Confined three-dimensional porous copper selective separation gel as well as preparation method and application thereof
By preparing a limited-domain three-dimensional porous copper selective separation gel, using waste wood fiber materials and polyvinyl alcohol to form a high-strength microchannel structure, the problems of small adsorption capacity and poor selectivity in electroplating wastewater are solved, and high efficiency is achieved Copper ion capture and wastewater treatment are economical and environmentally friendly, and the recycling of waste materials is realized.
Patent Information
- Application Number
- CN202411168324.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-22
AI Technical Summary
The existing sol-gel method has problems such as small adsorption capacity, slow adsorption rate and poor selectivity in electroplating wastewater treatment. The mechanical properties of traditional hydrogels are poor and cannot work stably in complex water environments.
The preparation method of a limited-domain three-dimensional porous copper selective separation gel is adopted. By mixing the waste wood fiber material with sodium chlorite and concentrated alkali and then mixing it with polyvinyl alcohol, the interpenetrating three-dimensional network structure is established using activator and coupling agent. , forming high-intensity microchannels and PVA network gels to achieve high selective adsorption of copper ions.
It realizes high selective adsorption and capture of copper ions in electroplating waste liquid, improves the separation effect, and through multiple recycling, it is economical and environmentally friendly, and realizes the recycling of waste materials and efficient management of copper-containing wastewater.
Smart Images

Figure CN118994696A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and more specifically to a confined three-dimensional porous copper selective separation gel and a preparation method and application thereof. Background Art
[0002] Electroplating is a widely used surface treatment technology. During the process, a large amount of wastewater containing copper and heavy metals will be generated. If it is discharged directly into the environment without treatment, it will cause serious environmental pollution. Therefore, how to effectively remove copper ions from electroplating wastewater has become an important research topic in the field of environmental protection.
[0003] As a commonly used method for preparing nanomaterials, the sol-gel method has the advantage of being able to prepare materials with high specific surface area and abundant active sites. It can also regulate the structure and properties of materials by changing raw materials or reaction conditions, which is of great significance for adsorption and separation in the environment.
[0004] However, its application in large-scale wastewater treatment is limited by its small adsorption capacity, slow adsorption rate, and poor selectivity for traditional adsorption materials. At the same time, traditional hydrogels are mostly synthesized by composite cross-linking, which has problems such as uneven channel structure, poor mechanical properties, and instability in complex water environments. Summary of the invention
[0005] The purpose of the present invention is to provide a confined three-dimensional porous copper selective separation gel and its preparation method and application to solve the problem of copper-containing heavy metal ion recovery in electroplating wastewater in a centralized control area.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] A method for preparing a confined three-dimensional porous copper selective separation gel comprises the following steps:
[0008] (1) soaking the waste wood fiber material in a sodium chlorite solution, adding acid to adjust the pH to 4-5, performing a first heating treatment to delignify, adding the treated product to a concentrated alkaline solution, performing a second heating treatment to remove hemicellulose, and obtaining a pretreated material;
[0009] (2) mixing the pretreated material and a polyvinyl alcohol solution to obtain a solution A;
[0010] (3) activating the solution A with an activator under alkaline conditions to obtain a solution B;
[0011] (4) subjecting the solution B to coupling treatment with a coupling agent under alkaline conditions, adding a neutralizing agent to adjust the pH to neutral, and obtaining the confined three-dimensional porous copper selective separation gel.
[0012] The invention also discloses a confined three-dimensional porous copper selective separation gel obtained by the above-mentioned preparation method.
[0013] The present invention also discloses a confined three-dimensional porous copper selective separation gel obtained by the above-mentioned preparation method, or the application of the confined three-dimensional porous copper selective separation gel in adsorbing copper ions.
[0014] Implementing the embodiments of the present invention will have the following beneficial effects:
[0015] The invention provides a simple and universal method for preparing a confined three-dimensional porous copper selective separation gel. The waste wood fiber material with a wide range of sources is used as a substrate. After being treated with sodium chlorite delignification and concentrated alkali hemicellulose removal, the material has a highly arranged pore configuration and a dense structure, and can be used as a natural micro-nano fiber channel to construct an ordered three-dimensional space. Polyvinyl alcohol is used as a gel scaffold, and an activator is used to establish an interpenetrating three-dimensional network structure to enhance its mechanical properties and toughness. Coupling modification using a coupling agent can effectively regulate the aggregation and cross-linking of molecules in the pores and surfaces, thereby realizing gel molding. A high-strength confined fiber three-dimensional microchannel and an interpenetrating PVA network gel structure are prepared. The coupling is mainly distributed in the surface layer of the gel resin, and the pore distribution is relatively uniform. The microtunneling effect is beneficial to the retention and interception of ions, and is beneficial to the adsorption and capture of copper ions, thereby improving the separation effect.
[0016] The preparation process of the invention is simple, the raw materials are cheap and easily available, and high-value utilization of resources is achieved. The prepared gel has a highly selective adsorption effect on copper ions in electroplating copper waste liquid and can be circulated for multiple times for adsorption, which is economical and environmentally friendly, and at the same time realizes the recycling of waste materials and the efficient treatment of copper-containing wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 N is the confined three-dimensional porous copper selective separation gel of Example 1 of the present invention. 2 Adsorption-desorption curves, pore volume and pore size distribution and FT-IR spectra.
[0018] Figure 2 XPS spectra of the confined three-dimensional porous copper selective separation gel before and after adsorption and desorption in Example 1 of the present invention: (a) full spectrum; (b) Cu2p; (c) Na1s; (d) O1s. DETAILED DESCRIPTION
[0019] The present invention is further described below in conjunction with specific embodiments, but the present invention is not limited in any way.
[0020] The present invention discloses a method for preparing a confined three-dimensional porous copper selective separation gel, comprising the following steps:
[0021] (1) The waste wood fiber material is soaked in a sodium chlorite solution, acid is added to adjust the pH to 4-5, and a first heating treatment is performed to delignify the waste wood fiber material. The treated product is added to a concentrated alkaline solution, and a second heating treatment is performed to remove hemicellulose to obtain a pretreated material.
[0022] In a specific embodiment, the waste wood fiber material includes one or more of wood, wood chips, and straw.
[0023] In a specific embodiment, the particle size of the waste wood fiber material is 50 mesh to 100 mesh.
[0024] In a specific embodiment, the particle size of the waste wood fiber material includes but is not limited to 50 mesh, 60 mesh, 70 mesh, 80 mesh, 90 mesh, 100 mesh, etc.
[0025] In a specific embodiment, the concentration of the sodium chlorite solution is 2 wt % to 3 wt %.
[0026] In a specific embodiment, the acid includes one or more of acetic acid solution, phosphoric acid, and citric acid, and the concentration of the acid is 2 wt % to 10 wt %.
[0027] In a specific embodiment, the concentrated alkali includes one or more of sodium hydroxide, sodium carbonate and sodium citrate, and the concentration of the alkali is 1 wt % to 3 wt %.
[0028] In a specific embodiment, the mass ratio of the waste wood fiber material to the sodium chlorite solution is 1-5:5-20.
[0029] In a specific embodiment, the temperature of the first heat treatment is 90°C to 95°C; the time of the first heat treatment is 1h to 1.5h; the temperature of the second heat treatment is 90°C to 100°C; the time of the second heat treatment is 1h to 2h.
[0030] (2) The pretreated material and the polyvinyl alcohol solution are mixed to obtain solution A.
[0031] In a specific embodiment, the concentration of the polyvinyl alcohol solution is 10 wt % to 20 wt %.
[0032] In a specific embodiment, the mixing temperature is 60° C. to 80° C.; and the mixing time is 0.5 h to 2 h.
[0033] (3) Activating solution A with an activator under alkaline conditions to obtain solution B.
[0034] In a specific embodiment, the activator is epichlorohydrin; the temperature of the activation treatment is 60° C. to 80° C.; and the time of the activation treatment is 1 h to 3 h.
[0035] (4) Solution B is subjected to coupling treatment with a coupling agent under alkaline conditions, and a neutralizing agent is added to adjust the pH to neutral to obtain a confined three-dimensional porous copper selective separation gel.
[0036] In a specific embodiment, the coupling agent includes one or more of iminodiacetic acid, acetamidoiminodiacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, (2-carboxyethyl)iminodiacetic acid, (2-carboxyphenyl)iminodiacetic acid, and N-(phosphonomethyl)iminodiacetic acid.
[0037] In a specific embodiment, the coupling treatment time is 60° C. to 80° C.; the coupling treatment time is 12 h to 24 h.
[0038] In a specific embodiment, the neutralizing agent includes one or more of acetic acid solution, phosphoric acid, and citric acid.
[0039] In a specific embodiment, the mass ratio of the waste wood fiber material, the polyvinyl alcohol solution, the activator, and the coupling agent in the present invention is 1-5: 10wt%-20wt%: 1wt%-2wt%: 1wt%-5wt%.
[0040] The invention discloses a confined three-dimensional porous copper selective separation gel obtained by a preparation method as in any embodiment.
[0041] In a specific embodiment, the pore size of the confined three-dimensional porous copper selective separation gel is 100 nm to 120 nm.
[0042] The present invention discloses a confined three-dimensional porous copper selective separation gel obtained by a preparation method as in any embodiment, or an application of the confined three-dimensional porous copper selective separation gel as in any embodiment in adsorbing copper ions.
[0043] In a specific embodiment, the present invention discloses a confined three-dimensional porous copper selective separation gel obtained by the preparation method of any embodiment, or the use of the confined three-dimensional porous copper selective separation gel of any embodiment in adsorbing copper ions in copper electroplating waste liquid.
[0044] The following are specific embodiments
[0045] Example 1
[0046] The preparation method of the confined three-dimensional porous copper selective separation gel of the present embodiment specifically includes: taking 10g of waste wood, crushing and screening to take 50 mesh particles, adding 100mL of 2% sodium chlorite solution to completely immerse it, and adding dilute acid to adjust the pH value to 4.6, placing it in a 90°C water bath and heating it for 1h, and then rinsing it with distilled water until it is neutral for removing lignin; then transferring it to 100mL of 2% sodium hydroxide solution, placing it in a 90°C water bath and heating it for 1h to further remove hemicellulose, after removing the solution; placing it in 200mL of 10wt% polyvinyl alcohol solution, stirring it at 60°C for 0.5h to form a suspension A; taking 10mL of epichlorohydrin and 50mL of 1mol / L sodium hydroxide mixed solution B, quickly adding solution B to the solution in a 60°C water bath, and ultrasonicating it for 0.5h, continuing the reaction for 2h, and then rinsing it with a large amount of deionized water; the gel resin cross-linked with epichlorohydrin is immersed in 25mL 0.2 mol / L iminodiacetic acid (IDA) and 1 mol / L Na 2 CO 3 The mixture was reacted at 60°C in the solution for 12 h; finally, it was neutralized with 5% acetic acid solution, rinsed with deionized water until neutral, and dried at room temperature.
[0047] Example 2
[0048] The preparation method of the confined three-dimensional porous copper selective separation gel of the present embodiment specifically includes: taking 10g of waste wood, crushing and screening to obtain 80 mesh particles, adding 50mL of 3% sodium chlorite solution to completely immerse it, and adding dilute acid to adjust the pH value to 4, placing it in a 90°C water bath and heating it for 1.2h, and then rinsing it with distilled water until it is neutral for removing lignin; then transferring it to 100mL of 2% sodium hydroxide solution, placing it in a 90°C water bath and heating it for 2h to further remove hemicellulose, and after removing the solution; placing it in 200mL of 10wt% polyvinyl alcohol solution, stirring it at 60°C for 0.5h to form a suspension A; taking 5mL of epichlorohydrin and 50mL of 1mol / L sodium hydroxide mixed solution B, quickly adding solution B to the solution in a 60°C water bath, and ultrasonicating it for 0.5h, continuing the reaction for 2h, and then rinsing it with a large amount of deionized water; the gel resin cross-linked with epichlorohydrin is immersed in 25mL 0.2 mol / L iminodiacetic acid, acetamidoiminodiacetic acid (1:1) and 1 mol / L Na 2 CO 3 The mixture was reacted at 60°C in the solution for 16 h; finally, it was neutralized with 5% acetic acid solution, rinsed with deionized water until neutral, and dried at room temperature.
[0049] Example 3
[0050] The preparation method of the confined three-dimensional porous copper selective separation gel of the present embodiment specifically includes: taking 10g of waste wood, crushing and screening to take 100 mesh particles, adding 200mL of 2% sodium chlorite solution to completely immerse it, and adding dilute acid to adjust the pH value to 5, placing it in a 95°C water bath and heating it for 1.5h, and then rinsing it with distilled water until it is neutral for removing lignin; then transferring it to 100mL of 3% sodium hydroxide solution, placing it in a 100°C water bath and heating it for 2h to further remove hemicellulose, and after removing the solution; placing it in 200mL of 10wt% polyvinyl alcohol solution, stirring it at 80°C for 1h to form a suspension A; taking 5mL of epichlorohydrin and 50mL of 1mol / L sodium hydroxide mixed solution B, quickly adding solution B to the solution in an 80°C water bath, and ultrasonicating it for 0.5h, continuing the reaction for 2h, and then rinsing it with a large amount of deionized water; the gel resin cross-linked with epichlorohydrin is immersed in 25mL 0.2 mol / L acetamidoiminodiacetic acid, N-(phosphonomethyl)iminodiacetic acid (2:1) and 1 mol / L Na 2 CO 3 The mixture was reacted at 60°C in the solution for 24 h; finally, it was neutralized with 5% acetic acid solution, rinsed with deionized water until neutral, and dried at room temperature.
[0051] Test Case
[0052] The basic properties of the confined three-dimensional porous copper selective separation gel prepared in Example 1 were tested, and the test results are as follows: Figure 1 As shown, it can be found that the pore size of the confined three-dimensional porous copper selective separation gel of Example 1 is concentrated in the range of 100nm to 120nm; its N 2 The adsorption-desorption curve shows a type IV adsorption-desorption isotherm with a H3 hysteresis loop. 0 <0.2) The adsorption curve changes very little. In the high pressure region (0.8<P / P 0 <1.0) rises rapidly, and combined with the pore volume and pore size distribution diagram, it shows that it has mesoporous and macroporous structures and the pore structure is irregular. From the test data, it can be obtained that the specific surface area of the gel is 20.07m 2 / g, pore volume 0.09m 3 / g. The existence of pore structure makes the gel resin have a larger specific surface area, Cu 2+ It enters the gel resin particles from the pores and continues to diffuse to the adsorption sites, increasing the contact area with the exchangeable ions on the functional groups. 2+ The exchange capacity is large, which is conducive to selective adsorption.
[0053] The confined three-dimensional porous copper selective separation gel prepared in Example 1 was subjected to a copper adsorption test to further explore the effect of the resin on Cu in copper-containing wastewater. 2+The adsorption mechanism of the gel resin was investigated by FT-IR and XPS tests before and after adsorption and desorption. Figure 1 As shown on the right, from the FT-IR spectrum characterization results, it can be seen that in the range of 3200-3700cm -1 The OH stretching vibration peak appears at 2841-2980cm -1 The stretching vibration absorption peak of the saturated bond CH is at about 1635 cm -1 The peak at 1390-1399 cm corresponds to the stretching vibration peak of C=O in the carboxyl group. -1 The protonated carboxyl group was identified at 1321-1215 cm -1 The range is the stretching vibration peak of CO and CN groups. Comparing the spectra before and after adsorption, it can be found that the adsorption of Cu 2+ After that, 1635cm -1 The peak at 1720 cm -1 A new vibration peak appeared at 1399cm -1 The peak at 1390 cm -1 , and 1470-1215cm -1 The peak at the position becomes broadened, and returns to the shape before adsorption after desorption. This indicates that during adsorption, the characteristic functional group acetic acid in the gel resin reacts with Cu 2+ The reaction occurred, causing the spectrum to change, which may be related to the presence of Na in -COONa. + Cu 2+ The exchange of acetate and CN bonds is related to the participation of ion adsorption.
[0054] like Figure 2 XPS spectrum shows that the Na1s absorption peak appears before the gel resin adsorption, indicating that the resin has a -COONa group structure. 2+ After that, the absorption peak of Cu2p appears, while the absorption peak of Na1s disappears, indicating that Cu 2+ and Na on the carboxyl group + The ion exchange reaction occurred, and the Na1s absorption peak was not reduced after desorption because the regeneration agent used was sulfuric acid solution, and NaOH was not used to convert the resin into Na type. From the characterization data, the two binding energies of Cu, 933.44eV and 953.14eV, represent Cu-O2p 3 / 2 and Cu-O2p 1 / 2The absorption peak of Cu forms a coordination bond with O in a divalent form; after adsorption, Na1s changes from 1 peak to 2 peaks, with binding energies of 1071.62eV and 1072.58eV respectively, and the morphology of Na changes; the existence forms of O in the structure are CO bonds, -COO bonds and C-OH bonds. Because of the existence of Na before adsorption, the spectrum of O element shows Na KLL Auger spectrum peaks. After adsorption, the absorption peaks of the two binding energies of O at 531.51eV and 532.28eV weakened and shifted, and returned to their original state after desorption.
[0055] In summary, the preparation method of the present invention is simple and universal. It uses widely available waste wood fiber materials as the substrate, and after being treated with sodium chlorite delignification and concentrated alkali hemicellulose removal, it has a highly arranged pore configuration and a dense structure, which can be used as a natural micro-nano fiber channel to construct an ordered three-dimensional space, and polyvinyl alcohol is used as a gel scaffold, and an activator is used to establish an interpenetrating three-dimensional network structure to enhance its mechanical properties and toughness. The coupling modification using a coupling agent can effectively regulate the aggregation and cross-linking of molecules in the pores and surfaces, thereby realizing gel molding. The prepared gel has a high-strength confined fiber three-dimensional microchannel and an interpenetrating PVA network structure, and the coupling is mainly distributed in the surface layer of the gel resin, and its pore distribution is relatively uniform, and the microtunneling effect is conducive to the retention and interception of ions, and has a highly selective adsorption effect on copper ions in electroplating copper waste liquid and can be adsorbed multiple times in cycles, which is economical and environmentally friendly, and at the same time realizes the recycling of waste materials and the efficient treatment of copper-containing wastewater.
[0056] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a confined three-dimensional porous copper selective separation gel, It is characterized in that The following steps are involved: (1) soaking the waste wood fiber material in a sodium chlorite solution, adding acid to adjust the pH to 4-5, performing a first heating treatment to delignify, adding the treated product to a concentrated alkaline solution, performing a second heating treatment to remove hemicellulose, and obtaining a pretreated material; (2) mixing the pretreated material and a polyvinyl alcohol solution to obtain a solution A; (3) activating the solution A with an activator under alkaline conditions to obtain a solution B; (4) subjecting the solution B to coupling treatment with a coupling agent under alkaline conditions, adding a neutralizing agent to adjust the pH to neutral, and obtaining the confined three-dimensional porous copper selective separation gel.
2. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that The pore size of the confined three-dimensional porous copper selective separation gel is 100nm to 120nm.
3. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that In step (1), the waste wood fiber material includes one or more of wood, sawdust, and straw; The particle size of the waste wood fiber material is 50 mesh to 100 mesh; The concentration of the sodium chlorite solution is 2wt% to 3wt%; The acid includes one or more of acetic acid, phosphoric acid, citric acid, etc., and the concentration of the acid is 2wt% to 10wt%; The concentrated alkali includes one or more of sodium hydroxide, sodium carbonate and sodium citrate, and the concentration of the alkali is 1wt% to 3wt%.
4. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that In step (1), the temperature of the first heating treatment is 90° C. to 95° C.; the time of the first heating treatment is 1 h to 1.5 h; The temperature of the second heating treatment is 90° C. to 100° C.; the time of the second heating treatment is 1 hour to 2 hours.
5. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that In step (2), the concentration of the polyvinyl alcohol solution is 10wt% to 20wt%; The mixing temperature is 60° C. to 80° C.; the mixing time is 0.5 h to 2 h.
6. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that In step (3), the activator is epichlorohydrin; The temperature of the activation treatment is 60° C. to 80° C.; the time of the activation treatment is 1 h to 3 h.
7. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that In step (4), the coupling agent includes one or more of iminodiacetic acid, acetamidoiminodiacetic acid, N-(2-hydroxyethyl)iminodiacetic acid, (2-carboxyethyl)iminodiacetic acid, (2-carboxyphenyl)iminodiacetic acid, and N-(phosphonomethyl)iminodiacetic acid; The coupling treatment time is 60°C to 80°C; the coupling treatment time is 12h to 24h; The neutralizing agent includes one or more of acetic acid solution, phosphoric acid and citric acid.
8. The method for preparing the confined three-dimensional porous copper selective separation gel according to claim 1, It is characterized in that The mass ratio of the waste wood fiber material, the polyvinyl alcohol solution, the activator and the coupling agent is 1-5: 10wt%-20wt%: 1wt%-2wt%: 1wt%-5wt%.
9. A confined three-dimensional porous copper selective separation gel obtained by the preparation method according to any one of claims 1 to 8.
10. Use of a confined three-dimensional porous copper selective separation gel obtained by the preparation method according to any one of claims 1 to 8, or a confined three-dimensional porous copper selective separation gel according to claim 9 in adsorbing copper ions.