with a paper towel, and it is left for about 1 hour. After the solvent is evaporated, an intermediate compound 1 (1,4-dibromo-2,3-diaminobenzene) is obtained.

[0054] Oxalic acid and 1,4-dibromo-2,3-diaminobenzene were weighed in a molar ratio of 1:1 to 1.3 and dissolved respectively with hydrochloric acid; the two solutions were mixed in a reaction container, heated under reflux for a period of time; after cooling to room temperature, the obtained precipitate was separated by filtration, washed with water and dried to obtain intermediate compound 2 (2,3-dihydroxy-5,8-dibromo-quinoxaline).

[0055] 1. Preparation Example

[0056] Example 1

[0057] The conjugated microporous polymer using quinoxaline diol as a recognition group comprises the following steps:

[0058] (1) Preparation of intermediate compound 1: 1.0385 g of 4,7-dibromobenzo[c]-1.2.5-thiadiazole and 1.3224 g of sodium borohydride were weighed in a molar ratio of 1:10, dissolved in 60 ml of anhydrous ethanol, and added to the flask of a reflux reaction device; then 0.008 g of cobalt chloride hexahydrate was added, and the mixture was placed in a reflux device for reflux reaction for 3 h; after the reflux was completed, the flask was cooled to room temperature; after the solution was filtered and separated, the filtrate was spin-dried and 100 ml of water was added, and dichloromethane was added in small amounts several times, and the mixture was extracted and collected in a conical flask; finally, anhydrous sodium carbonate was added, the upper opening was wrapped with a paper towel, and the mixture was left for 1 hour. After the solvent was evaporated, intermediate compound 1, i.e., 1,4-dibromo-2,3-diaminobenzene, was obtained with a yield of 3.6811 g and a yield of 81.4%;

[0059] (2) Preparation of intermediate compound 2 (2,3-dihydroxy-5,8-dibromo-quinoxaline): 0.3784 g of oxalic acid and 1.1443 g of intermediate compound 1 were weighed at a molar ratio of 1:1, and each was dissolved in 10 ml of hydrochloric acid; the two solutions were mixed in a flask, heated under reflux for 2 h; after cooling to room temperature, the resulting precipitate was separated by filtration, washed with water and dried to obtain intermediate compound 2, i.e., 2,3-dihydroxy-5,8-dibromo-quinoxaline, with a yield of 0.7884 and a yield of 61.8%;

[0060] (3) Preparation of CMP: 0.5 g of 2,3-dihydroxy-5,8-dibromo-quinoxaline and 0.396 g of raw material M [2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine] were weighed in a three-necked flask at a molar ratio of 1.5:1, and 0.0052 g of tetrakis(triphenylphosphine)palladium and 0.0020 g of cuprous iodide were added to the three-necked flask, and nitrogen degassing was performed for 20 min; 6 mL of toluene was injected into the three-necked flask, and at the same time, the instrument was started for stirring and nitrogen degassing was performed for 10 min; 6 mL of triethylamine was injected into the three-necked flask and stirred for 10 min. n Nitrogen degassing; after nitrogen degassing, the reaction temperature was raised to 80°C, and the reaction was continued for 48 hours under the condition of nitrogen protection and light protection with a cover; after the reaction, the three-necked flask was cooled to room temperature, washed with dichloromethane, acetone, distilled water, and methanol in turn, and subjected to Soxhlet extraction with methanol for 72 hours. The product was placed in a vacuum drying oven, the temperature was adjusted to 50°C, and the product CMP was dried for 24 hours, with a yield of 0.6598 g and a yield of 73.3%.

[0061] Example 2

[0062] The conjugated microporous polymer using quinoxaline diol as a recognition group comprises the following steps:

[0063] (1) Preparation of intermediate compound 1: 1.0385 g of 4,7-dibromobenzo[c]-1.2.5-thiadiazole and 1.5868 g of sodium borohydride were weighed in a molar ratio of 1:12, dissolved in 60 ml of anhydrous ethanol, and added to the flask of a reflux reaction device; then 0.008 g of cobalt chloride hexahydrate was added, and the mixture was placed in a reflux device for reflux reaction for 3 h; after the reflux was completed, the flask was cooled to room temperature; after the solution was filtered and separated, the filtrate was spin-dried and 100 ml of water was added, and dichloromethane was added in small amounts several times, and the mixture was extracted and collected in a conical flask; finally, anhydrous sodium carbonate was added, the upper opening was wrapped with a paper towel, and the mixture was left for 1 hour. After the solvent was evaporated, intermediate compound 1, i.e., 1,4-dibromo-2,3-diaminobenzene, was obtained with a yield of 3.6811 g and a yield of 81.4%;

[0064] (2) Preparation of intermediate compound 2 (2,3-dihydroxy-5,8-dibromo-quinoxaline): 0.3784 g of oxalic acid and 1.3732 g of intermediate compound 1 were weighed at a molar ratio of 1:1.2, and each was dissolved in 10 ml of hydrochloric acid; the two solutions were mixed in a flask, heated under reflux for 2 h; after cooling to room temperature, the resulting precipitate was separated by filtration, washed with water and dried to obtain intermediate compound 2, i.e., 2,3-dihydroxy-5,8-dibromo-quinoxaline;

[0065] (3) Preparation of CMP: 0.4 g of 2,3-dihydroxy-5,8-dibromo-quinoxaline and 0.396 g of raw material M [2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine] were weighed in a three-necked flask at a molar ratio of 1.2:1, and 0.0041 g of tetrakis(triphenylphosphine)palladium and 0.0016 g of cuprous iodide were added to the three-necked flask, and nitrogen degassing was performed for 20 min; 6 mL of toluene was injected into the three-necked flask, and at the same time, the instrument was stirred and nitrogen degassing was performed for 10 min; 6 mL of triethylamine was injected into the three-necked flask and stirred for 10 min. n Nitrogen degassing; after nitrogen degassing, the reaction temperature was raised to 78°C, and the reaction was continued for 55 hours under the condition of nitrogen protection and light protection with a cover; after the reaction, the three-necked flask was cooled to room temperature, washed with dichloromethane, acetone, distilled water, and methanol in turn, and subjected to Soxhlet extraction with methanol for 72 hours. The product was placed in a vacuum drying oven, the temperature was adjusted to 50°C, and the product CMP was dried for 24 hours.

[0066] Example 3

[0067] The conjugated microporous polymer using quinoxaline diol as a recognition group comprises the following steps:

[0068] (1) Preparation of intermediate compound 1: 1.0385 g of 4,7-dibromobenzo[c]-1.2.5-thiadiazole and 1.9836 g of sodium borohydride were weighed in a molar ratio of 1:15, dissolved in 60 ml of anhydrous ethanol, and added to the flask of a reflux reaction device; then 0.008 g of cobalt chloride hexahydrate was added, and the mixture was placed in a reflux device for reflux reaction for 3 h; after the reflux was completed, the flask was cooled to room temperature; after the solution was filtered and separated, the filtrate was spin-dried and 100 ml of water was added, and dichloromethane was added in small amounts several times, and the mixture was extracted and collected in a conical flask; finally, anhydrous sodium carbonate was added, the upper opening was wrapped with a paper towel, and the mixture was left for 1 hour. After the solvent was evaporated, intermediate compound 1, i.e., 1,4-dibromo-2,3-diaminobenzene, was obtained with a yield of 3.6811 g and a yield of 81.4%;

[0069] (2) Preparation of intermediate compound 2 (2,3-dihydroxy-5,8-dibromo-quinoxaline): 0.3784 g of oxalic acid and 1.1443 g of intermediate compound 1 were weighed at a molar ratio of 1:1.3, and each was dissolved in 10 ml of hydrochloric acid; the two solutions were mixed in a flask, heated under reflux for 2 h; after cooling to room temperature, the resulting precipitate was separated by filtration, washed with water and dried to obtain intermediate compound 2, i.e., 2,3-dihydroxy-5,8-dibromo-quinoxaline, with a yield of 0.7884 and a yield of 61.8%;

[0070] (3) Preparation of CMP: 0.32 g of 2,3-dihydroxy-5,8-dibromo-quinoxaline and 0.396 g of raw material M [2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine] were weighed in a molar ratio of 1:1 and placed in a three-necked flask. 0.0032 g of tetrakis(triphenylphosphine)palladium and 0.0013 g of cuprous iodide were added to the three-necked flask and degassed with nitrogen for 20 min. 6 mL of toluene was injected into the three-necked flask and the stirring of the instrument was started. The nitrogen degassed was carried out for 10 min. 6 mL of triethylamine was injected into the three-necked flask and the stirring was carried out for 10 min. n Nitrogen degassing; after nitrogen degassing, the reaction temperature was raised to 82°C, and the reaction was continued for 40 hours under the condition of nitrogen protection and light protection with a cover; after the reaction, the three-necked flask was cooled to room temperature, washed with dichloromethane, acetone, distilled water, and methanol in turn, and subjected to Soxhlet extraction with methanol for 72 hours. The product was placed in a vacuum drying oven, the temperature was adjusted to 50°C, and the product CMP was dried continuously for 24 hours.

[0071] Example 4

[0072] The conjugated microporous polymer is used as a fluorescent sensor for Ag in solution + The detection method used is:

[0073] (1) Use DMF as solvent to prepare 0.01 mg mL -1The fluorescence intensity I0 of CMP mother solution was tested at 450nm. + The solution was added to the conjugated microporous polymer mother solution and mixed. The fluorescence intensity I was tested at 450nm and (I0-I) / I0 was calculated. Ag was added dropwise. + Solution, test the fluorescence intensity I of the mixed solution, repeat several times, establish (I0-I) / I0 and Ag in the test solution + or MnO4 - The linear relationship between the concentration of

[0074] (2) Under the same conditions as step (1), add the sample solution to be tested to the CMP mother solution, detect the fluorescence intensity I of the mixed solution, and use the linear relationship obtained in step (1) to calculate the Ag content in the sample solution to be tested. + concentration.

[0075] Example 5

[0076] The conjugated microporous polymer was used as a fluorescent sensor for MnO4 in solution. - The detection method used is:

[0077] (1) Take a certain concentration of conjugated microporous polymer mother solution and test its fluorescence intensity I0 at 450nm. - The solution was added to the conjugated microporous polymer mother solution and mixed. The fluorescence intensity I was tested at 450nm and (I0-I) / I0 was calculated. MnO4 was added dropwise. - The fluorescence intensity I of the mixed solution was tested at 450 nm, and the relationship between (I0-I) / I0 and the MnO4 - The linear relationship between the concentration of

[0078] (2) Under the same conditions as step (1), add the sample solution to be tested to the CMP mother solution, detect the fluorescence intensity I of the mixed solution, and use the linear relationship obtained in step (1) to calculate the MnO4 content of the sample solution to be tested. - concentration.

[0079] 2. Characterization of Materials

[0080] 1. Fourier transform infrared spectroscopy (FTIR) analysis

[0081] Figure 1 The FTIR image of the prepared conjugated microporous polymer CMP shows that CMP has a wavelength of 1555 cm -1The characteristic absorption peak at 1352cm belongs to the vibration absorption peak of the benzene ring skeleton in the intermediate compound 2. The characteristic absorption peak in the structure of raw material M is not obvious. It may be due to the influence of noise signals in the environment, which leads to the fact that this group of characteristic peaks at 1352cm are not obvious in the CMP structure. -1 The characteristic absorption peak of disappeared, proving that -C-Br- in intermediate compound 2 disappeared. Intermediate compound 2 was combined with raw material M to successfully prepare conjugated microporous polymer CMP.

[0082] 2. Physical shape and scanning electron microscope (SEM) analysis

[0083] Figure 2 Figure 1 is a diagram of the physical shape of the polymer. It can be observed that the polymer CMP is a reddish brown powder. Figure 3 This is a scanning electron microscope image of CMP. It can be seen that CMP has a good fluffy feeling, indicating that the pore size is larger.

[0084] 3. X-ray diffraction (XRD) analysis

[0085] Figure 4 The XRD diagram of CMP shows that CMP has obvious and sharp dispersion diffraction peaks at 2θ=14.2° and 26.7°, and several dispersion diffraction peaks of different sizes appear near 2θ=21.3°. Combined with the scanning electron microscope image, the polymer is fluffy and arranged irregularly, which shows that CMP is a special amorphous material.

[0086] 4. Solid-state NMR characterization

[0087] The polymers were characterized at the molecular level by solid-state nuclear magnetic resonance spectroscopy. The solid-state nuclear magnetic resonance spectra of intermediate compound 2 and CMP are shown in Figure 5 and Figure 6 .from Figure 5 It can be seen that the chemical shift of hydrogen on carbon 5 and carbon 6 on the benzene ring is at 7.67ppm. Figure 6 It can be seen that the C=N (No. 1) on the triazine ring and the quinoxaline ring is assigned to 183.7ppm, 145.3ppm is the CN (No. 2) on the quinoxaline ring, the chemical shifts of No. 3, 4, and 5 C on the benzene ring are 133.4, 130.3, and 125.6ppm, respectively, and the chemical shift of the alkynyl (No. 6, -C≡C-) is 77.1ppm. These data indicate that the porous polymer was successfully prepared.

[0088] 2. Performance Test

[0089] 1. Preparation of relevant solutions:

[0090] 0.01mg·mL -1 Preparation of CMP mother solution

[0091] Use an electronic balance to accurately weigh 0.001 g of the CMP powder prepared in Example 1, put it into a beaker, add N,N-dimethylformamide (DMF) as a solvent to dissolve it, stir and ultrasonicate it during dissolution, then transfer it to a volumetric flask, make up the volume, attach a label, indicate the solution name, concentration, and preparation date, and use the resulting solution as a mother solution for later use.

[0092] 10 -3 mol·L -1 Preparation of cationic solution

[0093] Calculate the mass of the required compound solute, weigh it accurately using an electronic balance, place the compound in a beaker, add ultrapure water (H2O) as a solvent to dissolve it, and perform ultrasonic treatment on insoluble substances. Then transfer it to a volumetric flask, make up the volume, and label it, indicating the solution name, concentration, and preparation date. The resulting solution is the various ion solutions used subsequently.

[0094] 2. Cation selective sensitivity experiment

[0095] Preparation of cationic solution: Use an analytical balance to accurately weigh a certain amount of metal ion-containing compounds and dissolve them in ultrapure water (H2O) to form multiple 10 -3 mol·L -1 The cationic solution is ready for use. The compounds used are: Cd(NO2)2·4H2O, Ni(NO3)2·6H2O, FeCl3·6H2O, MnSO4·H2O, CoCl2·6H2O, BaCO3, Cr(NO3)3·9H2O, CuSO4·5H2O, MgCl2·6H2O, AgSO4, FeSO4·7H2O, CaCl2·4H2O, AlCl3·6H2O, Pb(NO3)2.

[0096] Add 2 mL of 0.01 mg mL -1 CMP mother solution, and then add 20μL of each metal cation solution, and observe the change of fluorescence intensity in each centrifuge tube under the irradiation of a portable ultraviolet analyzer (365nm), and take pictures for comparison. Figure 7 As shown in the figure, by comparing with the blank group without any cations added, it was found that most metal cations had almost no effect on the fluorescence intensity of CMP, a small number of metal cations could enhance the fluorescence intensity of CMP, and Ag + The addition of can almost quench the fluorescence of CMP. By comparing the pictures, such obvious quenching phenomenon can be concluded that CMP has a strong effect on Ag. + selection sensitivity.

[0097] 2. Chemical sensing of metal cations by CMP

[0098] The CMP mother solution prepared above is still used, with a mass concentration of 10 -2 mg·mL -1 ; The preparation contains (K + 、Na + , Ba 2+ Mg 2+ , Ca 2+ 、Ag + , Cu 2+ , Fe 2+ , Mn 2+ 、Ni 2+ 、Co 2+ Cr 3+ 、Zn 2+ 、Cd 2+ , Fe 3+ ) cation solution, the concentration is 10 -3 mol·L -1 The fluorescence intensity was detected using a fluorescence photometer.

[0099] Ag, where the quenching phenomenon is most obvious + For example, add 3 mL of mother solution into the cuvette, use a fluorescence photometer to measure the fluorescence intensity as I0, then gradually add silver ion solution, shake it to mix it thoroughly, and then measure its fluorescence intensity as I, and repeat this operation until the fluorescence intensity of CMP no longer changes or changes very little.

[0100] Based on the above experiments, the content of the solution added with each metal cation can be set to 0, 20, 40, 60, 80, and 100 μL. In order to eliminate the interference of H2O, we also conducted the above experiment. The results are as follows Figure 8 As shown in the figure, we can see from the comparison that H2O can increase the fluorescence intensity of CMP, but the range is not large; with the increase of the concentration of many cations, the fluorescence intensity of CMP has no obvious change; in the above experiment, we observed the Ag + The conclusion that it has a significant quenching effect on CMP is also established.

[0101] From this we can conclude that CMP materials are + There is no specific selection function, and it has no substantial effect on the research of CMP sensing performance. + As the concentration increases, the fluorescence intensity of the CMP gradually decreases, until finally all the fluorescence phenomena almost disappear completely. This is the effect of CMP on Ag. + The result of specific selection.

[0102] 3. Calculation of the quenching percentage of CMP after adding metal cations

[0103] The quenching percentage refers to an indicator that can intuitively compare the quenching effects of different metal cations on the polymer material itself at the same concentration, and can more accurately express the specific expression ability of the polymer material for metal cations.

[0104] The fluorescence quenching percentage formula is:

[0105] Quenching percentage (%) = (I0-I) / I0×100%

[0106] I0 refers to the fluorescence intensity of the polymer stock solution without the addition of analytes, and I refers to the fluorescence intensity after the addition of different analytes.

[0107] The comparison of the quenching percentage of CMP after adding metal cations is shown in the figure below. Fig. 9 As shown, add 10 -3 mol·L -1 Cation (100 μL), Ag + The quenching of CMP can basically reach 100%, which fully proves that the polymer material is resistant to silver ions (Ag + ) specific selection. At the same ion concentration, it is followed by copper ions (Cu 2+ )13%, ferrous ion (Fe 2+ )12%, manganese ion (Mn 2+ )12%, and there are also some ions that can enhance the fluorescence intensity of polymer materials, such as calcium ions (Ca 2+ ), magnesium ion (Mg 2+ ), iron ions (Fe 3+ ), H2O. The remaining other ions have little quenching effect on polymer materials.

[0108] 4. Competition experiment of metal cations

[0109] In previous experiments, we have clearly known that polymer materials have a + In order to better understand the degree of specific selection, we set up a competition experiment.

[0110] The experimental steps are as follows: Take the mass concentration of 10 -2 mg·mL -1 3 mL of CMP mother solution was placed in a cuvette and a concentration of 10 -3 mol·L -1 100 μL of metal cation solution was added, and its fluorescence intensity was measured by fluorescence photometer. The fluorescence intensity at this time was the effect of a single metal cation on the CMP. Finally, the same concentration and content of Ag were added. +, and detect the fluorescence intensity again. We can draw a comparison chart based on the changes in fluorescence intensity twice, and more intuitively see the effect of polymer materials on Ag under complex conditions. + The anti-interference ability of the detection is strong. Fig.10 , we can see that among many metal cations, polymer materials have the strongest affinity for Ag + single selectivity.

[0111] 5. CMP for Ag + Sensitivity testing

[0112] We all know that when determining whether a polymer can be used as a fluorescent sensor material, one of the important factors to consider is sensitivity. In the following experiment, we will use the limit of detection (LOD) to represent the detection sensitivity of the polymer material to the analyte.

[0113] Quenching constant (K SV )The formula is:

[0114] I0 / II=K SV ·[Q], formula (1)

[0115] [Q] refers to the concentration of the polymer suspension, K SV is referred to as the quenching constant.

[0116] The formula for the detection limit is:

[0117] LOD=3δ / K SV , formula (2)

[0118] δ is the calculated standard deviation obtained from 10 measurements of the fluorescence of the polymer stock solution.

[0119] S = Sqrt[(∑(Xi-X) 2 ) / (N-1)], formula (3)

[0120] Xi represents sample data, X represents the mean of sample data, and N represents the number of sample data.

[0121] Take the mass concentration as 10 -2 mg·mL -1 CMP mother solution, test its fluorescence intensity I0 at 450nm, and Ag + The solution was added to the CMP mother solution and mixed. The fluorescence intensity I at 450 nm was tested and (I0-I) / I0 was calculated. Ag was added dropwise. + The fluorescence intensity I of the mixed solution at 450nm was tested repeatedly to establish the relationship between (I0-I) / I0 and the Ag content in the solution to be tested. + The results are shown in Fig.11 .

[0122] From the above Fig.11 a It can be seen that CMP has a great influence on Ag + It has very good sensitivity and provides a very good entry point for the future exploration and application of polymer materials. Fig.11 b It can be seen that the addition of Ag + The fluorescence intensity change after Ag + The concentration showed an excellent linear relationship (R 2 =0.994). The linear equation is y (Ag+) =0.00576x-0.00143, R 2 =0.994, Ag + The quenching constant K SV =1.5×10 4 , the detection limit is (LOD) = 2.5 × 10 -6 mol·L -1 .

[0123] 6. Effect of pH value

[0124] In order to explore the tolerance of the polymer and whether the fluorescence intensity of the polymer changes under different pH environments, we conducted the following experiment: We used hydrochloric acid and potassium hydroxide to mix and prepare buffer solutions with pH values ​​of 2, 4, 6, 8, and 10, and used a pipette to accurately measure 3 mL of each solution and put it into a cuvette to create different pH environments. Finally, we added 500 μL of CMP mother solution and put it into a fluorescence photometer to measure the fluorescence intensity. The results are as follows: Fig.12 As shown in the figure, in an acidic environment, the peak value of the curve gradually decreases, reaching the highest value at pH = 6; in an alkaline environment, the curve does not change much; on the contrary, the fluorescence intensity is the weakest at pH = 7. This is because the H2O added to create a pH = 7 environment will dilute the concentration of the mother solution to a certain extent.

[0125] 7. Anion selective sensitivity test

[0126] The experimental steps are basically the same as those of metal cations. We chose (B4O7 2- WO4 2- , S 2- 、Cr2O7 2- 、S2O3 2- 、MnO4 - 、F - Br - 、NO2 - 、HSO4 - 、CO3 2- 、HCO3 - , Cl - 、SO42- ) ion solution was used for preliminary experiments, and the results were photographed as shown in Fig.13 As shown. Through visual observation, it was found that when MnO4 - , the fluorescence intensity becomes weaker. To explore this issue in more depth, we use a fluorescence photometer to detect changes in fluorescence intensity.

[0127] 8. Chemical sensing of anions by CMP

[0128] The operation is similar to that of cations, and the results are as follows Fig.14 As shown in the figure, it can be clearly seen from the comparison of the bar graph that with the continuous increase of anion concentration, most anions have a very small effect on CMP, and the degree of change in fluorescence intensity is very small; while MnO4 - , which makes the fluorescence intensity of CMP change significantly. When the added concentration reaches 33μM, the fluorescence intensity suddenly decreases. This experiment can be used to test the selective detection of MnO4 by fluorescent probes - possibility.

[0129] But MnO4 - , in the solution, it appears purple-red. In order to prove whether this color has an effect on the fluorescence phenomenon of CMP, we conducted a demonstration. First, 3 mL of CMP mother solution was added to the cuvette, and then potassium permanganate solution was added. The results are shown in Fig.15 a, with the MnO4 - As the concentration increases, the color of the solution in the cuvette becomes darker. Fig.15 b is the corresponding UV spectrum, an elliptical peak appears in the 300-400nm range. - As the concentration increases, a blue shift occurs and the absorbance intensity becomes weaker and weaker until the peak disappears. It can be inferred that MnO4 - The color itself has no effect on the CMP fluorescence intensity.

[0130] 9. Anion quenching percentage

[0131] like Fig.16 As shown in Figure 2, when 700 μL of anion solution was added, the quenching percentage of CMP by most anions was about 25%, and the one that had the greatest impact on the fluorescence intensity was MnO4 - 87.7%, followed by Cr2O7 2- 49.9%, followed by NO3 - 35%. Through experimental research, it was confirmed that the CMP can efficiently detect MnO4 - .

[0132] 10. Anion competition experiment

[0133] Even if CMP is effective for MnO4 - It has good selectivity and sensitivity, but if it is really used in practice in the future, there are many uncontrollable factors. For this reason, we need to conduct anion anti-interference tests on CMP. -2 mg·mL -1 3 mL of CMP mother solution was placed in a cuvette and a concentration of 10 -3 mol·L -1 100 μL of anion solution was added, and its fluorescence intensity was measured by a fluorescence photometer. The fluorescence intensity at this time was the effect of a single anion on the CMP; finally, the same concentration and content of MnO4 - , and detect the fluorescence intensity again. We can draw a comparison chart based on the changes in fluorescence intensity twice, and more intuitively see the effect of polymer materials on MnO4 under complex conditions. - The anti-interference ability of the detection is strong. Fig.17 As shown in Figure 2, many anions also showed an effect on CMP at the beginning, but in the second step, it was found that when MnO4 - The addition of MnO4 increases the intensity of quenching, and almost decreases to about 20% of the original fluorescence intensity. This experiment shows that the sudden decrease in CMP fluorescence intensity is mainly due to the addition of MnO4 - and is not affected by other anions.

[0134] 11. CMP for MnO4 - Sensitivity test

[0135] Similar to Ag + For the test, we used a low concentration of MnO4 - ions, a drop-adding experiment was conducted on the CMP mother solution, and the fluorescence intensity was detected by a fluorescence photometer to describe the polymer material's effect on MnO4 - The detection sensitivity of Fig.18 a shows that as MnO4 - With the increase of concentration, the fluorescence intensity of the polymer material became weaker and weaker until 650 μL MnO4 was added. - , the fluorescence intensity changes almost unchanged, we can think that the maximum limit has been reached. Fig.18 b It can be seen that with the increase of MnO4 - There is a good linear relationship between the increase of concentration and the decrease of CMP fluorescence intensity (R 2 =0.996), y (MnO4 -)=0.037x-1.65,R 2 =0.996; MnO4 - Ion quenching constant K SV =5.1×103 , limit of detection (LOD) = 7.4 × 10 -6 mol·L -1 . This shows that the polymer material has a great influence on the MnO4 - Good sensitivity.

[0136] 12. Ag + Anti-interference experiment (for anions)

[0137] Through the above experiments, we have learned that Ag + The fluorescence intensity of the polymer material can be reduced, while Ag + It can also combine with some anions to form precipitation, so in the next experiment, we will explore, in the first Ag + Under the premise of existence, adding different anions respectively has no effect on the polymer material.

[0138] The concentration of the mother solution used is still 10 -2 mg·mL -1 , Ag + The concentration is 10 -3 mol·L -1 , anion concentration is 0.1 mol·L -1 .

[0139] Add 3 mL of the mother solution to the cuvette and measure its initial fluorescence intensity; then add Ag + 100μL of solution was added and the fluorescence intensity was measured; finally, 300μL of anion solution was added and the final fluorescence intensity was measured. By comparing the fluorescence intensity at different stages, we can conclude Fig.19 .

[0140] pass Fig.19 We found that adding Ag + When the fluorescence intensity decreases, but when other anions are added, the already decreased fluorescence intensity is enhanced. 2- Br - , Cl - ), can recover to about 40% of the initial strength; while MnO4 - Can be in Ag + Under the premise of quenching the polymer material, the material tends to be completely quenched, reflecting the dual quenching ability of these two ions.

[0141] 13. Relative intensity of fluorescence quenching

[0142] The quenching constants of polymer CMP for different cations were calculated and compared. Fig. 20 As shown in a, polymer CMP has an effect on Ag +The quenching constant of Ag can be as low as 1000 times that of other ions and as high as 3500 times. Such clear data comparison can further highlight the effect of polymer CMP on Ag. + The sensitivity of the polymer material to Ag is much higher than that to other ions, which further illustrates that the polymer material is sensitive to Ag. + The excellent selectivity of the material has laid a good experimental data foundation for further exploration of the material.

[0143] The quenching constants of polymer CMP for different cations were calculated and compared. Fig. 20 As shown in b, CMP has an effect on MnO4 - The quenching constant of the ions can be as low as 50 times that of other ions and as high as 120 times, which is lower than that of Ag mentioned above. + data, but it still reflects the effect of polymer materials on MnO4 - Excellent selectivity.

[0144] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.

Claims

1. Conjugated microporous polymer with quinoxaline diol as recognition group, It is characterized in that The conjugated microporous polymer is denoted as CMP, and its structure is shown in formula (I):

2. The method for preparing a conjugated microporous polymer with quinoxaline diol as a recognition group according to claim 1, It is characterized in that The conjugated microporous polymer represented by formula (I) is obtained by polymerization through coupling reaction using 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine and 2,3-dihydroxy-5,8-dibromo-quinoxaline as monomers.

3. The preparation method according to claim 2, Features: The specific steps of the coupling reaction are as follows: 2,3-dihydroxy-5,8-dibromo-quinoxaline and 2,4,6-tris(4-ethynylphenyl)-1,3,5-triazine are weighed in a molar ratio of 1 to 1.5:1 and placed in a reaction container, catalysts tetrakis(triphenylphosphine)palladium and cuprous iodide are added to the reaction container, and the reaction container is degassed with nitrogen; toluene is injected into the reaction container, and at the same time, the instrument is turned on for stirring to degas with nitrogen; triethylamine is then injected into the reaction container to degas with nitrogen; after the nitrogen degassing is completed, the reaction temperature is raised to 78 to 82°C, and a cover is used to avoid light while maintaining nitrogen protection, and the reaction is continued for 40 to 55 hours; after the reaction is completed, the reaction container is cooled to room temperature, washed, and then Soxhlet extraction is performed with methanol, and the product is dried to obtain the conjugated microporous polymer.

4. The preparation method according to claim 2, Features: The 2,3-dihydroxy-5,8-dibromo-quinoxaline is prepared by the following method: oxalic acid and 1,4-dibromo-2,3-diaminobenzene are weighed in a molar ratio of 1:1 to 1.3, and are respectively dissolved with hydrochloric acid; the two solutions are mixed in a reaction container, and heated under reflux for a period of time; after cooling to room temperature, the obtained precipitate is separated by filtration, washed with water and dried to obtain 2,3-dihydroxy-5,8-dibromo-quinoxaline.

5. The preparation method according to claim 4, Features: The 1,4-dibromo-2,3-diaminobenzene is prepared by the following method: 4,7-dibromobenzo[c]-1.2.5-thiadiazole and sodium borohydride are weighed in a molar ratio of 1:10-15, dissolved in anhydrous ethanol, and added to a reaction container of a reflux reaction device; then a small amount of cobalt chloride hexahydrate is added to perform a reflux reaction; after the reflux is completed, the reaction container is cooled to room temperature; after the solution is filtered and separated, the filtrate is spin-dried and water is added, and then dichloromethane is added for extraction, and the extract is collected in a conical flask; finally, anhydrous sodium carbonate is added, the upper opening is wrapped with a paper towel, and it is left for about 1 hour. After the solvent is evaporated, 1,4-dibromo-2,3-diaminobenzene is obtained.

6. The preparation method according to claim 3, Features: The amounts of tetrakis(triphenylphosphine)palladium and cuprous iodide used are 1% and 0.4% of the mass of 2,3-dihydroxy-5,8-dibromo-quinoxaline, respectively.

7. The preparation method according to claim 5, Features: The reflux reaction time is 2 to 3 hours.

8. Use of the conjugated microporous polymer according to claim 1, Features: The conjugated microporous polymer was used as a fluorescent sensor for Ag in solution. + or MnO4 - Detection.

9. The use according to claim 8, It is characterized in that The Ag + Or the method used for the detection of MnO4- is: (1) Prepare a CMP mother solution of a certain concentration using DMF as solvent and test its fluorescence intensity I 0 , Ag + Or MnO4- solution is added to CMP mother solution and mixed, and the fluorescence intensity I is tested and calculated (I 0 -I) / I 0 ; Continue to add Ag + or MnO4 - Solution, test the fluorescence intensity I of the mixed solution, repeat several times to establish (I 0 -I) / I 0 With Ag in the test solution + Or the linear relationship of the concentration of MnO4-; (2) Under the same conditions as step (1), add the sample solution to be tested to the CMP mother solution, detect the fluorescence intensity I of the mixed solution, and use the linear relationship obtained in step (1) to calculate the Ag content in the sample solution to be tested. + or MnO4 - concentration.

10. The use according to claim 9, Features: The fluorescence intensity was tested at 450 nm.

Citation Information

Patent Citations

  • Quinoxaline-based conjugated microporous polymer, photoelectrochemical sensor, preparation methods of quinoxaline-based conjugated microporous polymer and photoelectrochemical sensor, and dopamine detection method

    CN115505104A

  • Quinoxaline-based conjugated microporous polymer grafted graphene material, photoelectrochemical sensor, preparation method and rifampicin detection method

    CN115612115A

  • Diketimine-connected covalent organic framework polymer material and preparation method thereof

    CN115947911A

  • Hydroxyl-rich triazinyl conjugated microporous polymer as well as preparation method and application thereof

    CN117304455A

  • Quinoxalinedione derivative and method for producing the same and use thereof

    JP2006241048A