Method for preparing bio-based polyester crosslinking material by using citric acid
Through the cross-linking reaction of citrate-based DMTE-M and secondary alcohol under heating and low vacuum conditions, a bio-based polyester cross-linking material with high Tg and high mechanical properties was prepared, and the bio-based epoxy resin was solved with low Tg and ring The problem of non-renewable pollution of oxygen resins has achieved high-performance and environmentally friendly material solutions.
Patent Information
- Application Number
- CN202310547089.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-22
AI Technical Summary
The glass transition temperature (Tg) of existing bio-based epoxy resins is low, making it difficult to meet the industrial application needs of high-use temperatures, especially in the fields of precision electronic instruments and aerospace, and the non-renewable and environmental pollution of traditional epoxy resins Problems are prominent.
Tetraethyl citrate 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester (DMTE) -M) crosslinked with secondary alcohol under heating and low vacuum conditions to prepare a high Tg bio-based polyester crosslinking material. Using tetrabutyl titanate as a catalyst, high crosslinking density and High mechanical properties material.
It achieves high glass transition temperature, mechanical strength and thermal stability, the materials are easy to process and diversify functions, and can chemically degrade, avoid environmental pollution, and have better performance than traditional bisphenol A epoxy resin, and has the potential for industrial production.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of renewable resource utilization and green synthesis, and specifically to a method for preparing a polyester cross-linking material by using citric acid-based 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester (DMTE-M) and secondary alcohol. Background Art
[0002] Bisphenol A epoxy resin is the most widely used epoxy resin, accounting for more than 90% of the entire epoxy resin market. However, as a petroleum-based derivative, bisphenol A is non-renewable, and most aged, damaged and discarded epoxy resins are disposed of by incineration or landfill, causing serious environmental pollution. In addition, global oil energy reserves have dropped sharply. It is particularly important to explore and find bio-based polymer materials to replace bisphenol A epoxy resin, which is in line with the needs of the era of sustainable development.
[0003] In industrial applications, the thermosetting materials produced need to have a high glass transition temperature (T g ) to meet the requirements of high operating temperatures, especially for precision electronic instruments and aerospace applications. The T g Relatively low, a commercially valuable high T g Bio-based polymer materials are of great significance.
[0004] The present invention proposes a solution to the above problems. In order to make the polyester material achieve high T g A new type of bio-based rigid tetraester monomer DMTE-M was synthesized using diethyl 1,3-acetonedicarboxylate as raw material, and was melt-polycondensed with rigid secondary alcohol to prepare a bio-based polyester cross-linked material with high cross-linking density, which also has strong mechanical properties and high thermal stability. Summary of the invention
[0005] In view of the above-mentioned problems, the present invention uses a new rigid tetraester monomer DMTE-M to prepare a polyester cross-linked material. The method has a simple synthesis process, mild reaction conditions, high yield, low raw material price, is green and environmentally friendly, and is easy to promote industrialization.
[0006] The technical solution of the present invention:
[0007] A method for preparing polyester using citric acid-based raw materials, using 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester and secondary alcohol as raw materials, using tetrabutyl titanate as a catalyst, and preparing a polyester cross-linked network under heating and low vacuum conditions, the steps are as follows:
[0008] 1) Preparation of monomer 3,7-dihydroxy-1,5-dimethylbicyclo[3.3.0]-2,6-diene-2,4,6,8-tetracarboxylic acid ethyl ester (DMTE) from 1,3-acetonedicarboxylic acid diethyl ester
[0009] A certain amount of sodium bicarbonate was added to the ethanol-water solution. After the sodium bicarbonate was fully dissolved, 1,3-acetone diethyl carboxylate and 2,3-butanedione were added. The mixture was stirred overnight at room temperature. When solid was generated, a crude product was obtained by suction filtration. The monomer DMTE was obtained by recrystallization with methanol.
[0010] 2) Preparation of 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester (DMTE-M) from monomer DMTE
[0011] First, an appropriate amount of monomer DMTE was dissolved in acetone, and then anhydrous potassium carbonate and excess methyl iodide were added. The mixture was stirred continuously at room temperature, and the reaction was monitored by TLC until completion. Finally, the mixture was filtered, rotary evaporated, and recrystallized with methanol to obtain the monomer DMTE-M.
[0012] 3) Preparation of bio-based polyester cross-linked materials
[0013] According to the alcohol-ester equivalent ratio of 1:1, the corresponding DMTE-M, 1,4-cyclohexanediol and castor oil are weighed in a three-necked flask, and finally an appropriate amount of tetrabutyl titanate catalyst is added. Under nitrogen atmosphere, heating and stirring are performed. As the temperature rises, the solid gradually dissolves. When the viscosity of the solution increases to a certain extent, the solution is quickly transferred to a PTFE tray and placed in a vacuum oven to continue heating for post-curing to obtain a polyester cross-linked material.
[0014] Beneficial effects of the present invention:
[0015] 1) The raw material of the polyester cross-linking material of the present invention is derived from 1,3-acetone dicarboxylic acid diethyl ester, which is a product processed from citric acid. This raw material has a wide source, is low in price, is renewable, and reduces dependence on petroleum resources.
[0016] 2) The polyester cross-linking material intermediate synthesis method provided by the present invention is green and environmentally friendly, has a high yield, and the polyester synthesis process is simple and easy to operate, which is conducive to industrial production.
[0017] 3) The polyester cross-linked material provided by the present invention has high cross-linking density, high glass transition temperature, high mechanical strength, and good thermal stability. At the same time, the material is easy to process and easy to achieve structural and functional diversification. The performance is better than that of bisphenol A epoxy resin material and has the potential for industrial output.
[0018] 4) The polyester cross-linked material provided by the present invention can be chemically degraded, will not cause environmental pollution, and meets environmental protection requirements. DETAILED DESCRIPTION
[0019] The specific implementation methods given below are only a further explanation of the present invention. It should be pointed out that the following implementation methods are only a further explanation of the present invention and cannot be understood as limiting the scope of protection of the present invention. Non-essential changes made to the present invention by ordinary personnel related to this field, including the selection of catalysts and the adjustment of vacuum conditions, all fall within the scope of protection of the present invention.
[0020] Example 1: Preparation of DMTE monomer
[0021] Take a 250mL three-necked flask, weigh 80mL water, 40mL ethanol, and 1.68g sodium bicarbonate, respectively, and add them to the three-necked flask in sequence, stir thoroughly until the sodium bicarbonate is completely dissolved, then add 24.90g of 1.3-acetone diethyl carboxylate to the mixed solution, and finally add 5.24g of 2,3-butanedione, continue stirring overnight at room temperature to generate a white solid. The reaction solution is filtered to obtain a crude product, and recrystallized with methanol to obtain a white solid 3,7-dihydroxy-1,5-dimethylbicyclo[3.3.0]-2,6-diene-2,4,6,8-tetracarboxylic acid ethyl ester (DMTE), with a yield of 76%.
[0022] Example 2: Preparation of DMTE-M monomer
[0023] Take a 150mL three-necked flask, add 5.00g of DMTE, 11.00g of anhydrous potassium carbonate, 11.02g of methyl iodide and 70mL of acetone solution in sequence, and stir continuously for 72h at room temperature. The reaction is completed by monitoring by TLC. The mixture is filtered with a Buchner funnel to remove potassium carbonate, the filtrate is collected and acetone is removed by rotary evaporation to obtain a crude product, and finally recrystallized with methanol to obtain a white solid powder DMTE-M with a yield of 81%.
[0024] Example 2: Preparation of bio-based polyester cross-linked materials
[0025] Take a 50mL three-necked flask, add 12.00g DMTE-M, 5.34g 1,4-cyclohexanediol, 4.68g castor oil and 11.01mg tetrabutyl titanate in sequence according to the alcohol-ester equivalent ratio of 1:1, heat to 140°C under nitrogen atmosphere and stir continuously. As the temperature rises, the solid gradually dissolves. When the viscosity of the solution increases to a certain extent, the solution is quickly transferred to a polytetrafluoroethylene tray, placed in a vacuum oven and continued to heat for post-curing. Slowly increase the temperature (80-120°C) and maintain a low vacuum degree to obtain a flat polyester cross-linked material.
Claims
1. A method for preparing a polyester crosslinking material using 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester (DMTE-M) and secondary alcohol, using monomers DMTE-M, 1,4-cyclohexanediol, and castor oil as raw materials and tetrabutyl titanate as a catalyst, under heating and low vacuum conditions to prepare the polyester crosslinking material, the steps are as follows: 1) Preparation of monomer 3,7-dihydroxy-1,5-dimethylbicyclo[3.3.0]-2,6-diene-2,4,6,8-tetracarboxylic acid ethyl ester (DMTE) from 1,3-acetonedicarboxylic acid diethyl ester Add distilled water, ethanol and sodium bicarbonate to a three-necked flask in sequence, stir thoroughly until the sodium bicarbonate is completely dissolved, then add 1.3-acetone diethyl carboxylate to the mixed solution, and finally add 2,3-butanedione, stir overnight at room temperature, and after the reaction is completed, filter the reaction solution to obtain a crude product, and recrystallize with methanol to obtain white solid DMTE. 2) Preparation of 2,5-dimethoxy-3a,6a-dimethyl-1,3a,4,6a-tetrahydropentene-1,3,4,6-tetracarboxylic acid tetraethyl ester (DMTE-M) from monomer DMTE In a three-necked flask, monomer DMTE, anhydrous potassium carbonate, methyl iodide and acetone solvent were added in sequence and stirred continuously for 72 hours at room temperature. The reaction was completed by monitoring by TLC. The mixture was filtered through a Buchner funnel to remove potassium carbonate, the filtrate was collected and acetone was removed by rotary evaporation to obtain a crude product, and finally recrystallized from methanol to obtain a white solid powder DMTE-M. 3) Preparation of polyester cross-linked materials The alcohol and ester are added into a three-necked flask in a molar ratio of 1:1, and the monomers DMTE-M, 1,4-cyclohexanediol, castor oil and tetrabutyl titanate are added in sequence. Under nitrogen atmosphere, the mixture is heated to 140°C and stirred continuously. As the temperature rises, the solid gradually dissolves. When the viscosity of the solution increases to a certain extent, the solution is quickly transferred to a PTFE tray and placed in a vacuum oven for continued heating for post-curing. The temperature is slowly increased and a low vacuum degree is maintained to obtain a smooth polyester cross-linked material.
2. The method for preparing DMTE monomer using diethyl 1,3-acetonedicarboxylate according to claim 1, characterized in that: The usage ratio of the distilled water, ethanol, sodium bicarbonate, diethyl 1,3-acetone dicarboxylate and 2,3-butanedione is 80 mL: 40 mL: 1.68 g: 24.90 g: 5.24 g.
3. The method for preparing DMTE-M monomer from DMTE monomer according to claim 1, characterized in that: The usage ratio of the monomers DMTE, anhydrous potassium carbonate, methyl iodide and acetone is 5.00 g: 11.00 g: 11.02 g: 70 mL.
4. The method for preparing a polyester cross-linked material using a monomer DMTE-M and a secondary alcohol according to claim 1, characterized in that The mass of the catalyst tetrabutyl titanate is 0.05% of the total mass of the reactants.
5. During the preparation of the polyester, the catalyst is preferably tetrabutyl titanate; and the vacuum degree of post-curing is carried out at 0.03-0.05 mbar.