Preparation method of SF hydrogel with initial equivalence and different conformation conversion rates

By regulating the crosslinking reaction conditions and proportions, SF hydrogels with equivalent initial characteristics and different protein conformation transformation rates are constructed, which solves the problem of dynamic changes in hydrogel materials in the prior art that affect cell behavior, and realizes the biological process Effective application and regulation in the field of medicine.

CN118994638AActive Publication Date: 2024-11-22DONGHUA UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410962976.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-22
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The prior art cannot effectively regulate and utilize the protein conformation in SF hydrogel to transform the microenvironment, resulting in dynamic changes in material characteristics in in vivo implantation or in vitro cell culture, affecting cell behavior, and the inability to construct equivalent initial characteristics and different proteins. Conformational transition rate hydrogel.

Method used

By mixing the SF hydrogel precursor solutions α and β, the crosslinking reaction conditions and proportions are controlled, and the initial characteristics of the hydrogel are equivalent, and the SF hydrogel preparation method is used for different conformational transformation rates. The SF/X/SPS system performs cross-linking reactions, and regulates the uniformity of the cross-linking point to control the conformational transition rate.

Benefits of technology

The construction of SF hydrogels with initial equivalent and different conformational transformation rates under mild conditions provides a platform for accurately studying the impact of protein conformational transformation on cell behavior and provides valuable guidance for tissue repair in the field of biomedical science.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994638A_ABST
    Figure CN118994638A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of biomedicine, and relates to a preparation method of an SF hydrogel with initial equivalence and different conformation transition rates, two SF hydrogel precursor solutions alpha and beta are mixed according to different proportions, and a cross-linking reaction is carried out under certain conditions for a certain time to obtain the SF hydrogel with equivalent initial characteristics and different conformation transition rates. The SF in the SF hydrogel precursor solution alpha and the SF in the SF hydrogel precursor solution beta are the same, and the concentrations of the SF are the same; the stress-strain curves of the two kinds of SF hydrogel formed after the SF hydrogel precursor solution alpha and the SF hydrogel precursor solution beta are subjected to cross-linking reaction are equivalent, the average pore size is equivalent, and the uniformity of cross-linking points is different. According to the invention, the SF hydrogel with initial equivalence and different conformation conversion rates is successfully prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedicine and relates to a method for preparing SF hydrogels with initial equivalence and different conformational transition rates. Background Art

[0002] As a natural protein material, SF (silk fibroin) has attracted much research and attention for its excellent biocompatibility, degradability and processing convenience. Among various SF materials, chemically cross-linked SF hydrogel not only inherits the natural advantages of SF, but also exhibits unique extracellular matrix biomimetic properties and highly adjustable mechanical properties. In recent years, researchers have tried to use SF hydrogel in in vitro cell culture, corneal materials, in vivo tissue repair and other fields, and have confirmed that it has good application prospects in related fields.

[0003] However, in the in vivo implantation or in vitro cell culture environment, the free movement and self-assembly of the hydrophobic segments of the SF molecules in the chemically cross-linked SF hydrogel will cause it to transform from a random coil conformation to a β-folded conformation of a lower energy level. This will inevitably lead to a dynamic conformational transition of the SF molecules in the hydrogel, which will in turn bring about dynamic changes in the physical characteristics of the SF hydrogel material, such as pore size, hardness and transmittance. A large number of research reports have confirmed that the characteristic parameters of the material, such as pore size, hardness and transmittance, can have a profound effect on the adhesion, proliferation and differentiation of cells. The conformational transition is generally evident within 1-3 weeks of initial use, and the relevant time period is generally considered to be a critical period for the material characteristics to affect cell behavior. Based on this, the protein conformational transition microenvironment in the SF hydrogel is also likely to effectively regulate the adhesion and differentiation of cells, thereby bringing a class of unknown effects that cannot be ignored to the application of such important biomaterials in interdisciplinary fields such as living cell encapsulation culture, in vitro tissue construction and in vivo tissue repair.

[0004] So far, there has been no report on the research and development of in-depth and effective regulation and utilization strategies for similar conformational transition microenvironments in the above-mentioned interdisciplinary fields, especially the development of SF hydrogel construction strategies with equivalent initial characteristics (initial characteristics refer to the initial compressive mechanical properties and average pore size characteristics of SF hydrogels. Studies have shown that the compressive mechanical properties and pore size characteristics of biomaterials have a profound impact on cell proliferation and differentiation. In the process of studying the influence of the protein conformational transition microenvironment in SF hydrogels on cell behavior, if the initial compressive mechanical properties and average pore size of the hydrogel are not equivalent, then they will be mixed with the protein conformational transition to affect related cell behaviors, so that it is impossible to accurately obtain the influence of the single factor of protein conformational transition on cell behavior) and different protein conformational transition rates. The construction of relevant material platforms is expected to study and reveal the influence of protein conformational transition microenvironments on cell behavior under the premise of eliminating various interference factors, and ultimately provide important guidance for the effective regulation of protein conformational transition in SF hydrogels and their rational utilization in the biomedical field.

[0005] At present, a small number of researchers have begun to try to construct SF hydrogels with "different conformational transition rates" and use them to study the effects of related factors on cell behavior. For example, the literature (ACS Applied Materials & Interfaces 2022, 14, 7531-7550) used SF combined with carboxymethyl cellulose and gelatin to prepare several composite hydrogels with "different conformational transition rates" and examined their effects on stem cell differentiation. However, this scheme is to achieve the purpose of changing the protein conformational transition rate in the composite hydrogel by regulating the ratio of the SF component to the other two components. Therefore, there are large differences in the initial chemical components, mechanical properties, and cross-linking density of hydrogel materials in different groups, and the initial characteristic equivalence requirements cannot be met. The literature (Journal of Functional Polymers 2024, 37, 312-321) constructed SF hydrogels with different protein conformational transition rates based on the strategy of regulating chemical cross-linking density and using a single SF material component, and examined its effect on the proliferation of cells adhering to the hydrogel surface. Although this scheme eliminates the interference of different chemical compositions to a certain extent, there are still significant differences in the initial average pore size and mechanical properties of hydrogels in different groups (caused by different chemical cross-linking densities).

[0006] In summary, existing strategies cannot achieve the preparation of SF hydrogels with equivalent initial characteristics and different protein conformational transition rates. Summary of the invention

[0007] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing SF hydrogels with initial equivalence and different conformational transition rates.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing SF hydrogels with initial equivalence and different conformational transition rates, comprising mixing SF hydrogel precursor solution α and SF hydrogel precursor solution β in different proportions, and subjecting the mixture to cross-linking reaction for a certain period of time under certain conditions, thereby obtaining SF hydrogels with initial equivalence and different conformational transition rates;

[0010] The SF in the SF hydrogel precursor solution α and the SF hydrogel precursor solution β are the same, and the concentration of SF is the same;

[0011] The SF hydrogel precursor solution α, the SF hydrogel precursor solution β, the certain conditions, and the certain time satisfy: the SF hydrogel formed by the cross-linking reaction of the SF hydrogel precursor solution α under the certain conditions for the certain time and the SF hydrogel formed by the cross-linking reaction of the SF hydrogel precursor solution β under the certain conditions for the certain time have equivalent stress-strain curves (i.e., almost completely the same), equivalent average pore sizes, and different cross-linking point uniformity;

[0012] SF hydrogels with equivalent initial characteristics and different conformational transition rates refer to SF hydrogels with equivalent initial characteristics and different protein conformational transition rates.

[0013] As the preferred technical solution:

[0014] As described above, the preparation method of SF hydrogels with initial equivalence and different conformational transition rates, the SF hydrogel precursor solution α is a SF / HRP / H2O2 system, and the SF hydrogel precursor solution β is a SF / X / SPS system. The core gelation principle of the two is the same, both rely on the formation of an appropriate amount of di-tyrosine bonds to form a chemically cross-linked SF hydrogel, HRP is horseradish peroxidase, H2O2 is hydrogen peroxide, X is Ru or Rf, Ru is ruthenium, Rf is riboflavin, and SPS is sodium persulfate.

[0015] The method for preparing the SF hydrogels with initial equivalent and different conformational transition rates as described above comprises the following specific steps:

[0016] (1) adding HRP solution to SF solution, and then adding H2O2 solution to obtain SF hydrogel precursor solution α, and crosslinking reaction at temperature T for time t to obtain SF hydrogel A;

[0017] (2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0018] (3) adding X solution to SF solution, and then adding SPS solution to obtain multiple SF hydrogel precursor solutions B with different X dosages, and subjecting them to crosslinking reaction for a time t under visible light irradiation with a light intensity L to obtain multiple SF hydrogels B;

[0019] (4) Using an electronic universal testing machine to perform compression testing on SF hydrogel B to obtain the stress-strain curve of SF hydrogel B. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel B and then perform statistics to obtain the average pore size of SF hydrogel B;

[0020] (5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record the corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0021] (6) After mixing SF hydrogel precursor solution α and SF hydrogel precursor solution β in different proportions, the mixture is subjected to crosslinking reaction for a time t under visible light irradiation at a temperature T and a light intensity L, thereby obtaining SF hydrogels with initial equivalent and different conformational transition rates.

[0022] In the method for preparing the SF hydrogel with initial equivalent and different conformational transition rates as described above, in step (1), the volume ratio of the SF solution to the HRP solution is 1 mL:15-50 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.3-1:0.7.

[0023] In the method for preparing SF hydrogels with initial equivalence and different conformational transition rates as described above, in step (1), the concentration of the SF solution is 2-10 wt%, the concentration of the HRP solution is 800-1200 U / mL, the concentration of the H2O2 solution is 0.3-0.7 mol / L, T is 35-39°C, and t is more than 30 min.

[0024] In the method for preparing the SF hydrogel with initial equivalent and different conformational transition rates as described above, in step (3), the volume ratio of the SF solution to the X solution is 1 mL:10-40 μL, and the volume ratio of the X solution to the SPS solution is 1:0.8-1:1.2.

[0025] In the method for preparing the SF hydrogel with initial equivalent and different conformational transition rates as described above, in step (3), the concentration of the SF solution is 2-10 wt %, the concentration of the SPS solution is 0.3-0.7 mol / L, and L is 30-80 mW cm -2 When X is Ru, the concentration of the X solution is 3 to 7 mol / L; when X is Rf, the concentration of the X solution is 0.03 to 0.07 mol / L.

[0026] In the method for preparing SF hydrogels with initial equivalence and different conformational transition rates as described above, in step (6), mixing the SF hydrogel precursor solution α and the SF hydrogel precursor solution β in different proportions means mixing the SF hydrogel precursor solution α and the SF hydrogel precursor solution β in different volume ratios, for example, mixing in a volume ratio of 1:0, 3:1, 1:1, 1:3, or 0:1.

[0027] As described above, the preparation method of SF hydrogels with initial equivalent and different conformational transition rates, the preparation steps of SF in all SF solutions are as follows:

[0028] (a) Degumming;

[0029] The silk is placed in a sodium carbonate solution with a concentration of 2 to 5 wt% and a temperature of 95 to 100° C. and boiled for 20 to 60 minutes, washed with deionized water at least three times, and dried to obtain SF fibers;

[0030] (b) dissolving;

[0031] The SF fiber is placed in a lithium bromide solution having a concentration of 9 to 9.3 mol / L and a temperature of 40 to 60° C. and dissolved for 2 to 4 hours to obtain a SF solution;

[0032] (c) dialysis;

[0033] The SF solution obtained in step (b) is filtered and placed in a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution is ≤4.0 μS / cm;

[0034] (d) freeze drying;

[0035] The dialyzed filtrate is injected into a mold and frozen at -20 to -80°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF.

[0036] Principle of the invention:

[0037] The present invention innovatively proposes to construct SF hydrogels with equivalent initial characteristics and different protein conformational transition rates based on the regulation of chemical crosslinking point uniformity. The core principles involved are as follows: ① When the crosslinking point density is equivalent and the crosslinking point uniformity is different, the initial characteristic parameters such as the overall compressive mechanical properties and average pore size of the SF hydrogel are basically equivalent; ② When the crosslinking point density is equivalent and the crosslinking point uniformity is low, the length of the free chain segment of the SF molecule in the hydrogel is also more uneven. In this case, there are both "very short" free chain segments and "longer" free chain segments. For this reason, those "longer" free chain segments are relatively easy to move freely and trigger the SF molecules to change from the random coil conformation to the β-folded conformation of the lower energy level state faster, thereby accelerating the conformational transition process of the hydrogel; ③ When the crosslinking point density is equivalent and the crosslinking point uniformity is high, the length of the free chain segment of the SF molecule in the hydrogel is also more uniform. The free chain segments are all between the intermediate values, and the length is relatively "shorter". The "shorter" chain segments move slowly freely, which will significantly slow down the conformational transition process of the corresponding hydrogel.

[0038] In summary, it is theoretically feasible to adjust the conformational transition rate of SF hydrogels based on the uniformity of chemical crosslinking points while ensuring the equivalence of the initial characteristics of the hydrogels. However, there are still certain challenges in preparing SF hydrogels with equivalent crosslinking point density but different crosslinking point uniformity.

[0039] To solve this problem, the present invention uses the SF / HRP / H2O2 system and the SF / X / SPS system (specifically the SF / Ru / SPS system or the SF / Rf / SPS system) with similar cross-linking principles to prepare the SF hydrogel material. Specifically, both systems rely on the generation of an appropriate amount of dityrosine bonds to form a chemically cross-linked SF hydrogel, and the reaction conditions are extremely mild, which is conducive to the encapsulation and culture of living cells in the hydrogel. Among them, the SF / HRP / H2O2 system only needs to be incubated at a constant temperature of 37°C (body temperature) to complete the cross-linking gelation, and the SF / X / SPS system only needs to be irradiated with visible light to complete the cross-linking gelation. The schematic diagram of the gelation principle of the SF / HRP / H2O2 and SF / Ru / SPS systems to form SF hydrogels is shown as follows. Figure 1 shown.

[0040] The reasons why the SF / HRP / H2O2 system and the SF / X / SPS system can be used to successfully construct SF hydrogels with similar crosslinking point density but different crosslinking point uniformity are as follows. Both types of crosslinking reaction systems rely on the formation of an appropriate amount of dityrosine bonds to form chemically crosslinked hydrogels. The biggest difference between them is that the molecular weight of HRP (Mw=44000Da) is much larger than that of X. According to molecular dynamics and diffusion theory, in the same medium, small molecules have higher diffusion coefficients and weaker intermolecular forces than large molecules, so they disperse faster and more evenly per unit time. Under similar other conditions, compared with HRP with an "abnormally large" molecular weight, small molecules Ru or Rf are very easy to be evenly dispersed in the raw material system to form a hydrogel crosslinking network with excellent uniformity. The crosslinking points in the hydrogel formed by the SF / X / SPS system are "relatively uniform", while the crosslinking points in the hydrogel formed by the SF / HRP / H2O2 system are relatively "uneven". It can be inferred that at the same cross-linking density, the cross-linking density of the hydrogel formed by the SF / X / SPS system is more uniform and the conformational transition rate is slower than that of the hydrogel formed by the SF / HRP / H2O2 system.

[0041] Beneficial effects:

[0042] The present invention innovatively proposes a regulation strategy based on the uniformity of cross-linking points to construct SF hydrogels with initial equivalence and different conformational transition rates. In addition, the synthesis of the hydrogels is also based on a mild cross-linking reaction, which to a large extent ensures that the hydrogel system is non-toxic and harmless to cells, thereby facilitating the encapsulation and culture of living cells. This strategy not only provides an important material platform for the precise study of the impact of the microenvironment of protein conformational transitions on cell behavior in SF hydrogels, but also provides valuable reference and important guidance for the in-depth and effective regulation of protein conformational transitions in hydrogels and the development of efficient tissue repair hydrogel scaffolds. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Schematic diagram of the gelation principle of SF hydrogel formed by the reaction of SF / HRP / H2O2 and SF / Ru / SPS systems;

[0044] Figure 2 The stress-strain curves of α(SF / HRP / H2O2), β(SF / Ru / SPS) and α:β=1:1 hydrogels of Example 1;

[0045] Figure 3 is the average pore size of the α(SF / HRP / H2O2), β(SF / Ru / SPS) and α:β=1:1 hydrogels of Example 1;

[0046] Figure 4The conformational transitions of α(SF / HRP / H2O2), β(SF / Ru / SPS) and α:β=1:1 hydrogels of Example 1 when incubated for different days in a simulated cell culture environment;

[0047] Figure 5 The proliferation of stem cells in the α(SF / HRP / H2O2) hydrogel encapsulating stem cells at different days of culture;

[0048] Figure 6 The proliferation of stem cells in the α:β=1:1 hydrogel encapsulating stem cells at different days of culture;

[0049] Figure 7 The proliferation of stem cells in the β(SF / Ru / SPS) hydrogel encapsulating stem cells at different days of culture. DETAILED DESCRIPTION

[0050] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0051] The following are the test methods for the relevant performance indicators in each embodiment:

[0052] Conductivity: FG3 conductivity meter is used for testing.

[0053] Example 1

[0054] A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, the specific steps are as follows:

[0055] (1) Preparation of raw materials;

[0056] Silk: extracted from the cocoons of the "Qiufeng Baiyu" variety of silkworms, produced in Jiangsu;

[0057] Sodium carbonate solution: the solvent is deionized water, the concentration is 2wt%, and the temperature is 95°C;

[0058] Deionized water;

[0059] Lithium bromide solution: the solvent is deionized water, the concentration is 9 mol / L, and the temperature is 40°C;

[0060] HRP solution: HRP is horseradish peroxidase (CAS No. 9003-99-0), the solvent is deionized water, and the concentration is 800U / mL;

[0061] H2O2 solution: H2O2 is hydrogen peroxide, the solvent is deionized water, and the concentration is 0.3 mol / L;

[0062] Ru solution: Ru is tris(2,2'-bipyridine)dichlororuthenium(II) hexahydrate, the solvent is deionized water, and the concentration is 3 mol / L;

[0063] SPS solution: SPS is sodium persulfate, the solvent is deionized water, and the concentration is 0.3 mol / L;

[0064] (2) Preparation of SF;

[0065] (2.1) The silk was boiled in a sodium carbonate solution for 20 min, washed three times with deionized water, and dried to obtain SF fibers;

[0066] (2.2) Dissolve the SF fiber in lithium bromide solution for 2 hours to obtain a SF solution;

[0067] (2.3) The SF solution obtained in step (2.2) was filtered and placed into a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution reached 4 μS / cm;

[0068] (2.4) The dialyzed filtrate is injected into a mold and frozen at -20°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF;

[0069] (3) Preparation of SF hydrogels with initial equivalent and different conformational transition rates;

[0070] (3.1) preparing a 2 wt % SF solution (the solvent is deionized water), adding an HRP solution to the SF solution, and then adding an H2O2 solution to obtain an SF hydrogel precursor solution α, and performing a cross-linking reaction at a temperature of 35° C. for 35 min to obtain an SF hydrogel A; wherein the volume ratio of the SF solution to the HRP solution is 1 mL:15 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.3;

[0071] (3.2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0072] (3.3) A 2 wt% SF solution (solvent: deionized water) was prepared, and Ru solution was added to the SF solution, followed by SPS solution, to obtain multiple SF hydrogel precursor solutions B with different Ru dosages. -2The cross-linking reaction was carried out under visible light irradiation for 35 minutes to obtain a plurality of SF hydrogels B; wherein the volume ratio of SF solution to Ru solution was 1 mL:10 μL, and the volume ratio of Ru solution to SPS solution was 1:0.8;

[0073] (3.4) Performing compression test on SF hydrogel B using an electronic universal testing machine to obtain the stress-strain curve of SF hydrogel B. At the same time, taking cross-sectional photos of freeze-dried SF hydrogel B using a scanning electron microscope and performing statistics to obtain the average pore size of SF hydrogel B;

[0074] (3.5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record its corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0075] (3.6) SF hydrogel precursor solution α and SF hydrogel precursor solution β were mixed at a volume ratio of 1:0, 3:1, 1:1, 1:3, and 0:1, and then heated at a temperature of 35 °C and a light intensity of 30 mW cm -2 The cross-linking reaction was carried out under visible light irradiation for 35 minutes to obtain SF hydrogels with initial equivalent and different conformational transition rates, which were recorded as α(SF / HRP / H2O2) hydrogel, α:β=3:1 hydrogel, α:β=1:1 hydrogel, α:β=1:3 hydrogel, and β(SF / Ru / SPS) hydrogel. The α(SF / HRP / H2O2) hydrogel, α:β=1:1 hydrogel, and β(SF / Ru / SPS) hydrogel were tested to verify that the three had equivalent initial characteristics and different protein conformational transition rates, as follows:

[0076] The α(SF / HRP / H2O2) hydrogel, α:β=1:1 hydrogel, and β(SF / Ru / SPS) hydrogel were tested respectively. The initial characteristics of the three hydrogels are as follows: Figure 2 , Figure 3 As shown, it can be seen that the three hydrogels have equivalent initial characteristics;

[0077] The three hydrogels were immersed in DMEM complete culture medium and incubated in a cell culture incubator at 37°C, 95% relative humidity, and 5% CO2 volume concentration for 10 days. The medium was changed every two days. The β-fold conformation contents of the three hydrogels on different days were as follows: Figure 4 As shown in the figure, it can be seen that the conformational transition of α(SF / HRP / H2O2) hydrogel in the simulated cell culture environment is the fastest, the conformational transition of β(SF / Ru / SPS) hydrogel is the slowest, and the conformational transition speed of α:β=1:1 hydrogel is between the two. It can be seen that the three hydrogels have different protein conformational transition rates.

[0078] In summary, the hydrogel with the fastest conformational transition can be constructed by a separate SF / HRP / H2O2 system, the hydrogel with the slowest conformational transition can be constructed by a separate SF / Ru / SPS system, and the SF hydrogel with an intermediate conformational transition can be constructed by regulating the volume ratio of these two systems with similar gelation principles.

[0079] In addition, since both systems are gelled under extremely mild (cell-friendly) conditions, the combination of the two systems is also gelled under mild conditions. Therefore, the hydrogel formation process is non-toxic and harmless to cells, which is conducive to the encapsulation of living cells and the subsequent three-dimensional cell culture and comprehensive investigation of cell behavior. To confirm this view, the following experiments are conducted:

[0080] The α(SF / HRP / H2O2) hydrogel encapsulating stem cells, the α:β=1:1 hydrogel encapsulating stem cells, and the β(SF / Ru / SPS) hydrogel encapsulating stem cells were prepared respectively, wherein:

[0081] The preparation process of α(SF / HRP / H2O2) hydrogel encapsulating stem cells is basically the same as that of α(SF / HRP / H2O2) hydrogel, except that before adding HRP solution to SF solution, an equal volume of bone marrow mesenchymal stem cell suspension is added to SF solution, and the number of stem cells in the suspension is 10×10 5 cells / mL;

[0082] The preparation process of the α:β=1:1 hydrogel encapsulating stem cells is basically the same as that of the α:β=1:1 hydrogel, except that when the SF hydrogel precursor solution α and the SF hydrogel precursor solution β are mixed, a bone marrow mesenchymal stem cell suspension of the same volume as the SF solution is also added, and the number of stem cells in the suspension is 10×10 5 cells / mL;

[0083] The preparation process of β(SF / Ru / SPS) hydrogel encapsulating stem cells is basically the same as that of β(SF / Ru / SPS) hydrogel, except that before adding Ru solution to SF solution, an equal volume of bone marrow mesenchymal stem cell suspension is added to SF solution, and the number of stem cells in the suspension is 10×10 5 cells / mL;

[0084] The stem cell-encapsulated α(SF / HRP / H2O2) hydrogel, stem cell-encapsulated α:β=1:1 hydrogel, and stem cell-encapsulated β(SF / Ru / SPS) hydrogel were immersed in DMEM complete medium and incubated in a cell culture incubator at 37°C, 95% relative humidity, and 5% CO2 volume concentration for 10 days, with the medium changed every two days. Figure 5 to Figure 7 It can be seen that after long-term culture, the total cell activity of the cells inside the three hydrogels gradually increased (indirectly indicating that the number of cells gradually increased), and obvious cell proliferation occurred.

[0085] Therefore, SF hydrogels with equivalent compressive mechanical properties and average pore size can be successfully constructed by using SF / HRP / H2O2 and SF / Ru / SPS systems alone, or based on the composite of the two systems. These hydrogels show good biocompatibility in cell culture, providing a powerful tool for exploring the impact of protein conformational transitions on cell behavior.

[0086] Example 2

[0087] A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, the specific steps are as follows:

[0088] (1) Preparation of raw materials;

[0089] Silk: extracted from the cocoons of the "Qiufeng Baiyu" variety of silkworms, produced in Jiangsu;

[0090] Sodium carbonate solution: the solvent is deionized water, the concentration is 2wt%, and the temperature is 95°C;

[0091] Deionized water;

[0092] Lithium bromide solution: the solvent is deionized water, the concentration is 9 mol / L, and the temperature is 40°C;

[0093] HRP solution: HRP is horseradish peroxidase (CAS No. 9003-99-0), the solvent is deionized water, and the concentration is 900U / mL;

[0094] H2O2 solution: H2O2 is hydrogen peroxide, the solvent is deionized water, and the concentration is 0.4 mol / L;

[0095] Ru solution: Ru is tris(2,2'-bipyridine)dichlororuthenium(II) hexahydrate, the solvent is deionized water, and the concentration is 5 mol / L;

[0096] SPS solution: SPS is sodium persulfate, the solvent is deionized water, and the concentration is 0.4 mol / L;

[0097] (2) Preparation of SF;

[0098] (2.1) The silk was boiled in a sodium carbonate solution for 30 min, washed four times with deionized water, and dried to obtain SF fibers;

[0099] (2.2) Dissolve the SF fiber in lithium bromide solution for 2 hours to obtain a SF solution;

[0100] (2.3) The SF solution obtained in step (2.2) was filtered and placed into a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution reached 3 μS / cm;

[0101] (2.4) The dialyzed filtrate is injected into a mold and frozen at -30°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF;

[0102] (3) Preparation of SF hydrogels with initial equivalent and different conformational transition rates;

[0103] (3.1) preparing a 4 wt % SF solution (the solvent is deionized water), adding an HRP solution to the SF solution, and then adding an H2O2 solution to obtain an SF hydrogel precursor solution α, and performing a cross-linking reaction at a temperature of 36° C. for 40 min to obtain an SF hydrogel A; wherein the volume ratio of the SF solution to the HRP solution is 1 mL:15 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.3;

[0104] (3.2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0105] (3.3) A 4 wt% SF solution (solvent: deionized water) was prepared, and Ru solution was added to the SF solution, followed by SPS solution, to obtain multiple SF hydrogel precursor solutions B with different Ru dosages. -2 The cross-linking reaction was carried out under visible light irradiation for 40 minutes to obtain a plurality of SF hydrogels B; wherein the volume ratio of SF solution to Ru solution was 1 mL:10 μL, and the volume ratio of Ru solution to SPS solution was 1:0.8;

[0106] (3.4) Performing compression test on SF hydrogel B using an electronic universal testing machine to obtain the stress-strain curve of SF hydrogel B. At the same time, taking cross-sectional photos of freeze-dried SF hydrogel B using a scanning electron microscope and performing statistics to obtain the average pore size of SF hydrogel B;

[0107] (3.5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record its corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0108] (3.6) SF hydrogel precursor solution α and SF hydrogel precursor solution β were mixed at a volume ratio of 1:0, 3:1, 1:1, 1:3, and 0:1, and then heated at a temperature of 36 °C and a light intensity of 40 mW cm -2 The cross-linking reaction was carried out under visible light irradiation for 40 minutes to obtain SF hydrogels with initial equivalent but different conformational transition rates.

[0109] Example 3

[0110] A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, the specific steps are as follows:

[0111] (1) Preparation of raw materials;

[0112] Silk: extracted from the cocoons of the "Qiufeng Baiyu" variety of silkworms, produced in Jiangsu;

[0113] Sodium carbonate solution: the solvent is deionized water, the concentration is 3wt%, and the temperature is 98°C;

[0114] Deionized water;

[0115] Lithium bromide solution: the solvent is deionized water, the concentration is 9.3 mol / L, and the temperature is 50°C;

[0116] HRP solution: HRP is horseradish peroxidase (CAS No. 9003-99-0), the solvent is deionized water, and the concentration is 1000U / mL;

[0117] H2O2 solution: H2O2 is hydrogen peroxide, the solvent is deionized water, and the concentration is 0.5 mol / L;

[0118] Ru solution: Ru is tris(2,2'-bipyridine)dichlororuthenium(II) hexahydrate, the solvent is deionized water, and the concentration is 7 mol / L;

[0119] SPS solution: SPS is sodium persulfate, the solvent is deionized water, and the concentration is 0.5 mol / L;

[0120] (2) Preparation of SF;

[0121] (2.1) The silk was boiled in a sodium carbonate solution for 40 min, washed four times with deionized water, and dried to obtain SF fibers;

[0122] (2.2) Dissolve the SF fiber in lithium bromide solution for 3 hours to obtain a SF solution;

[0123] (2.3) The SF solution obtained in step (2.2) was filtered and placed into a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution reached 3 μS / cm;

[0124] (2.4) The dialyzed filtrate is injected into a mold and frozen at -50°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF;

[0125] (3) Preparation of SF hydrogels with initial equivalent and different conformational transition rates;

[0126] (3.1) preparing a 6 wt % SF solution (the solvent is deionized water), adding an HRP solution to the SF solution, and then adding an H2O2 solution to obtain an SF hydrogel precursor solution α, and performing a cross-linking reaction at 37° C. for 45 min to obtain an SF hydrogel A; wherein the volume ratio of the SF solution to the HRP solution is 1 mL:50 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.7;

[0127] (3.2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0128] (3.3) A 6 wt% SF solution (solvent: deionized water) was prepared, and Ru solution was added to the SF solution, followed by SPS solution, to obtain multiple SF hydrogel precursor solutions B with different Ru dosages. -2 The cross-linking reaction was carried out under visible light irradiation for 45 minutes to obtain a plurality of SF hydrogels B; wherein the volume ratio of SF solution to Ru solution was 1 mL:40 μL, and the volume ratio of Ru solution to SPS solution was 1:1.2;

[0129] (3.4) Performing compression test on SF hydrogel B using an electronic universal testing machine to obtain the stress-strain curve of SF hydrogel B. At the same time, taking cross-sectional photos of freeze-dried SF hydrogel B using a scanning electron microscope and performing statistics to obtain the average pore size of SF hydrogel B;

[0130] (3.5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record its corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0131] (3.6) SF hydrogel precursor solution α and SF hydrogel precursor solution β were mixed at a volume ratio of 1:0, 3:1, 1:1, 1:3, and 0:1, and then heated at a temperature of 37 °C and a light intensity of 60 mW cm -2 The cross-linking reaction was carried out under visible light irradiation for 45 minutes to obtain SF hydrogels with initial equivalent but different conformational transition rates.

[0132] Example 4

[0133] A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, the specific steps are as follows:

[0134] (1) Preparation of raw materials;

[0135] Silk: extracted from the cocoons of the "Qiufeng Baiyu" variety of silkworms, produced in Jiangsu;

[0136] Sodium carbonate solution: the solvent is deionized water, the concentration is 4wt%, and the temperature is 100°C;

[0137] Deionized water;

[0138] Lithium bromide solution: the solvent is deionized water, the concentration is 9 mol / L, and the temperature is 60°C;

[0139] HRP solution: HRP is horseradish peroxidase (CAS No. 9003-99-0), the solvent is deionized water, and the concentration is 1100U / mL;

[0140] H2O2 solution: H2O2 is hydrogen peroxide, the solvent is deionized water, and the concentration is 0.6 mol / L;

[0141] Rf solution: Rf is riboflavin, the solvent is deionized water, and the concentration is 0.03 mol / L;

[0142] SPS solution: SPS is sodium persulfate, the solvent is deionized water, and the concentration is 0.6 mol / L;

[0143] (2) Preparation of SF;

[0144] (2.1) The silk was boiled in a sodium carbonate solution for 50 min, washed with deionized water 5 times, and dried to obtain SF fibers;

[0145] (2.2) Dissolving the SF fiber in a lithium bromide solution for 4 hours to obtain a SF solution;

[0146] (2.3) The SF solution obtained in step (2.2) was filtered and placed into a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution reached 2 μS / cm;

[0147] (2.4) The dialyzed filtrate is injected into a mold and frozen at -70°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF;

[0148] (3) Preparation of SF hydrogels with initial equivalent and different conformational transition rates;

[0149] (3.1) preparing an SF solution with a concentration of 8 wt % (the solvent is deionized water), adding an HRP solution to the SF solution, and then adding an H2O2 solution to obtain an SF hydrogel precursor solution α, and performing a cross-linking reaction at a temperature of 38° C. for 50 min to obtain an SF hydrogel A; wherein the volume ratio of the SF solution to the HRP solution is 1 mL:50 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.7;

[0150] (3.2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0151] (3.3) Prepare SF solution with a concentration of 8 wt % (solvent is deionized water), add Rf solution to the SF solution, and then add SPS solution to obtain multiple SF hydrogel precursor solutions B with different Rf dosages. -2 The cross-linking reaction was carried out under visible light irradiation for 50 minutes to obtain a plurality of SF hydrogels B; wherein the volume ratio of SF solution to Rf solution was 1 mL:40 μL, and the volume ratio of Rf solution to SPS solution was 1:1.2;

[0152] (3.4) Performing compression test on SF hydrogel B using an electronic universal testing machine to obtain the stress-strain curve of SF hydrogel B. At the same time, taking cross-sectional photos of freeze-dried SF hydrogel B using a scanning electron microscope and performing statistics to obtain the average pore size of SF hydrogel B;

[0153] (3.5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record its corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0154] (3.6) SF hydrogel precursor solution α and SF hydrogel precursor solution β were mixed at a volume ratio of 1:0, 3:1, 1:1, 1:3, and 0:1, and then heated at a temperature of 38 °C and a light intensity of 70 mW cm -2 The cross-linking reaction was carried out under visible light irradiation for 50 min to obtain SF hydrogels with initial equivalent but different conformational transition rates.

[0155] Example 5

[0156] A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, the specific steps are as follows:

[0157] (1) Preparation of raw materials;

[0158] Silk: extracted from the cocoons of the "Qiufeng Baiyu" variety of silkworms, produced in Jiangsu;

[0159] Sodium carbonate solution: the solvent is deionized water, the concentration is 4wt%, and the temperature is 100°C;

[0160] Deionized water;

[0161] Lithium bromide solution: the solvent is deionized water, the concentration is 9.3 mol / L, and the temperature is 60°C;

[0162] HRP solution: HRP is horseradish peroxidase (CAS No. 9003-99-0), the solvent is deionized water, and the concentration is 1200U / mL;

[0163] H2O2 solution: H2O2 is hydrogen peroxide, the solvent is deionized water, and the concentration is 0.7 mol / L;

[0164] Rf solution: Rf is riboflavin, the solvent is deionized water, and the concentration is 0.07 mol / L;

[0165] SPS solution: SPS is sodium persulfate, the solvent is deionized water, and the concentration is 0.7 mol / L;

[0166] (2) Preparation of SF;

[0167] (2.1) The silk was boiled in a sodium carbonate solution for 60 min, washed with deionized water 5 times, and dried to obtain SF fibers;

[0168] (2.2) Dissolving the SF fiber in a lithium bromide solution for 4 hours to obtain a SF solution;

[0169] (2.3) The SF solution obtained in step (2.2) was filtered and placed into a dialysis bag, and dialyzed with deionized water, with the deionized water being changed three times a day until the conductivity of the SF solution reached 2 μS / cm;

[0170] (2.4) The dialyzed filtrate is injected into a mold and frozen at -80°C. The frozen body is then placed in a freeze dryer for freeze drying to obtain SF;

[0171] (3) Preparation of SF hydrogels with initial equivalent and different conformational transition rates;

[0172] (3.1) preparing a 10 wt% SF solution (the solvent is deionized water), adding an HRP solution to the SF solution, and then adding an H2O2 solution to obtain an SF hydrogel precursor solution α, and performing a cross-linking reaction at a temperature of 39°C for 50 min to obtain an SF hydrogel A; wherein the volume ratio of the SF solution to the HRP solution is 1 mL:50 μL, and the volume ratio of the HRP solution to the H2O2 solution is 1:0.7;

[0173] (3.2) Using an electronic universal testing machine to perform compression testing on SF hydrogel A to obtain the stress-strain curve of SF hydrogel A. At the same time, using a scanning electron microscope to take cross-sectional photos of freeze-dried SF hydrogel A and then perform statistics to obtain the average pore size of SF hydrogel A;

[0174] (3.3) A 10 wt% SF solution (solvent: deionized water) was prepared, Rf solution was added to the SF solution, and then SPS solution was added to obtain multiple SF hydrogel precursor solutions B with different Rf dosages. -2 The cross-linking reaction was carried out under visible light irradiation for 50 minutes to obtain a plurality of SF hydrogels B; wherein the volume ratio of SF solution to Rf solution was 1 mL:40 μL, and the volume ratio of Rf solution to SPS solution was 1:1.2;

[0175] (3.4) Performing compression test on SF hydrogel B using an electronic universal testing machine to obtain the stress-strain curve of SF hydrogel B. At the same time, taking cross-sectional photos of freeze-dried SF hydrogel B using a scanning electron microscope and performing statistics to obtain the average pore size of SF hydrogel B;

[0176] (3.5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record its corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β;

[0177] (3.6) SF hydrogel precursor solution α and SF hydrogel precursor solution β were mixed at a volume ratio of 1:0, 3:1, 1:1, 1:3, and 0:1, and then heated at a temperature of 39 °C and a light intensity of 80 mW cm -2 The cross-linking reaction was carried out under visible light irradiation for 50 min to obtain SF hydrogels with initial equivalent but different conformational transition rates.

Claims

1. A method for preparing SF hydrogels with initial equivalent and different conformational transition rates, characterized in that: After SF hydrogel precursor solution α and SF hydrogel precursor solution β are mixed in different proportions, cross-linking reaction is carried out under certain conditions for a certain time to obtain SF hydrogels with initial equivalent and different conformational transition rates; The SF in the SF hydrogel precursor solution α and the SF hydrogel precursor solution β are the same, and the concentration of SF is the same; The SF hydrogel precursor solution α, the SF hydrogel precursor solution β, the certain conditions, and the certain time satisfy: the SF hydrogel formed by the cross-linking reaction of the SF hydrogel precursor solution α under the certain conditions for the certain time and the SF hydrogel formed by the cross-linking reaction of the SF hydrogel precursor solution β under the certain conditions for the certain time have equivalent stress-strain curves, equivalent average pore sizes, and different cross-linking point uniformity; SF hydrogels with equivalent initial characteristics and different conformational transition rates refer to SF hydrogels with equivalent initial characteristics and different protein conformational transition rates.

2. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 1, characterized in that: The SF hydrogel precursor solution α is a SF / HRP / H2O2 system, the SF hydrogel precursor solution β is a SF / X / SPS system, HRP is horseradish peroxidase, H2O2 is hydrogen peroxide, X is Ru or Rf, Ru is ruthenium, Rf is riboflavin, and SPS is sodium persulfate.

3. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 2, characterized in that: The specific steps are as follows: (1) adding HRP solution to SF solution, and then adding H2O2 solution to obtain SF hydrogel precursor solution α, and crosslinking reaction at temperature T for time t to obtain SF hydrogel A; (2) obtaining the stress-strain curve of SF hydrogel A and, at the same time, obtaining the average pore size of SF hydrogel A; (3) adding X solution to SF solution, and then adding SPS solution to obtain multiple SF hydrogel precursor solutions B with different X dosages, and subjecting them to crosslinking reaction for a time t under visible light irradiation with a light intensity L to obtain multiple SF hydrogels B; (4) obtaining the stress-strain curve of SF hydrogel B and the average pore size of SF hydrogel B; (5) Find SF hydrogel B with equivalent stress-strain curve and average pore size to SF hydrogel A, and record the corresponding SF hydrogel precursor solution B as SF hydrogel precursor solution β; (6) After mixing SF hydrogel precursor solution α and SF hydrogel precursor solution β in different proportions, the mixture is subjected to crosslinking reaction for a time t under visible light irradiation at a temperature T and a light intensity L, thereby obtaining SF hydrogels with initial equivalent and different conformational transition rates.

4. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 3, characterized in that: In step (1), the volume ratio of SF solution to HRP solution is 1 mL:15-50 μL, and the volume ratio of HRP solution to H2O2 solution is 1:0.3-0.

7.

5. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 3, characterized in that: In step (1), the concentration of SF solution is 2-10 wt %, the concentration of HRP solution is 800-1200 U / mL, the concentration of H2O2 solution is 0.3-0.7 mol / L, T is 35-39° C., and t is more than 30 min.

6. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 3, characterized in that: In step (3), the volume ratio of SF solution to X solution is 1 mL:10-40 μL, and the volume ratio of X solution to SPS solution is 1:0.8-1.

2.

7. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 3, characterized in that: In step (3), the concentration of the SF solution is 2-10 wt%, the concentration of the SPS solution is 0.3-0.7 mol / L, and L is 30-80 mW cm -2 When X is Ru, the concentration of the X solution is 3 to 7 mol / L; when X is Rf, the concentration of the X solution is 0.03 to 0.07 mol / L.

8. The method for preparing SF hydrogels with initial equivalent and different conformational transition rates according to claim 3, characterized in that: In step (6), mixing the SF hydrogel precursor solution α and the SF hydrogel precursor solution β in different proportions means mixing the SF hydrogel precursor solution α and the SF hydrogel precursor solution β in different volume ratios.

Citation Information

Patent Citations

  • Ultrasonic-mediated silk fibroin composite collagen hydrogel and preparation method thereof

    CN110698866A

  • Mechanically enhanced gelatin chilled hydrogel as well as preparation method and application thereof

    CN112759774A

  • Preparation method of macroporous silk fibroin hydrogel

    CN114716726A

  • Silk / Li < + > conductive hydrogel pressure sensor and construction method and application thereof

    CN115232478A

  • High-strength and high-toughness silk fibroin self-reinforced hydrogel and preparation method thereof

    CN118027686A