Silicon-based polyethersulfone, preparation method thereof, polyethersulfone coating and application of polyethersulfone coating
By grafting silicone in polyethersulfone to form a network structure, the problem of poor wear resistance of polyethersulfone non-stick coating is solved, which significantly improves the hardness and wear resistance of the coating and extends the service life of the cooker.
Patent Information
- Application Number
- CN202411249901.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
Polyethersulfone non-stick coatings have poor wear resistance, resulting in surface scratches and coating peeling during use at high temperatures, affecting the service life of the cooker.
Using silicon-based polyethersulfone, the network structure is formed by grafting silicones in the polyethersulfone, which improves the hardness and wear resistance of the coating, and optimizes the polyethersulfone coating by specific preparation methods and component ratios. performance.
It significantly improves the hardness and wear resistance of the polyethersulfone coating, extends the service life of the cooker, and maintains good performance at high temperatures.
Smart Images

Figure CN118994581A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of coatings, and in particular to a silicon-based polyethersulfone and a preparation method thereof, a polyethersulfone coating and an application thereof. Background Art
[0002] Polyethersulfone (PESU) is a high-performance thermoplastic engineering plastic with excellent heat resistance. It can work stably at higher temperatures. Due to its good adhesion to metals such as iron, it is used in non-stick coatings for cookware.
[0003] Although polyethersulfone non-stick coatings can ensure chemical stability at high temperatures, the coating formed by polyethersulfone non-stick coatings is soft in texture and has poor wear resistance, which leads to problems such as surface scratches and coating shedding during use, affecting the service life of the cookware. Summary of the invention
[0004] In view of the above problems, the present invention proposes a silicon-based polyethersulfone and a preparation method thereof, a polyethersulfone coating and an application thereof, aiming to solve the problems of poor wear resistance of existing polyethersulfone non-stick coatings.
[0005] To this end, the present invention provides a silicon-based polyethersulfone, which includes at least one of the compounds represented by formula (I);
[0006]
[0007] Among them, R1 and R2 are alkyl groups.
[0008] In one embodiment, R1 and R2 are each selected from a methyl group, an ethyl group, a propyl group, and a butyl group.
[0009] In one embodiment, R1 and R2 are the same.
[0010] In one embodiment, n≧21, and / or n≦25.
[0011] The present invention also provides a method for preparing silicon-based polyether sulfone, wherein at least one of the compounds represented by formula (II) is subjected to an addition reaction with a monomer under the catalytic action of a catalyst to obtain silicon-based polyether sulfone represented by formula (I);
[0012]
[0013] The monomer is selected from at least one of 4,4'-bis(sulfonyl) chloride diphenyl ether and 4-sulfonyl chloride diphenyl ether.
[0014] In one embodiment, the addition reaction temperature is 130° C.-170° C.; and / or the addition reaction time is 3.5 h-5.0 h.
[0015] In one embodiment, the catalyst is ferric chloride, and the amount of ferric chloride added is 0.8%-1.5% of the mass of the base material.
[0016] In one embodiment, the compound represented by formula (II) is obtained by reacting the compound represented by formula (III) in sequence under the catalytic action of deaminase, sulfuric acid, and antimony trioxide;
[0017]
[0018] Among them, R3 and R4 are alkyl groups.
[0019] In one embodiment, the addition amount of the deaminase is 0.2%-0.8% of the mass of the base material; and / or the catalytic reaction temperature of the deaminase is 20° C.-35° C., and the catalytic reaction time of the deaminase is 1.5 h-4 h.
[0020] In one embodiment, the mass concentration of sulfuric acid is 85%-95%, and the amount of sulfuric acid added is 1.5%-4% of the mass of the base material.
[0021] In one embodiment, the addition amount of antimony trioxide is 1%-1.5% of the base material mass; and / or, the catalytic reaction temperature of antimony trioxide is 70° C.-90° C., and the catalytic reaction time of antimony trioxide is 3h-6h.
[0022] The present invention also provides a polyethersulfone coating, comprising the above silicon-based polyethersulfone or the silicon-based polyethersulfone prepared by the above preparation method.
[0023] In one embodiment, the amount of silicon-based polyethersulfone added to the polyethersulfone coating is 35 wt%-50 wt%.
[0024] In one embodiment, the polyethersulfone coating comprises the following components in percentage by weight:
[0025] Silicon-based polyethersulfone 35%-50%, polyamide-imide 5%-15%, silicon carbide 5%-15%, aluminum oxide 2%-7%, dispersant 1%-3%, preservative 1%-3%, carbon black powder 1%-3%, neutralizer 1%-3%, enhancer 1%-3%, surfactant 0.5%-2%, defoamer 0.5%-2%, and the balance is water.
[0026] In one embodiment, the polyethersulfone coating has a Si═O bond absorption peak and a Si—O bond absorption peak in its infrared spectrum.
[0027] The invention also proposes the application of the polyethersulfone coating in cooking utensils and household appliances.
[0028] In one embodiment, the cooking utensils include pots, baking utensils, and cutting tools; and / or the household appliances include heaters, rice cookers, pressure cookers, electric kettles, air fryers, and oil heaters.
[0029] In one embodiment, the polyethersulfone coating is sprayed on cookers and household appliances to form a coating with a spraying thickness of 12 μm-20 μm.
[0030] In one embodiment, the polyethersulfone coating is baked at 250° C.-300° C. for 10 min-20 min to form a coating.
[0031] The repeating units of the silicon-based polyphenylene ether provided by the present invention are grafted with siloxane, which is a compound with silicon and oxygen forming the main chain through Si-O-Si bonds, and has excellent thermal stability and chemical stability, and siloxane can maintain its physical properties in a wide temperature range (-100°C-250°C). In addition, the silicon element in siloxane can form a strong covalent bond, which can make the coating tougher when used in coatings; the silicon-oxygen bonds in siloxane can also form more crosslinks with other components in the coating, thereby improving the overall performance of the coating. Therefore, when the silicon-based polyether sulfone proposed by the present invention is applied to coatings, it can solve the problems of poor wear resistance of polyether sulfone non-stick coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 FIG. 4 is an infrared spectrum of silicon-based polyethersulfone in one embodiment of the present invention. DETAILED DESCRIPTION
[0033] The following embodiments are only used to more clearly illustrate the technical solutions of the present invention and are therefore only used as examples and are not intended to limit the scope of protection of the present invention.
[0034] "Scope" disclosed in the present invention is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3,4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present invention, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0035] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0036] In the description of the embodiments of the present invention, the term "multiple" refers to more than two (including two), and similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces). The term "at least one" refers to one or more.
[0037] Reference to "embodiments" in the present invention means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0038] The molecular structure of polyethersulfone is mainly composed of sulfone group, ether group and phenylene group. Sulfone group and ether group are alternately connected to the phenylene structure to form non-crystalline polyethersulfone. Sulfone group gives polyethersulfone heat resistance, and ether group makes polyethersulfone chain segment have good fluidity in molten state, which is easy to form and process. In addition, polyethersulfone has advantages such as good adhesion to metals such as iron, and can be used in non-stick coatings for cookware.
[0039] Although polyethersulfone non-stick coatings can ensure chemical stability at high temperatures, the coating formed by polyethersulfone non-stick coatings is soft in texture, has a hardness between FH, and has poor wear resistance, which leads to problems such as surface scratches and coating shedding during use, affecting the service life of the cookware.
[0040] In order to improve the hardness and wear resistance of the polyethersulfone non-stick coating, polyethersulfone can be grafted with a silicon source, which can form a network structure in the coating, thereby increasing the hardness and wear resistance of the coating.
[0041] Based on the above considerations, the present invention provides a silicon-based polyethersulfone, in which siloxane is grafted into the repeating unit of silicon-based polyphenylene ether.
[0042] According to some embodiments of the invention, the present invention provides a silicon-based polyethersulfone, which includes at least one of the compounds shown in formula (I);
[0043]
[0044] Among them, R1 and R2 are alkyl groups.
[0045] According to some embodiments of the present invention, R1 and R2 are respectively selected from one of methyl, ethyl, propyl and n-butyl.
[0046] R1 and R2 are respectively selected from one of methyl, ethyl, propyl and n-butyl, which means that the silicon-based polyethersulfone includes at least one of the following 16 compounds: R1 is methyl and R2 is methyl; R1 is methyl and R2 is ethyl; R1 is methyl and R2 is propyl; R1 is methyl and R2 is n-butyl; R1 is ethyl and R2 is methyl; R1 is ethyl and R2 is ethyl; R1 is ethyl and R2 is propyl; R1 is ethyl and R2 is n-butyl; R1 is propyl and R2 is methyl; R1 is propyl and R2 is ethyl; R1 is propyl and R2 is propyl; R1 is propyl and R2 is n-butyl; R1 is n-butyl and R2 is methyl; R1 is n-butyl and R2 is ethyl; R1 is n-butyl and R2 is propyl; R1 is n-butyl and R2 is n-butyl.
[0047] In the embodiment of the present invention, R1 and R2 are selected from low-carbon straight-chain alkyl groups, which have a small molecular volume and can reduce the influence of steric hindrance during grafting.
[0048] The repeating units of the silicon-based polyphenylene ether provided by the present invention are grafted with siloxane, which is a compound with silicon and oxygen forming the main chain through Si-O-Si bonds, and has excellent thermal stability and chemical stability, and siloxane can maintain its physical properties in a wide temperature range (-100°C-250°C). In addition, the silicon element in siloxane can form a strong covalent bond, which can make the coating tougher when used in coatings; the silicon-oxygen bonds in siloxane can also form more crosslinks with other components in the coating, thereby improving the overall performance of the coating. Therefore, when the silicon-based polyether sulfone proposed by the present invention is applied to coatings, it can solve the problems of poor wear resistance of polyether sulfone non-stick coatings.
[0049] According to some embodiments of the present invention, R1 and R2 are the same.
[0050] R1 and R2 being the same means that the silicon-based polyethersulfone includes at least one of the following four compounds: R1 is methyl and R2 is methyl; R1 is ethyl and R2 is ethyl; R1 is propyl and R2 is propyl; R1 is n-butyl and R2 is n-butyl.
[0051] In the embodiment of the present invention, R1 and R2 are set to be the same, which can improve the yield and reduce side reactions during grafting.
[0052] According to some embodiments of the present invention, n≥21, and / or, n≤25.
[0053] n represents the degree of polymerization of polyethersulfone, which refers to the number of repeating units contained in the polyethersulfone macromolecular chain. The embodiment of the present invention selects n≥21 because when n is less than 21, the hardness of the formed polyethersulfone resin decreases, and its color is transparent or slightly yellow (within Ghana color number 1#); n≤25 is selected because when n exceeds 25, the formed polyethersulfone resin is easily coked, and the color becomes dark yellow (Ghana color number greater than 7#); and when 21≤n≤25, the color of the formed polyethersulfone resin is transparent or slightly yellow, within Ghana color number 1#, and is more suitable for application in coatings.
[0054] According to some embodiments of the present invention, the present invention also provides a method for preparing silicon-based polyether sulfone, wherein the monomer and the compound represented by formula (II) are subjected to an addition reaction under the catalytic action of a catalyst to obtain silicon-based polyether sulfone represented by formula (I);
[0055] The monomer is selected from at least one of 4,4'-bissulfonyl chloride diphenyl ether and 4-sulfonyl chloride diphenyl ether;
[0056] Formula (II) is
[0057] Monomer refers to the compound used to form the main chain of silicon-based polyethersulfone, in which the structural formula of 4,4'-bissulfonyl chloride diphenyl ether is The structural formula of 4-sulfonyl chloride diphenyl ether is
[0058] The compound represented by formula (II) is siloxane, which has higher reactivity than silane coupling agents commonly used as silicon sources and is easier to graft into the repeating units of polyethersulfone. The silicon element in siloxane can form a strong covalent bond, which can make the coating tougher when used in coatings; in addition, the silicon-oxygen bonds in siloxane can also form more crosslinks with other components in the coating, thereby improving the overall performance of the coating.
[0059] The reaction equation of the monomer and the compound shown in formula (II) is:
[0060]
[0061] According to some embodiments of the present invention, the temperature of the addition reaction is 130° C.-170° C.; and / or the time of the addition reaction is 3.5 h-5.0 h.
[0062] The time of the addition reaction affects the degree of polymerization of the formed silicon-based polyether sulfone. When the reaction time is less than 3.5 hours, the degree of polymerization n of the formed silicon-based polyether sulfone is less than 21. When the reaction time is greater than 5 hours, the degree of polymerization n of the formed silicon-based polyether sulfone is greater than 25. Therefore, the preferred addition reaction time in this embodiment is 3.5 hours to 5 hours.
[0063] According to some embodiments of the present invention, the catalyst is ferric chloride, and the amount of ferric chloride added is 0.8%-1.5% of the mass of the base material, wherein the mass of the base material refers to the total mass of the monomer and the compound represented by formula (II).
[0064] Ferric chloride as a catalyst can increase the electrophilic affinity of chloride ions, reduce the activation energy between the electrophilic chlorine source (chlorine anions of monomer molecules) and the organic substrate, and thus provide the energy required for the reaction; secondly, the ferric chloride catalyst can react with the electrophilic chlorine source to form an intermediate, in which the metal ion forms a complex with the chloride anions of the electrophilic chlorine source, while releasing other ions or molecules (such as nucleophiles). This intermediate has high activity and can react with the organic substrate. That is, ferric chloride effectively catalyzes the self-polymerization reaction of the monomer through its Lewis acid properties, and optimizes the reaction process by increasing the activity of the electrophilic chlorine source and reducing the activation energy of the reaction.
[0065] According to some embodiments of the present invention, the compound represented by formula (II) is obtained by reacting the compound represented by formula (III) in sequence under the catalytic action of deaminase, sulfuric acid, and antimony trioxide;
[0066]
[0067] Among them, R3 and R4 are alkyl groups.
[0068] In order to obtain the siloxane represented by formula (II), the embodiment of the present invention selects to treat the silane coupling agent represented by formula (III) with relatively stable chemical properties.
[0069] The reaction equation is:
[0070]
[0071] The first step is to react under oxygen conditions, and deaminase cuts off the amino group to form an aldehyde group; the second step is to break the aldehyde group through catalytic oxidation by concentrated sulfuric acid under acidic conditions; the third step is to form the siloxane shown in formula (II) under the catalytic action of antimony trioxide.
[0072] According to some embodiments of the present invention, the addition amount of the deaminase is 0.2%-0.8% of the mass of the base material; and / or the catalytic reaction temperature of the deaminase is 20° C.-35° C., and the catalytic reaction time of the deaminase is 1.5h-4h.
[0073] The mass of the base material in the reaction process refers to the mass of the compound represented by formula (III).
[0074] According to some embodiments of the present invention, the mass concentration of sulfuric acid is 85%-95%, and the amount of sulfuric acid added is 1.5%-4% of the mass of the base material.
[0075] The mass of the base material in the reaction process refers to the mass of the product of the first step reaction.
[0076] According to some embodiments of the present invention, the addition amount of antimony trioxide is 1%-1.5% of the base material mass; and / or the catalytic reaction temperature of antimony trioxide is 70° C.-90° C., and the catalytic reaction time of antimony trioxide is 3h-6h.
[0077] The mass of the base material in this reaction process refers to the mass of the second step reaction product.
[0078] According to some embodiments of the present invention, the present invention further provides a polyethersulfone coating, including the above-mentioned silicon-based polyethersulfone or the silicon-based polyethersulfone prepared by the above-mentioned preparation method. The silicon-based polyethersulfone specifically refers to the above-mentioned embodiments. Since the polyethersulfone coating adopts all the technical solutions of all the above-mentioned embodiments, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.
[0079] According to some embodiments of the present invention, the amount of silicon-based polyethersulfone added to the polyethersulfone coating is 35wt%-50wt%. When the amount of silicon-based polyethersulfone added is too much, the coating viscosity is large, which is not conducive to spraying; when the amount of silicon-based polyethersulfone added is too low, the performance of the coating is reduced, and problems such as low adhesion and decreased hardness will occur.
[0080] According to some embodiments of the present invention, the polyethersulfone coating comprises the following components in percentage by mass:
[0081] Silicon-based polyethersulfone 35%-50%, polyamide-imide 5%-15%, silicon carbide 5%-15%, aluminum oxide 2%-7%, dispersant 1%-3%, preservative 1%-3%, carbon black powder 1%-3%, neutralizer 1%-3%, enhancer 1%-3%, surfactant 0.5%-2%, defoamer 0.5%-2%, and the balance is water.
[0082] According to some embodiments of the present invention, the infrared spectrum of the polyethersulfone coating has a Si=O bond absorption peak and a Si-O bond absorption peak.
[0083] Molecules can selectively absorb certain wavelengths of infrared light to cause transitions in the vibrational and rotational energy levels of the molecules. Infrared spectroscopy is a spectrum obtained by detecting the absorption of infrared light. Liquid polyethersulfone coating can be directly dropped between two infrared transparent salt sheets to form a liquid film, which can then be tested in an infrared spectrometer. When the polyethersulfone coating is dried into a solid sample, the sample can be mixed with an infrared transparent matrix such as potassium bromide by a tabletting method and then pressed into a thin sheet.
[0084] The wavelength range of Si=O bond absorption peak is generally 1020cm -1 -1200cm -1 The Si-O bond absorption peak includes the Si-O bond stretching vibration absorption peak and the bending vibration absorption peak. The Si-O bond stretching vibration absorption peak is generally at 800cm -1 -1000cm -1 The Si-O bond bending vibration absorption peak is generally at 450cm -1 -500cm -1 .
[0085] The invention also proposes the application of the polyethersulfone coating in cooking utensils and household appliances.
[0086] According to some embodiments of the present invention, cooking utensils include but are not limited to various pots (woks, frying pans, soup pots, etc.), baking utensils (baking trays, grills, etc.), cutting tools (kitchen knives, scissors), etc. Household appliances include but are not limited to heaters, rice cookers, pressure cookers, electric kettles, air fryers, oil heaters, etc.
[0087] According to some embodiments of the present invention, the polyethersulfone coating is sprayed on cookers and household appliances to form a coating with a spraying thickness of 12 μm-20 μm.
[0088] When spraying, the surface of the cookware can be treated by 60-100 mesh corundum sandblasting to make the surface roughness reach 2μm-3μm, and then sprayed with a starter spray gun to improve the bonding strength of the coating. Multi-layer spraying can also be performed as needed.
[0089] If the coating is too thick, the coating will be harder, the adhesion will be poor, and the coating will easily fall off; if the coating is too thin, the covering power will be poor, and substrate defects (pinholes, marks, etc.) will be easily exposed.
[0090] According to some embodiments of the present invention, the polyethersulfone coating is baked at 250° C.-300° C. for 10 min-20 min to form a coating.
[0091] The following describes the invention in conjunction with specific embodiments.
[0092] Example 1
[0093] A polyethersulfone coating comprising the following components in percentage by mass:
[0094] Silicon-based polyethersulfone 45%, Mitsubishi K2 polyamide-imide 10%, Guangzhou Nansha silicon carbide 10%, Japan Sumitomo alumina 5%, BYK110 dispersant 2%, Kason 2525 preservative 1.5%, 6# carbon black powder 1.5%, AMP-95 ammonia neutralizer 1.5%, BYK3300 enhancer 1.5%, XL80 surfactant 1%, BYK085 defoamer 1%, deionized water 20%.
[0095] The preparation method of silicon-based polyethersulfone comprises:
[0096] (1) Take 22.1g of silane coupling agent, add 0.11g of deaminase thereto, react under oxygen, the reaction temperature is 25°C, and the reaction time is 2h; after the reaction, add 0.66g of sulfuric acid with a mass concentration of 90% for catalytic reaction, the reaction temperature is 100°C, and the reaction time is 4h; after the reaction, add 0.22g of antimony trioxide, react at 80°C for 4h to obtain siloxane, the reaction equation is as follows;
[0097]
[0098] (2) 3.672 g of 4,4'-bis(sulfonyl) chloride diphenyl ether) and 1.2 g of the siloxane obtained in step (1) were mixed, 0.049 g of ferric chloride was added, and the mixture was reacted at 150° C. to obtain silicon-based polyethersulfone. The reaction equation is as follows:
[0099]
[0100] The infrared spectrum of silicon-based polyethersulfone is as follows Figure 1 As shown, among them, 1090.11cm-1 is the absorption peak of Si=O bond, 962.22cm -1 It is the stretching vibration absorption peak of Si-O bond, indicating that siloxane is grafted into the molecular chain of polyethersulfone.
[0101] Example 2
[0102] The difference from Example 1 is that the amount of silicon-based polyethersulfone added to the polyethersulfone coating of this example is 35%, and the amount of deionized water added is 25%. The remaining components and steps are the same as those of Example 1.
[0103] Example 3
[0104] The difference from Example 1 is that the amount of silicon-based polyethersulfone added to the polyethersulfone coating of this example is 50%, and the amount of deionized water added is 15%. The remaining components and steps are the same as those of Example 1.
[0105] Comparative Example 1
[0106] Comparative Example 1 is an existing polyethersulfone coating, which is purchased from Kaifeng Quark New Materials and is a polyethersulfone coating with a number of ET53300.
[0107] Comparative Example 2
[0108] A polyethersulfone coating comprising the following components in percentage by mass:
[0109] Polyethersulfone 40%, siloxane 5% (siloxane shown in Example 1), Mitsubishi K2 polyamideimide 10%, Guangzhou Nansha silicon carbide 10%, Japan Sumitomo alumina 5%, BYK110 dispersant 2%, Kason 2525 preservative 1.5%, 6# carbon black powder 1.5%, AMP-95 ammonia neutralizer 1.5%, BYK3300 thickener 1.5%, XL80 surfactant 1%, BYK085 defoamer 1%, deionized water 20%.
[0110] Comparative Example 3
[0111] Comparative Example 3 is an existing Teflon coating, which is purchased from Daikin Coatings of Japan and is numbered EK-3793M-601L.
[0112] Comparative Example 4
[0113] Comparative Example 4 is an existing ceramic coating, which is purchased from Wisdom Technology with a product number of 85007.
[0114] Comparative Example 5
[0115] Comparative Example 5 is an existing organosilicon coating, which is purchased from AsiaInfo Corporation and has a serial number of SP-6177B.
[0116] Comparative Example 6
[0117] Comparative Example 6 is an existing thermosetting coating, which is purchased from Green Earth Company with a code number of SP-2025.
[0118] Comparative Example 7
[0119] Comparative Example 7 is an existing thermoplastic coating, which is purchased from Green Earth Company with a serial number of K-8064.
[0120] Comparative Example 8
[0121] Comparative Example 8 is an existing hydroxypropyl type coating, which is purchased from Green Earth Company with a serial number of SX-AMG-3277.
[0122] Performance Test:
[0123] 20 g of the coatings in Examples 1-3 and Comparative Examples 1-8 were respectively sprayed on a tinplate substrate with a spraying thickness of , and then placed in an oven at 280° C. for 15 min to fully dry the coating. The hardness, tensile properties, wear resistance, scratch resistance and high temperature resistance of the coating were then tested.
[0124] Hardness test method: Use a specific pencil (Zhonghua brand pencil) to make a 45° angle to the coating surface, and use enough force not to break the pencil (about 20N is appropriate), or use a hardness test cart to push the coating surface, pushing forward at a uniform speed of about 1cm / s, with a scratch length of about 1cm, and scratch five times on the coating surface. The tip of the pencil should be re-grinded after each scratch before use. The result should meet the requirements of the general inspection standards).
[0125] Tensile performance test method: Place the pre-coated metal substrate in a stretching machine. The substrate stretching length is 10mm. The fracture of the coating is judged. If there is a fault or break, it is considered to be non-stretchable.
[0126] Wear resistance test method: Use detergent to prepare washing water with a concentration of 5%, 3M (7447C) scouring pad, load 2.5kgf, swing left and right as one stroke, replace the scouring pad every 250 strokes, check whether the coating is exposed to the substrate every 250 strokes (non-filled type: the test is terminated when ≥10 lines are exposed; filled type: the test is terminated when flaking falls off), and record the number of times the coating is exposed to the substrate.
[0127] Scratch resistance test method: The scraping fingers of five independent shafts act vertically on the surface of the test sample to evaluate whether there are damaging scratches on the surface of the sample, whether the material is deformed, whether there are cracks, hairiness, etc.
[0128] High temperature resistance test method: After being placed in a constant temperature environment of 250℃±2℃ for 48 hours, visually inspect the surface quality to determine if the coating has obvious discoloration, cracking, blistering, etc.
[0129] The test results are shown in Table 1.
[0130] Table 1 Test results in Examples 1-3 and Comparative Examples 1-8
[0131]
[0132] It can be seen from Table 1 that the hardness of the coating formed by the polyethersulfone coating of the embodiment of the present invention is 2H-3H, which is significantly improved compared with the hardness FH of the existing polyethersulfone coating; the wear resistance is improved from 1500 times to 6000 times, and the coating is not easily scratched. It shows that the addition of the silicon-based polyethersulfone of the present invention can significantly improve the hardness, wear resistance and scratch resistance of the polyethersulfone coating.
[0133] By comparing Example 1 and Comparative Example 2, it can be seen that the hardness, wear resistance and other properties of the polyethersulfone coating formed by mixing polyethersulfone and siloxane are significantly lower than those of the polyethersulfone coating to which silicon-based polyethersulfone is added in the present invention, indicating that the silicon-based polyethersulfone formed by grafting siloxane onto the main chain of polyethersulfone in the present invention can significantly improve the hardness and wear resistance of the coating compared to directly mixing polyethersulfone and siloxane.
[0134] Although the hardness of high temperature resistant coatings (resistant to high temperatures above 250°C) such as the ceramic coating in Comparative Example 4 and the silicone coating in Comparative Example 5 is higher than that of the polyethersulfone coating in the embodiment of the present invention, and the wear resistance is also better than that of the polyethersulfone coating in the embodiment of the present invention, the toughness of the silicone coating and the ceramic coating is poor, and cracking occurs during stretching, which easily causes the coating to fall off, thereby affecting the service life. Although the Teflon coating in Comparative Example 3 has a certain toughness, its hardness and wear resistance are lower than those of the polyethersulfone coating in the embodiment of the present invention. The thermosetting coating in Comparative Example 6, the thermoplastic coating in Comparative Example 7, and the hydroxypropyl coating in Comparative Example 8 also have a certain toughness, but their hardness, wear resistance, scratch resistance and temperature resistance are all worse than those of the polyethersulfone coating in the present invention. It can be seen from this that the coating formed by the polyethersulfone coating in the embodiment of the present invention can meet the requirements of hardness, toughness, wear resistance, scratch resistance and high temperature resistance, and has the best comprehensive performance.
[0135] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A silicon-based polyethersulfone, characterized in that: The silicon-based polyethersulfone comprises at least one of the compounds represented by formula (I); Among them, R1 and R2 are alkyl groups.
2. The silicon-based polyethersulfone according to claim 1, characterized in that The R1 and R2 are selected from methyl, ethyl, propyl and butyl respectively.
3. The silicon-based polyethersulfone according to claim 1 or 2, characterized in that The R1 and R2 are the same.
4. The silicon-based polyethersulfone according to claim 1, characterized in that Said n≥21, and / or n≤25.
5. A method for preparing silicon-based polyether sulfone, characterized in that: The silicon-based polyethersulfone represented by formula (I) can be obtained by subjecting at least one of the compounds represented by formula (II) to an addition reaction with a monomer under the catalytic action of a catalyst; The monomer is selected from at least one of 4,4'-bissulfonyl chloride diphenyl ether and 4-sulfonyl chloride diphenyl ether.
6. The method for preparing silicon-based polyethersulfone according to claim 5, characterized in that: The temperature of the addition reaction is 130° C.-170° C.; and / or the time of the addition reaction is 3.5 h-5.0 h.
7. The method for preparing silicon-based polyethersulfone according to claim 5, characterized in that: The catalyst is ferric chloride, and the addition amount of the ferric chloride is 0.8%-1.5% of the mass of the base material.
8. The method for preparing silicon-based polyethersulfone according to claim 5, characterized in that: The compound represented by formula (II) is obtained by reacting the compound represented by formula (III) in sequence under the catalytic action of deaminase, sulfuric acid and antimony trioxide; Among them, R3 and R4 are alkyl groups.
9. The method for preparing silicon-based polyethersulfone according to claim 8, characterized in that: The amount of the deaminase added is 0.2%-0.8% of the base material mass; and / or, The catalytic reaction temperature of the deaminase is 20° C.-35° C., and the catalytic reaction time of the deaminase is 1.5 h-4 h.
10. The method for preparing silicon-based polyethersulfone according to claim 8, characterized in that: The mass concentration of the sulfuric acid is 85%-95%, and the amount of sulfuric acid added is 1.5%-4% of the mass of the base material.
11. The method for preparing silicon-based polyethersulfone according to claim 8, characterized in that: The amount of antimony trioxide added is 1%-1.5% of the base material mass; and / or, The catalytic reaction temperature of the antimony trioxide is 70° C.-90° C., and the catalytic reaction time of the antimony trioxide is 3 h-6 h.
12. A polyethersulfone coating, characterized in that: The invention comprises the silicon-based polyethersulfone as described in any one of claims 1 to 4 or the silicon-based polyethersulfone prepared by the preparation method as described in any one of claims 5 to 11.
13. The polyethersulfone coating according to claim 12, characterized in that: The silicon-based polyethersulfone is added in an amount of 35wt%-50wt% in the polyethersulfone coating.
14. The polyethersulfone coating according to claim 13, characterized in that The polyethersulfone coating comprises the following components in percentage by mass: Silicon-based polyethersulfone 35%-50%, polyamide-imide 5%-15%, silicon carbide 5%-15%, aluminum oxide 2%-7%, dispersant 1%-3%, preservative 1%-3%, carbon black powder 1%-3%, neutralizer 1%-3%, enhancer 1%-3%, surfactant 0.5%-2%, defoamer 0.5%-2%, and the balance is water.
15. The polyethersulfone coating according to claim 12, characterized in that: The polyethersulfone coating has a Si=O bond absorption peak and a Si-O bond absorption peak in the infrared spectrum.
16. Use of the polyethersulfone coating according to any one of claims 12 to 15 in cooking utensils and household appliances.
17. The use according to claim 16, characterized in that The cooking utensils include pots, baking utensils, and cutting tools; and / or the household appliances include heaters, rice cookers, pressure cookers, electric kettles, air fryers, and oil heaters.
18. The use according to claim 16, characterized in that The polyethersulfone coating is sprayed on cookers and household appliances to form a coating with a spraying thickness of 12 μm to 20 μm.
19. The use according to claim 18, characterized in that The polyethersulfone coating is baked at 250° C.-300° C. for 10 min-20 min to form the coating.