A method for preparing lithium sulfide, sulfide solid electrolyte and all-solid-state battery

Lithium sulfide was prepared by heating ball milling method of lithium source precursor and solid carbon source under the atmosphere of dopamine hydrochloride and carbon monoxide inert gas, which solved the problem of many by-products and low conversion in the preparation of lithium sulfide, and achieved high purity, High yields of lithium sulfide preparation reduce costs.

CN116969422BActive Publication Date: 2024-12-06WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310964431.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-31
Publication Date
2024-12-06
Estimated Expiration
2043-07-31

AI Technical Summary

Technical Problem

In the prior art, the by-product content and low conversion rate during the preparation process of lithium sulfide, resulting in low purity and yield of lithium sulfide and high cost.

Method used

Lithium sulfide is prepared by mixing the lithium source precursor with a solid carbon source and heating it under an atmosphere of dopamine hydrochloride and carbon monoxide inert gas. Conversion and purity are improved and by-product generation is reduced.

Benefits of technology

It significantly improves the conversion rate of lithium sulfide to more than 99%, reduces the by-product content, improves the yield and purity, and is safe and simple in process, low in cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004372963310000121
    Figure BDA0004372963310000121
  • Figure HDA0004372963330000011
    Figure HDA0004372963330000011
Patent Text Reader

Abstract

The present application relates to a method for preparing lithium sulfide, a sulfide solid electrolyte and an all-solid-state battery. The method for preparing lithium sulfide provided in the present application comprises the following steps: mixing a lithium source precursor and a solid carbon source, adding a solvent and dopamine hydrochloride, ball milling, then heating and drying to obtain a solid mixture; heating the solid mixture in a mixed atmosphere of carbon monoxide and an inert gas, and then cooling to obtain lithium sulfide. The method provided in the present application simultaneously utilizes a solid carbon source and carbon monoxide gas as a reducing agent. During the reduction process, the carbon monoxide gas is wrapped around the outer surface of the lithium source precursor, which can reduce the production of byproducts Li2O, Li2CO3, etc. The content of the byproduct Li2O in the obtained product is 0.2%-0.4%, and the content of the byproduct Li2CO3 is 0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of solid electrolyte technology, and in particular to a method for preparing lithium sulfide, a sulfide solid electrolyte and an all-solid-state battery. Background Art

[0002] The demand for high energy density and high safety lithium batteries as a power source for electronics and electric vehicles is growing. However, the most advanced lithium-ion batteries have encountered a bottleneck in further improving the energy density. This requires innovation in battery chemistry beyond lithium-ion batteries. Since metallic lithium has the highest theoretical capacity (3860mA·h·g -1 ) and the lowest electrochemical potential (-3.04V relative to hydrogen electrode). When it is matched with a high-capacity positive electrode, it is expected to obtain a specific density of about 2 to 5 times. Therefore, metallic lithium as a negative electrode of the battery has aroused widespread research interest. However, the growth of metallic lithium dendrites is prone to occur at the lithium negative electrode during the battery cycle. The penetration of lithium dendrites through the diaphragm will cause a short circuit between the positive and negative electrodes of the battery, thereby generating a strong exothermic reaction, rapidly heating the battery and causing thermal runaway. Liquid electrolytes are highly flammable and may have side reactions with metallic lithium. Therefore, solid electrolytes with high modulus have important prospects in solving the problem of lithium batteries with metallic lithium as the negative electrode.

[0003] Solid electrolyte materials usually use polymers, oxides or sulfides. Among them, sulfide solid electrolytes have the highest ionic conductivity, which can reach 10 -2 S / cm. In addition, sulfide solid electrolytes generally have good mechanical properties, are easy to process, and can form good interface contact with electrodes at room temperature. Lithium sulfide is a key raw material for sulfide solid electrolytes. Lithium sulfide is usually obtained by reduction using lithium compounds. For example, patent CN112678780A discloses a method for preparing high-purity lithium sulfide, using a lithium sulfide precursor (one or more of lithium sulfate, lithium sulfite, lithium bisulfate, and lithium dithionate) and a sugar reducing agent to react at high temperature to prepare a substance containing lithium sulfide, and then the lithium sulfide in the mixture is leached and purified, and finally a lithium sulfide product with controllable morphology is obtained by spray drying. However, a mixture of lithium sulfate will be obtained during the reaction preparation process, and further leaching, filtering and drying are required, and the cost of preparing lithium sulfide is relatively high. Patent CN113401878A discloses a method for preparing lithium sulfide, which reacts carbon monoxide with powdered anhydrous lithium sulfate to obtain lithium sulfide. However, this technology only uses gas to reduce lithium sulfate, and the reaction mainly takes place at the gas-solid interface. The reaction rate is slow, and the product easily wraps the raw material lithium sulfate. The conversion rate of the reaction is low, and it is difficult to obtain a high-yield lithium sulfide solid product. Summary of the invention

[0004] The embodiment of the present application provides a method for preparing lithium sulfide to solve the problems of high by-product content and low conversion rate when preparing lithium sulfide in the related art.

[0005] In a first aspect, the present application provides a method for preparing lithium sulfide, comprising the following steps:

[0006] S101, mixing a lithium source precursor and a solid carbon source, adding a solvent and dopamine hydrochloride, ball milling, and then heating and drying to obtain a solid mixture;

[0007] S102, heating the solid mixture in a mixed atmosphere of carbon monoxide and inert gas, and then cooling it to obtain lithium sulfide.

[0008] In some embodiments, the lithium source precursor is any one of lithium sulfate, lithium carbonate, lithium sulfite, and lithium hydroxide.

[0009] In some preferred embodiments, the lithium source precursor is lithium sulfate with a particle size of 10 μm to 100 μm.

[0010] In some preferred embodiments, the lithium source precursor is lithium sulfate with a particle size of 10 μm to 50 μm.

[0011] In some embodiments, the solid carbon source is a mixture of any one or more of graphene, carbon black, carbon nanotubes, activated carbon, petroleum coke or polymer compounds.

[0012] In some embodiments, the solvent is any one of ethanol, methanol, and butanol.

[0013] In some embodiments, the polymer compound is any one of glucose, sucrose, fructose, and maltose.

[0014] In some embodiments, the inert gas is any one of nitrogen, argon, and carbon dioxide.

[0015] In some embodiments, the volume of carbon monoxide accounts for 10% to 80% of the total volume of carbon monoxide and inert gas. When carbon monoxide is not used as a reducing gas or the volume of carbon monoxide is not within the range of 10% to 80% of the total volume of carbon monoxide and inert gas, the conversion rate of lithium sulfide is significantly reduced, the content of byproducts Li2O and Li2CO3 increases, the purity of the product lithium sulfide is reduced, and the particle size of the product lithium sulfide is also affected.

[0016] In some embodiments, the lithium source precursor and the solid carbon source are mixed in a molar ratio of lithium element to carbon element of 1:4 to 1:12.

[0017] In some preferred embodiments, the lithium source precursor and the solid carbon source are mixed in a molar ratio of lithium element to carbon element of 1:4 to 1:8.

[0018] In some embodiments, the amount of dopamine hydrochloride added is 0.2% to 0.5% of the mass of the solid carbon source.

[0019] In some embodiments, the purity of the lithium sulfide obtained in step S102 is greater than 99%, wherein the impurity ions Ca are less than 50 ppm, Mg are less than 80 ppm, Na are less than 250 ppm, and K are less than 50 ppm.

[0020] In some embodiments, in step S101, the heating temperature is 25-60°C; in step S102, the heating temperature is 750°C-1000°C.

[0021] In some preferred embodiments, the heating temperature is 850°C to 950°C. In the temperature range below 700°C, the reaction rate of the lithium source precursor and the solid carbon source is slow and the productivity is low. In the temperature range above 950°C, the temperature is higher than the melting point of the raw lithium salt precursor, especially lithium sulfate, so the unreacted lithium salt precursor melts. In the temperature range above 850°C and below 950°C, the lithium salt precursor, especially lithium sulfate, does not melt, and lithium sulfide can be obtained while maintaining the particle shape. At high temperatures of 850 to 950°C, carbon monoxide gas will react with lithium sulfate solid. If the carbon monoxide concentration is less than 10%, lithium oxide is generated as a by-product of the reduction reaction. When the carbon monoxide concentration is above 80%, some by-product lithium carbonate is generated.

[0022] In some embodiments, in step S102 , the temperature is cooled to below 200° C., and the cooling process is performed naturally in an inert gas atmosphere.

[0023] In a second aspect, the present application provides a sulfide solid electrolyte, wherein the sulfide solid electrolyte comprises the lithium sulfide prepared as described above.

[0024] In a third aspect, the present application provides a method for preparing a sulfide solid electrolyte, comprising the following steps: mixing the lithium sulfide and phosphorus sulfide prepared above, ball milling, and obtaining a solid electrolyte having an ionic conductivity of not less than 0.5×10 -3 ms / cm sulfide solid electrolyte.

[0025] In some embodiments, the ionic conductivity of the sulfide solid electrolyte is 1×10 -3 ms / cm.

[0026] In some embodiments, the thickness of the sulfide solid electrolyte membrane is 1 μm to 1000 μm.

[0027] In some preferred embodiments, the thickness of the sulfide solid electrolyte membrane is 10 μm to 100 μm. In terms of ionic conductivity and energy density, the smaller the thickness, the higher the ionic conductivity and energy density, and the thickness generally needs to be less than 100 μm; on the other hand, in terms of physical strength, the higher the thickness, the greater the strength, and the thickness generally needs to be greater than 10 μm.

[0028] In a fourth aspect, the present application also provides an all-solid-state battery comprising the above-mentioned sulfide solid electrolyte.

[0029] The beneficial effects of the technical solution provided by this application include:

[0030] 1. The method provided in the present application, on the one hand, adds dopamine hydrochloride during the mixing process of the lithium source precursor and the solid carbon source. One end of the dopamine hydrochloride is chelated with the lithium source precursor, and the other end is chelated with the solid carbon source, playing the role of an intermediate bridge, effectively improving the encapsulation of the solid carbon source and the lithium source precursor; on the other hand, the solid carbon source and carbon monoxide gas are used as reducing agents at the same time. During the reduction process, the carbon monoxide gas is wrapped on the outer surface of the lithium source precursor, which can reduce the generation of by-products such as Li2O and Li2CO3. In the final product, the content of the by-product Li2O is 0.2%-0.4%, and the content of the by-product Li2CO3 is 0, and the conversion rate of lithium sulfide is increased from 80% to more than 99%, effectively improving the yield and purity of lithium sulfide;

[0031] 2. The method provided in the present application ball-mills the lithium source precursor to obtain solid particles with a relatively low particle size (~10 μm), making it easier to prepare fine-particle sulfide solid electrolytes;

[0032] 3. The present application adopts a lithium sulfate carbonization reduction method to prepare lithium sulfide, which is safe, simple, and low-cost. The obtained high-purity lithium sulfide product has stable and reliable quality, which is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 A schematic flow chart of a method for preparing lithium sulfide provided in an embodiment of the present application. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0036] The embodiment of the present application provides a method for preparing lithium sulfide, which can solve the problems of high by-product content and low conversion rate when preparing lithium sulfide in the prior art.

[0037] refer to Figure 1 The present invention provides a method for preparing lithium sulfide, comprising the following steps:

[0038] Step S101, mixing a lithium source precursor and a solid carbon source, adding a solvent and dopamine hydrochloride, and then ball milling, then heating to 25-60° C., and spray drying to obtain a solid mixture; the amount of dopamine hydrochloride added is 0.2%-0.5% of the mass of the solid carbon source;

[0039] Step S102, heating the solid mixture in an atmosphere of carbon monoxide and an inert gas, and then naturally cooling it to below 200° C. in an inert gas atmosphere to obtain lithium sulfide.

[0040] The reaction formula involved in the above-mentioned lithium sulfide preparation process is:

[0041] Li2SO4+4C→Li2S+4CO

[0042] Li2SO4+4CO→Li2S+4CO2

[0043] The preparation method of lithium sulfide provided in the present application is described in detail below with reference to the embodiments and comparative examples.

[0044] Embodiment 1:

[0045] Embodiment 1 provides a method for preparing lithium sulfide, comprising the following steps:

[0046] (1) lithium sulfate (particle size 20 μm) and glucose were weighed in a molar ratio of Li2SO4:C=1:2.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.4% of the mass of glucose) were added, mixed using a ball mill, heated to 35° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0047] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace. A mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 10% of the total volume of carbon monoxide and argon. The temperature of the tubular furnace is raised to 900°C and maintained at 900°C for 2 hours. Thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 8 μm and a conversion rate of 99.5%.

[0048] The high-purity lithium sulfide powder obtained in Example 1 was tested: the purity of the lithium sulfide powder was 99.90%, the residual amount of Li2SO4 was 0.007%, the content of by-product Li2O was 0.3%, the content of Li2CO3 was 0, the impurity ions Ca were less than 50ppm, Mg were less than 80ppm, Na were less than 250ppm, and K were less than 50ppm.

[0049] The lithium sulfide powder prepared in Example 1 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 2.7×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0050] Embodiment 2:

[0051] Embodiment 2 provides a method for preparing lithium sulfide, comprising the following steps:

[0052] (1) lithium sulfate (particle size 35 μm) and petroleum coke were weighed in a molar ratio of Li2SO4:C=1:2.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.25% of the mass of petroleum coke) were added, mixed using a ball mill, heated to 40° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0053] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace; then, a mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 80% of the total volume of carbon monoxide and argon, and the temperature of the tubular furnace is raised to 850°C and maintained at 850°C for 2 hours; thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 13 μm and a conversion rate of 99.2%.

[0054] The high-purity lithium sulfide powder obtained in Example 2 was tested: the purity of the lithium sulfide powder was 99.91%, the residual amount of Li2SO4 was 0.009%, the content of by-product Li2O was 0.4%, the content of Li2CO3 was 0, the impurity ions Ca were less than 50ppm, Mg were less than 80ppm, Na were less than 250ppm, and K were less than 50ppm.

[0055] The lithium sulfide powder prepared in Example 2 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 1.8×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0056] Embodiment 3:

[0057] Embodiment 3 provides a method for preparing lithium sulfide, comprising the following steps:

[0058] (1) lithium sulfate (particle size 30 μm) and sucrose were weighed in a molar ratio of Li2SO4:C=1:2.5, ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.3% of the mass of sucrose) were added, mixed using a ball mill, heated to 55° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0059] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace. Then, a mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 50% of the total volume of carbon monoxide and argon. The temperature of the tubular furnace is raised to 900°C and maintained at 900°C for 2 hours. Thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 11 μm and a conversion rate of 99.4%.

[0060] The high-purity lithium sulfide powder obtained in Example 3 was tested: the purity of the lithium sulfide powder was 99.91%, the residual amount of Li2SO4 was 0.005%, the content of by-product Li2O was 0.2%, the content of Li2CO3 was 0, the impurity ions Ca were less than 50ppm, Mg were less than 80ppm, Na were less than 250ppm, and K were less than 50ppm.

[0061] The lithium sulfide powder prepared in Example 3 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 3.5×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0062] Embodiment 4:

[0063] Embodiment 4 provides a method for preparing lithium sulfide, comprising the following steps:

[0064] (1) lithium sulfate (particle size 25 μm) and maltose were weighed in a molar amount of Li2SO4:C=1:3.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.35% of the mass of maltose) were added, mixed using a ball mill, heated to 60° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0065] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace; then, a mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 15% of the total volume of carbon monoxide and argon, and the temperature of the tubular furnace is raised to 875°C and maintained at 875°C for 2 hours; thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 9 μm and a conversion rate of 99.0%.

[0066] The high-purity lithium sulfide powder obtained in Example 4 was tested: the purity of the lithium sulfide powder was 99.90%, the residual amount of Li2SO4 was 0.006%, the content of by-product Li2O was 0.3%, the content of Li2CO3 was 0, the impurity ions Ca were less than 50ppm, Mg were less than 80ppm, Na were less than 250ppm, and K were less than 50ppm.

[0067] The lithium sulfide powder prepared in Example 4 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 2.3×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0068] Embodiment 5:

[0069] Embodiment 5 provides a method for preparing lithium sulfide, comprising the following steps:

[0070] (1) lithium sulfate (particle size 40 μm) and maltose were weighed in a molar ratio of Li2SO4:C=1:4, anhydrous butanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.5% of the mass of maltose) were added, mixed using a ball mill, heated to 30° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0071] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace; then, a mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 65% of the total volume of carbon monoxide and argon, and the temperature of the tubular furnace is raised to 825°C and maintained at 825°C for 2 hours; thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 13 μm and a conversion rate of 99.6%.

[0072] The high-purity lithium sulfide powder obtained in Example 5 was tested: the purity of the lithium sulfide powder was 99.91%, the residual amount of Li2SO4 was 0.005%, the content of by-product Li2O was 0.2%, the content of Li2CO3 was 0, the impurity ions Ca were less than 50ppm, Mg were less than 80ppm, Na were less than 250ppm, and K were less than 50ppm.

[0073] The lithium sulfide powder prepared in Example 5 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 4.4×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0074] Embodiment 6:

[0075] The only difference between Example 6 and Example 1 is that lithium hydroxide with a particle size of 20 μm is used as a lithium source precursor in Example 6; the rest of the preparation process is basically the same as that in Example 1.

[0076] Example 6 obtained high-purity lithium sulfide powder with a particle size of 11 μm and a conversion rate of 99.4%.

[0077] Embodiment 7:

[0078] The only difference between Example 7 and Example 1 is that in Example 7, lithium carbonate with a particle size of 20 μm is used as a lithium source precursor; the rest of the preparation process is basically the same as in Example 1.

[0079] Example 7 obtained high-purity lithium sulfide powder with a particle size of 9 μm and a conversion rate of 99.2%.

[0080] Comparative Example 1:

[0081] Comparative Example 1 provides a method for preparing lithium sulfide, comprising the following process:

[0082] (1) lithium sulfate (particle size 20 μm) and glucose were weighed in a molar ratio of Li2SO4:C=1:2.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.4% of the mass of glucose) were added, mixed using a ball mill, heated to 35° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0083] (2) The solid mixture was transferred to an alumina crucible, and the alumina crucible and the solid mixture were placed in a tubular furnace; then argon gas was flowed into the tubular furnace, and the temperature of the tubular furnace was raised to 900°C and maintained at 900°C for 2 hours; thereafter, the tubular furnace was naturally cooled to collect samples, and the recovered samples were placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 68 μm and a conversion rate of 81.1%.

[0084] The high-purity lithium sulfide powder obtained in Comparative Example 1 was tested: the purity of the lithium sulfide powder was 91%, the residual amount of Li2SO4 was 0.13%, the content of by-product Li2O was 3.9%, and the content of Li2CO3 was 1.9%.

[0085] The lithium sulfide powder prepared in Comparative Example 1 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 0.3×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0086] Comparative Example 2:

[0087] Comparative Example 2 provides a method for preparing lithium sulfide, comprising the following steps:

[0088] (1) lithium sulfate (particle size 20 μm) and glucose were weighed in a molar ratio of Li2SO4:C=1:2.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.4% of the mass of glucose) were added, mixed using a ball mill, heated to 35° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0089] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace. A mixed gas of argon and carbon monoxide is passed into the tubular furnace so that the volume of carbon monoxide is 5% of the total volume of carbon monoxide and argon. The temperature of the tubular furnace is raised to 900°C and maintained at 900°C for 2 hours. Thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain lithium sulfide powder with a particle size of 86 μm and a conversion rate of 85.9%.

[0090] The lithium sulfide powder obtained in Comparative Example 2 was tested: the purity of the lithium sulfide powder was 93%, the residual amount of Li2SO4 was 0.18%, the content of by-product Li2O was 2.2%, and the content of Li2CO3 was 1.5%.

[0091] The lithium sulfide powder prepared in Comparative Example 2 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 0.4×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0092] Comparative Example 3:

[0093] Comparative Example 3 provides a method for preparing lithium sulfide, comprising the following process:

[0094] (1) lithium sulfate and glucose were weighed in a molar ratio of Li2SO4:C=1:2.5, anhydrous ethanol and dopamine hydrochloride (the amount of dopamine hydrochloride added was 0.4% of the mass of glucose), mixed using a ball mill, heated to 35° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0095] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace. A mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 85% of the total volume of carbon monoxide and argon. The temperature of the tubular furnace is raised to 900°C and maintained at 900°C for 2 hours. Thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain lithium sulfide powder with a particle size of 70 μm and a conversion rate of 84.8%.

[0096] The lithium sulfide powder prepared in Comparative Example 3 was tested: the purity of the lithium sulfide powder was 90%, the residual amount of Li2SO4 was 0.14%, the content of by-product Li2O was 3.1%, and the content of Li2CO3 was 1.4%.

[0097] The lithium sulfide powder prepared in Comparative Example 3 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 0.1×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0098] Comparative Example 4:

[0099] Comparative Example 4 provides a method for preparing lithium sulfide, comprising the following steps:

[0100] (1) lithium sulfate (particle size 20 μm) and glucose were weighed in a molar amount of Li2SO4:C=1:2.5, anhydrous ethanol was added, mixed using a ball mill, heated to 35° C., mixed evenly, and dried using a spray dryer to obtain a solid mixture;

[0101] (2) The solid mixture is transferred to an alumina crucible, and the alumina crucible and the solid mixture are placed in a tubular furnace. A mixed gas of argon and carbon monoxide is circulated into the tubular furnace so that the volume of carbon monoxide is 10% of the total volume of carbon monoxide and argon. The temperature of the tubular furnace is raised to 900°C and maintained at 900°C for 2 hours. Thereafter, the tubular furnace is naturally cooled to collect samples, and the recovered samples are placed in an agate mortar and crushed to obtain high-purity lithium sulfide powder with a particle size of 75 μm and a conversion rate of 83.4%.

[0102] The high-purity lithium sulfide powder obtained in Comparative Example 4 was tested: the purity of the lithium sulfide powder was 90.4%, the residual amount of Li2SO4 was 0.15%, the content of by-product Li2O was 1.8%, and the content of Li2CO3 was 1.6%.

[0103] The lithium sulfide powder prepared in Comparative Example 4 was mixed with phosphorus sulfide and ball-milled to obtain an ionic conductivity of 0.16×10 -3 S / cm sulfide solid electrolyte, and then assembled the sulfide solid electrolyte with lithium metal and lithium cobalt oxide (LiCoO2) into an all-solid-state battery.

[0104] The results of the embodiments and comparative examples are shown in Table 1.

[0105] Table 1: Results of various examples and comparative examples

[0106]

[0107] It can be seen from the results of Example 1 and Comparative Example 4 that failure to add dopamine hydrochloride will result in reduced conversion rate and purity of lithium sulfide and increased content of by-products Li2O and Li2CO3.

[0108] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0109] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.

[0110] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing lithium sulfide, characterized in that: The following steps are involved: S101, mixing a lithium source precursor and a solid carbon source, adding a solvent and dopamine hydrochloride, ball milling, heating and drying to obtain a solid mixture; the lithium source precursor is lithium sulfate with a particle size of 10 μm to 100 μm; the solid carbon source is a mixture of any one or more of graphene, carbon black, carbon nanotubes, activated carbon, petroleum coke, glucose, sucrose, fructose, and maltose; the solvent is any one of ethanol, methanol, and butanol; S102, heating the solid mixture to 850°C to 950°C in a mixed atmosphere of carbon monoxide and inert gas, and then cooling to obtain lithium sulfide; the inert gas is any one of nitrogen, argon, and carbon dioxide; the volume of carbon monoxide accounts for 10% to 80% of the total volume of carbon monoxide and the inert gas.

2. The method for preparing lithium sulfide according to claim 1, characterized in that: The lithium source precursor and the solid carbon source are mixed in a molar ratio of lithium element to carbon element of 1:4 to 1:

12.

3. The method for preparing lithium sulfide according to claim 1, characterized in that: The added amount of dopamine hydrochloride is 0.2% to 0.5% of the mass of the solid carbon source.

4. The method for preparing lithium sulfide according to claim 1, characterized in that: The purity of the lithium sulfide obtained in step S102 is greater than 99%, wherein the impurity ions Ca are less than 50 ppm, Mg are less than 80 ppm, Na are less than 250 ppm, and K are less than 50 ppm.

5. The method for preparing lithium sulfide according to claim 1, characterized in that: In step S101, the heating temperature is 25-60°C; in step S102, the heating temperature is 850-950°C.

6. A sulfide solid electrolyte, characterized in that: It comprises lithium sulfide prepared by the preparation method according to any one of claims 1 to 5.

7. An all-solid-state battery, characterized in that: Comprising the sulfide solid electrolyte as claimed in claim 6.

Citation Information

Cited By

  • Preparation method of high-purity lithium sulfide

    CN120622414A

  • Synthesis method of lithium sulfide

    CN122212040A