Flexible controllable porous piezoelectric catalytic water purification membrane and preparation method thereof

By adding water-soluble sugars to the piezoelectric polymer and using spin coating and annealing processes, a flexible and controllable porous piezoelectric catalytic water purification film is prepared, which solves the problems of complexity and high cost of preparation of organic porous materials and achieves high efficiency The organic degradation and antibacterial properties are suitable for large-scale production.

CN118994707AInactive Publication Date: 2024-11-22XINYU UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411101381.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation process of existing organic porous piezoelectric materials is complex, costly and unenvironmental, especially in porosity regulation.

Method used

By incorporating and dissolving water-soluble sugars into the piezoelectric polymer, a flexible controlled porous piezoelectric catalytic water purification film was prepared, and a dense film was formed by spin coating and annealing, and formed by pure water dissolution and annealing air quenching. Controllable porous structure to improve piezoelectric performance.

Benefits of technology

It has achieved improvement in piezoelectric performance and controllability of pore size and porosity. When used for water purification, the degradation rate of organic compounds can reach 90% and the antibacterial rate can reach 80%. It has a simple process, environmental protection, low cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994707A_ABST
    Figure CN118994707A_ABST
Patent Text Reader

Abstract

The invention discloses a flexible controllable porous piezoelectric catalytic water purification membrane and a preparation method thereof, and the preparation method comprises the following steps: preparing a pore-forming agent / piezoelectric polymer mixed solution: adding a piezoelectric polymer into a pore-forming agent dispersion solution according to the mass ratio of a pore-forming agent to the piezoelectric polymer to obtain the pore-forming agent / piezoelectric polymer mixed solution; spin-coating the pre-treated substrate with the pore-forming agent / piezoelectric polymer mixed solution to form a film, and carrying out heat preservation to obtain a dense film; soaking the dense membrane in pure water to obtain a controllable porous membrane; and annealing and air-quenching the controllable porous membrane to obtain the porous piezoelectric catalytic membrane. According to the prepared porous piezoelectric catalytic membrane, the piezoelectric property of the membrane is effectively improved, so that the organic matter degradation rate and the antibacterial rate in the water purification process are greatly improved. The aperture of the water purification membrane can be regulated and controlled within 0.5-5 microns, and the porosity can be regulated and controlled within 10-60%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of piezoelectric catalysis, and in particular to a method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane. Background Art

[0002] In recent years, piezoelectric materials have been widely used in the fields of nanogenerators, sensors, catalysis, etc. Among them, polyvinylidene fluoride (PVDF) and its copolymers have attracted widespread attention due to their high flexibility, biocompatibility and good stability. In practical applications, introducing pore structures into piezoelectric materials to improve piezoelectric properties has become a common and effective strategy. Inorganic porous piezoelectric materials have been widely studied, proving that pore structures can effectively improve the piezoelectric and pyroelectric properties of materials. At present, the preparation process of organic porous piezoelectric materials is relatively complicated, costly or not environmentally friendly, and there are still great challenges in porosity regulation.

[0003] Natural water-soluble sugars are rich in hydroxyl groups. When introduced into PVDF, they can act as inducers, forming hydrogen bonds with their dipoles and inducing the formation of the electroactive phase of the polymer. At the same time, water-soluble sugars are easily dissolved from the composite material by pure water, and act as pore-forming agents to form a controllable porous structure. Moreover, by controlling the content of sugar incorporated, the pore size and porosity of the piezoelectric film can be effectively regulated. By improving the preparation process, the piezoelectric film is immediately kept warm after spin coating to avoid uncontrollable pore structures formed by slow evaporation of the solvent; annealing and air quenching after the water-soluble sugar can further improve the performance of the porous piezoelectric film. Summary of the invention

[0004] The purpose of the present invention is to solve the preparation demand of controllable porous organic materials, combine the piezoelectric catalytic properties of the materials, and use a specific process to prepare a controllable porous piezoelectric catalytic water purification membrane. By incorporating and dissolving water-soluble sugars into the piezoelectric polymer, the dual goals of increasing the piezoelectric active phase and forming a controllable porous structure are achieved at the same time. Moreover, the preparation process of the membrane is simple, green and environmentally friendly, low-cost, and suitable for large-scale production applications.

[0005] One aspect of the present invention provides a method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane, comprising the following steps:

[0006] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0007] According to the mass ratio of the pore-forming agent to the piezoelectric polymer being 10 to 40%, the piezoelectric polymer is added into the pore-forming agent dispersion, and stirred to dissolve to obtain a pore-forming agent / piezoelectric polymer mixed solution;

[0008] (2) Film making:

[0009] Spin-coat the pore-forming agent / piezoelectric polymer mixed solution on the pretreated substrate to form a film, and immediately place it in a forced air drying oven for heat preservation to obtain a dense film;

[0010] (3) Hole formation:

[0011] The dense membrane is immersed in pure water to obtain a controllable porous membrane;

[0012] (4) Post-processing:

[0013] The controllable porous membrane is annealed and air-quenched to obtain a porous piezoelectric catalytic membrane.

[0014] Preferably, the pore-forming agent is glucose, fructose or sucrose.

[0015] Preferably, the piezoelectric polymer is polyvinylidene fluoride PVDF and its derivatives, and the polyvinylidene fluoride PVDF derivative is any one of polyvinylidene fluoride-trifluoroethylene PVDF-TrFE and polyvinylidene fluoride-hexafluoropropylene PVDF-HFP.

[0016] Preferably, the solvent is any one of N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO, N-methylpyrrolidone NMP and N,N-dimethylacetamide DMAc, or a mixed solvent consisting of N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO and acetone.

[0017] Preferably, the pore-forming agent is added to the solvent according to a mass ratio and ultrasonically dispersed to obtain a pore-forming agent dispersion with a mass concentration of 6 to 60 mg / mL.

[0018] Preferably, the substrate is made of flat glass, which is pre-treated by washing with pure water and alcohol and then drying.

[0019] Preferably, the spin coating speed is 500-2000 rpm, and the time is 30-90 s; the film forming insulation temperature on the substrate is 50-80° C., and the time is 0.5-1 h; and the dense film immersion time is 24-48 h.

[0020] Preferably, the annealing temperature is 120-140° C., and the annealing time is 1-3 hours.

[0021] Another aspect of the present invention provides a flexible controllable porous piezoelectric catalytic water purification membrane prepared by the method.

[0022] The present invention adopts the above technical solution, which has the following beneficial effects:

[0023] 1. The present invention achieves the dual goals of increasing the piezoelectric active phase and forming a controllable porous structure by incorporating and dissolving water-soluble sugar into the piezoelectric polymer, thereby effectively improving the piezoelectric performance of the membrane.

[0024] 2. The pore size of the water purification membrane in the present invention can be adjusted between 0.5 and 5 μm, and the porosity can be adjusted between 10 and 60%.

[0025] 3. The porous membrane of the present invention can be used in the field of water purification, and can simultaneously achieve organic matter degradation and antibacterial effects under the action of piezoelectric catalysis. The organic matter degradation rate can reach 90%, and the antibacterial rate can reach 80%.

[0026] 4. The preparation process of the present invention is simple, green and environmentally friendly, low-cost, and suitable for large-scale production applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:

[0028] Figure 1 is the SEM morphology of the piezoelectric catalytic film in the embodiment of the present invention;

[0029] Figure 2 is the pore size and porosity of the piezoelectric catalytic film in the embodiment of the present invention;

[0030] Figure 3 is the voltage response sensitivity of the piezoelectric catalytic film in the embodiment of the present invention;

[0031] Figure 4 It is the organic matter degradation rate and antibacterial rate of the piezoelectric catalytic film in the embodiment of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The exemplary embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0033] The present invention provides a method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane, comprising the following steps:

[0034] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0035] The pore-forming agent (glucose, fructose or sucrose) is added to a solvent (any one of N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO, N-methylpyrrolidone NMP and N,N-dimethylacetamide DMAc or a mixed solvent composed of acetone) according to a certain mass ratio, and ultrasonically dispersed to obtain a pore-forming agent dispersion with a mass concentration of 6 to 60 mg / mL; according to the mass ratio of the pore-forming agent to the piezoelectric polymer (polyvinylidene fluoride PVDF and its derivatives, the polyvinylidene fluoride PVDF derivatives are polyvinylidene fluoride-trifluoroethylene PVDF-TrFE, polyvinylidene fluoride-hexafluoropropylene PVDF-HFP) of 10 to 40%, the piezoelectric polymer is added to the pore-forming agent dispersion, stirred and dissolved, and a pore-forming agent / piezoelectric polymer mixed solution is obtained.

[0036] Among them, the pore former acts as an auxiliary agent to induce the formation of piezoelectric phase in the piezoelectric polymer. The pore former is rich in hydroxyl groups and forms hydrogen bonds with the dipoles of the piezoelectric polymer, which can enhance the generation of polar piezoelectric phase in the piezoelectric polymer, thereby improving the piezoelectric properties of the material. A small amount of pore former is wrapped by the piezoelectric polymer, which can also improve the thermal stability of the film.

[0037] (2) Film making:

[0038] The flat glass substrate is cleaned with pure water and alcohol and then dried. The substrate can withstand high temperatures above 200°C. The pore-forming agent / piezoelectric polymer mixture is then spin-coated on the substrate at a speed of 500 to 2000 rpm for 30 to 90 seconds to form a film. The film is immediately placed in a forced air drying oven at a temperature of 50 to 80°C for 0.5 to 1 hour for heat preservation to obtain a dense film.

[0039] Among them, spin coating can play a role in stretching and polarizing the composite film while preforming the material, so that the dipoles in the polymer are arranged in order, thereby improving the piezoelectric properties of the material. Low-temperature drying allows the solvent in the preformed composite film to evaporate quickly to avoid vapor-induced phase separation with water molecules in the air, thereby avoiding the formation of disordered cross-linked pores.

[0040] (3) Hole formation:

[0041] The dense membrane is immersed in pure water for 24 to 48 hours to allow the pore-forming agent to fully dissolve in the pure water, thereby obtaining a controllable porous membrane.

[0042] The pore-forming agent in the composite film is dissolved by pure water to form uniformly distributed ordered pores, thereby reducing the dielectric constant of the material and further improving the piezoelectric properties of the material. Moreover, by controlling the content of the pore-forming agent in step (1), the pore size and porosity of the piezoelectric film can be effectively regulated, thereby optimizing the piezoelectric properties of the material and controlling the passage of organic matter and bacteria in water purification.

[0043] (4) Membrane post-treatment:

[0044] The porous membrane is placed in a forced air drying oven for annealing at a temperature of 120 to 140° C. for 1 to 3 hours; and air quenching is performed to obtain a high-performance porous piezoelectric water purification membrane.

[0045] Among them, controlling the annealing temperature to be higher than the Curie temperature of the material and lower than the melting point of the material can have a thermal polarization effect on the material, and play a synergistic role with the induced polarization in step (1) and the tensile polarization in step (2), ensuring that the piezoelectric properties of the material are reasonably optimized, thereby maximizing the degradation of organic matter and sterilization effect in the subsequent piezoelectric catalytic process.

[0046] The preparation method of the present invention is further described in detail below through specific examples.

[0047] Embodiment 1:

[0048] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0049] Sucrose was added into a mixed solvent of N,N-dimethylformamide DMF / acetone (volume ratio 2:3), and ultrasonically dispersed to obtain a sucrose dispersion with a mass concentration of 20 mg / mL;

[0050] According to the mass ratio of sucrose to polyvinylidene fluoride-hexafluoropropylene PVDF-HFP being 40%, PVDF-HFP was added into the sucrose dispersion, and stirred to dissolve, thereby obtaining a sucrose / PVDF-HFP mixed solution;

[0051] (2) Film making:

[0052] The glass substrate was cleaned with pure water and alcohol and then dried. Then, the sucrose / PVDF-HFP mixed solution was spin-coated on the substrate to form a film. The spin-coating speed was 1000 rpm for 60 seconds. The substrate was immediately placed in a forced air drying oven at 80°C for 0.5 hours to obtain a dense film.

[0053] (3) Hole formation:

[0054] The dense membrane was immersed in pure water for 36 hours to allow the sucrose to fully dissolve in the pure water, thereby obtaining a controllable porous membrane;

[0055] (4) Post-processing:

[0056] The porous membrane was placed in a forced air drying oven for annealing at 120° C. for 3 h, and then air quenched to obtain a high-performance porous piezoelectric catalytic membrane.

[0057] After testing, the SEM morphology of the porous piezoelectric catalytic membrane prepared in this embodiment has uniform pore size and uniform pore distribution; the average pore size of the piezoelectric catalytic membrane is 3.2μm and the porosity is 58%; the piezoelectric response sensitivity is 46mV / N, which is 31% higher than that of the pure membrane (35mV / N), and the organic matter degradation rate and antibacterial rate are 65% and 61% respectively.

[0058] Embodiment 2:

[0059] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0060] Glucose was added into a mixed solvent of dimethyl sulfoxide (DMSO) and acetone (volume ratio 2:3), and ultrasonically dispersed to obtain a glucose dispersion with a mass concentration of 40 mg / mL.

[0061] According to the mass ratio of glucose to polyvinylidene fluoride (PVDF) being 30%, PVDF was added into the glucose dispersion, and stirred to dissolve, thereby obtaining a glucose / PVDF mixed solution;

[0062] (2) Film making:

[0063] The glass substrate was cleaned with pure water and alcohol and then dried. Then, the glucose / PVDF mixture was spin-coated on the substrate to form a film. The spin-coating speed was 1500 rpm for 40 seconds. The substrate was immediately placed in a forced air drying oven at 70°C for 0.5 hours to obtain a dense film.

[0064] (3) Hole formation:

[0065] The dense membrane was immersed in pure water for 48 hours to allow the sucrose to fully dissolve in the pure water, thereby obtaining a controllable porous membrane;

[0066] (4) Post-processing:

[0067] The porous membrane was placed in a forced air drying oven for annealing at 130° C. for 3 h, and then air quenched to obtain a high-performance porous piezoelectric catalytic membrane.

[0068] After testing, the SEM morphology of the porous piezoelectric catalytic membrane prepared in this embodiment has uniform pore size and uniform pore distribution; the average pore size of the piezoelectric catalytic membrane is 2.6μm, and the porosity is 55%; the piezoelectric response sensitivity is 63mV / N, which is 80% higher than that of the pure membrane (35mV / N), and the organic matter degradation rate and antibacterial rate are 78% and 71% respectively.

[0069] Embodiment 3:

[0070] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0071] Fructose was added into N-methylpyrrolidone (NMP) solvent and ultrasonically dispersed to obtain a fructose dispersion with a mass concentration of 60 mg / mL;

[0072] According to the mass ratio of fructose to polyvinylidene fluoride-trifluoroethylene PVDF-TrFE being 20%, PVDF-TrFE was added into the fructose dispersion, and stirred to dissolve, thereby obtaining a fructose / PVDF-TrFE mixed solution;

[0073] (2) Film making:

[0074] The glass substrate was cleaned with pure water and alcohol and then dried. Then, the fructose / PVDF-TrFE mixed solution was spin-coated on the substrate to form a film. The spin-coating speed was 2000 rpm for 30 seconds. The film was immediately placed in a forced air drying oven at 60°C for 1 hour to obtain a dense film.

[0075] (3) Hole formation:

[0076] The dense membrane was immersed in pure water for 24 hours to allow the sucrose to fully dissolve in the pure water, thereby obtaining a controllable porous membrane;

[0077] (4) Post-processing:

[0078] The porous membrane was placed in a forced air drying oven for annealing at 125° C. for 2 h, and then air quenched to obtain a high-performance porous piezoelectric catalytic membrane.

[0079] After testing, the SEM morphology of the porous piezoelectric catalytic membrane prepared in this embodiment has uniform pore size and uniform pore distribution; the average pore size of the piezoelectric catalytic membrane is 1.8μm and the porosity is 38%; the piezoelectric response sensitivity is 103mV / N, which is 194% higher than that of the pure membrane (35mV / N), and the organic matter degradation rate and antibacterial rate are 92% and 83% respectively.

[0080] Embodiment 4:

[0081] (1) Preparation of porogen / piezoelectric polymer mixed solution:

[0082] Sucrose was added into N,N-dimethylacetamide DMAc solvent and ultrasonically dispersed to obtain a sucrose dispersion with a mass concentration of 6 mg / mL;

[0083] According to the mass ratio of sucrose to polyvinylidene fluoride (PVDF) being 10%, PVDF was added into the sucrose dispersion, and stirred to dissolve, thereby obtaining a sucrose / PVDF mixed solution;

[0084] (2) Film making:

[0085] The glass substrate was cleaned with pure water and alcohol and then dried. Then, the sucrose / PVDF mixed solution was spin-coated on the substrate to form a film. The spin-coating speed was 500 rpm and the time was 90 s. The film was immediately placed in a forced air drying oven at 50°C for 1 h to obtain a dense film.

[0086] (3) Hole formation:

[0087] The dense membrane was immersed in pure water for 40 hours to fully dissolve the sucrose in the pure water, thereby obtaining a controllable porous membrane;

[0088] (4) Post-processing:

[0089] The porous membrane was placed in a forced air drying oven for annealing at 140° C. for 1 h, and then air quenched to obtain a high-performance porous piezoelectric catalytic membrane.

[0090] After testing, the SEM morphology of the porous piezoelectric catalytic membrane prepared in this embodiment has uniform pore size and uniform pore distribution; the average pore size of the piezoelectric catalytic membrane is 0.6μm, the porosity is 19%, and the piezoelectric response sensitivity is 77mV / N, which is 120% higher than that of the pure membrane (35mV / N). The organic matter degradation rate and antibacterial rate are 82% and 75%, respectively.

[0091] From the above embodiments and Figure 1-4 The experimental results show that the pores prepared by the method of the present invention are evenly distributed with uniform pore size. The SEM morphology of the piezoelectric catalytic membrane is shown in Figure 1 As shown in Figure 2, the pore size and porosity of the piezoelectric catalytic membrane are shown in Figure 2 As shown, the pore size can be adjusted between 0.5 and 5 μm, and the porosity can be adjusted between 10 and 60%. Figure 3 The voltage response sensitivity of the piezoelectric catalytic membrane shows that the piezoelectric performance of the membrane is effectively improved due to the incorporation of the functional group-rich pore-forming agent to induce the piezoelectric phase and dissolve to form a porous process; further, when the membrane is used for water purification, the organic matter degradation rate can reach 90%, and the antibacterial rate can reach 80%, which is greatly improved compared with the pure membrane. Figure 4 shown.

[0092] It can be seen from this that the method of the present invention is a method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane. The obtained water purification membrane has excellent organic matter degradation and antibacterial properties, and the preparation process is simple, green and environmentally friendly, low cost, and suitable for large-scale production applications.

[0093] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.

Claims

1. A method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane, characterized in that: The following steps are involved: (1) Preparation of porogen / piezoelectric polymer mixed solution: According to the mass ratio of the pore-forming agent to the piezoelectric polymer being 10 to 40%, the piezoelectric polymer is added into the pore-forming agent dispersion, and stirred to dissolve to obtain a pore-forming agent / piezoelectric polymer mixed solution; (2) Film making: Spin-coat the pore-forming agent / piezoelectric polymer mixed solution on the pretreated substrate to form a film, and immediately place it in a forced air drying oven for heat preservation to obtain a dense film; (3) Hole formation: The dense membrane is immersed in pure water to obtain a controllable porous membrane; (4) Post-processing: The controllable porous membrane is annealed and air-quenched to obtain a porous piezoelectric catalytic membrane.

2. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The pore-forming agent is glucose, fructose or sucrose.

3. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The piezoelectric polymer is polyvinylidene fluoride and its derivatives, and the polyvinylidene fluoride derivative is any one of polyvinylidene fluoride-trifluoroethylene and polyvinylidene fluoride-hexafluoropropylene.

4. The method for preparing the flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The solvent is any one of N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylacetamide or a mixed solvent of N,N-dimethylformamide and acetone.

5. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The pore-forming agent is added into the solvent according to the mass ratio, and ultrasonically dispersed to obtain a pore-forming agent dispersion with a mass concentration of 6-60 mg / mL.

6. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The substrate is made of flat glass, which is pre-treated by washing with pure water and alcohol and then drying.

7. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The spin coating speed is 500-2000 rpm, and the time is 30-90 seconds; the film forming insulation temperature on the substrate is 50-80° C., and the time is 0.5-1 hour; and the dense film immersion time is 24-48 hours.

8. The method for preparing a flexible controllable porous piezoelectric catalytic water purification membrane according to claim 1, characterized in that: The annealing temperature is 120-140°C and the time is 1-3 hours.

9. A flexible controllable porous piezoelectric catalytic water purification membrane prepared by the method according to any one of claims 1 to 8.

10. Application of the flexible controllable porous piezoelectric catalytic water purification membrane according to claim 9 in organic matter degradation and antibacterial in the field of water purification.

Citation Information

Cited By

  • PVTF flexible piezoelectric film having double-layer structure, and preparation method therefor and use thereof

    WO2026129993A1