Polypropylene micropolyethylene membrane, method for preparing said

CN118994776APending Publication Date: 2024-11-22SK INNOVATION CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410574906.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

然而,这种微孔膜的穿刺强度显著低至小于0.05N/μm,并且热收缩稳定性与现有技术相比没有大幅提高,从而在热箱(hot-box)评价等高温环境中电池的安全性差,因此具有不适合应用于具有高容量的大型化电池的缺点

Benefits of technology

[0026]根据本发明的聚丙烯微孔膜可以具有优异的穿刺强度和透过率的同时确保显著提高的高温下的耐热性。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994776A_ABST
    Figure CN118994776A_ABST
Patent Text Reader

Abstract

The invention relates to a polypropylene microporous membrane, a method for preparing the microporous membrane and a diaphragm comprising the microporous membrane. According to one embodiment, there is provided a polypropylene microporous membrane comprising a polypropylene having a viscosity average molecular weight of 1 * 106 g / mol to 3 * 106 g / mol, the thickness of the polypropylene microporous membrane being 3-30 [mu] m, the puncture strength being 0.20 N / [mu] m or more, the air permeability being 1.0 * 10-5 Darcy or more, the porosity being 25-60%, and the average pore diameter being 25-50 nm, and the lateral shrinkage rate measured after standing at 150 DEG C for 1 hour is 20% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polypropylene microporous membrane, a method for preparing the microporous membrane, and a separator comprising the microporous membrane. According to one embodiment, the present invention relates to a polypropylene microporous membrane having excellent puncture strength and permeability and improved heat resistance, a method for preparing the microporous membrane, and a separator comprising the microporous membrane. Background Art

[0002] Polyolefin-based microporous membranes are used in various fields such as separation filters, secondary battery separators, fuel cell separators, and supercapacitor separators. Among them, polyolefin-based microporous membranes are widely used as secondary battery separators due to their excellent electrical insulation and ion permeability.

[0003] In recent years, secondary batteries are being made high-capacity and large-scale for use in electric vehicles, energy storage systems (ESS), etc., so ensuring the safety of the battery has become a more important factor. For example, when the battery is exposed to a high temperature environment or is working, the diaphragm shrinks, so an internal short circuit may be caused, and a fire may occur due to the internal short circuit. Therefore, it is necessary to develop a polyolefin-based microporous membrane with excellent heat resistance that can cope with the increase in battery temperature. In addition to heat resistance, high mechanical strength is also required to improve the safety of the battery during manufacturing and use, and high transmittance is required to increase capacity and power.

[0004] High molecular weight polyethylene used as a main material of a secondary battery separator has a low melting temperature of about 140° C. and thus has limited heat resistance. As a solution to overcome this problem, polypropylene having a high melting temperature is used as a material of a secondary battery separator.

[0005] However, the existing polypropylene microporous membrane is prepared by a dry process. Due to the characteristics of the dry process, this dry polypropylene microporous membrane is mainly stretched with a low longitudinal / transverse stretch ratio or unidirectional stretching, and because the puncture strength is relatively low, it can only be compensated by increasing the thickness. In addition, the pores of the microporous membrane obtained by the dry process are straight and have a large size, and have the characteristics of low uniformity of pore size. The characteristics as described above have a negative impact on the performance of the battery, so the dry polypropylene microporous membrane is not suitable for application in the field of secondary batteries.

[0006] In order to solve this problem, Korean Patent Publication No. 10-2011-0101202 discloses a polypropylene microporous membrane prepared by a wet process and having excellent heat resistance and strength. However, the puncture strength of this microporous membrane is significantly low, less than 0.05N / μm, and the thermal shrinkage stability is not greatly improved compared with the prior art, so that the safety of the battery in a high temperature environment such as a hot box evaluation is poor, and therefore it has the disadvantage of being unsuitable for application to large-scale batteries with high capacity.

[0007] Therefore, it is necessary to develop a polypropylene microporous membrane, which has high puncture strength and high transmittance in terms of battery performance and safety, and at the same time has significantly improved heat resistance at higher temperatures, so that excellent battery safety can be achieved, especially in a hot box evaluation at 140°C, which is an indicator for high-temperature safety evaluation. Summary of the invention

[0008] Technical issues to be solved

[0009] In order to solve the above problems, an object of the present invention is to provide a polypropylene microporous membrane having excellent puncture strength and permeability and significantly improved heat resistance at high temperatures, a method for preparing the microporous membrane, and a separator including the microporous membrane.

[0010] In particular, an object of the present invention is to provide a polypropylene microporous film that can achieve excellent battery safety even in a hot box evaluation at 140° C. after battery assembly.

[0011] The polypropylene microporous membrane of the present invention can be widely used in electric vehicles, battery charging stations, other green technology fields such as solar power generation and wind power generation using batteries. In addition, the polypropylene microporous membrane of the present invention can be used in eco-friendly electric vehicles and hybrid vehicles to prevent climate change by inhibiting air pollution and greenhouse gas emissions.

[0012] Technical Solution

[0013] As a method for achieving the above technical problem, the present invention provides a polypropylene microporous membrane, wherein the polypropylene microporous membrane comprises a polypropylene microporous membrane having a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of polypropylene, the thickness of the polypropylene microporous membrane is 3-30 μm, the puncture strength is above 0.20 N / μm, and the air permeability is 1.0×10 -5The microporous membrane has a porosity of 25-60%, an average pore size of 25-50 nm, and a transverse shrinkage of 20% or less measured after being placed at 150°C for 1 hour. The porosity refers to the proportion of the volume of the microporous membrane composed of voids or pores. The polypropylene resin can be a homopolymer polypropylene. As an example, the homopolymer polypropylene resin can have a high crystallinity of more than 40%, more than 50%, more than 60%, or more than 70%. As an example, a high crystalline homopolymer polypropylene resin can have a melting point of 160-170°C.

[0014] In one embodiment, the polypropylene microporous membrane may have a melt fracture temperature of 165° C. or higher.

[0015] In one embodiment, the transverse shrinkage of the polypropylene microporous membrane may be 15% or less.

[0016] In one embodiment, the polypropylene microporous membrane may be prepared by a wet process including a sequential biaxial stretching process.

[0017] In addition, as another method for achieving the above technical problem, the present invention provides a method for preparing a polypropylene microporous membrane, the method comprising the following steps: (a) extruding a polypropylene microporous membrane having a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of a polypropylene resin and a diluent are melt-kneaded to prepare a melt; (b) the melt is extruded to form a sheet; (c) the sheet is sequentially biaxially stretched in the longitudinal and transverse directions to form a film; (d) the diluent is extracted from the stretched film and dried; and (e) the dried film is heat-stretched at a temperature at which 2-5% of the crystals of the polypropylene resin melt, and the heat-stretched film is heat-set and heat-relaxed at a temperature at which 25-60% of the crystals of the polypropylene resin melt for heat treatment.

[0018] In one embodiment, the heat stretching of step (e) may be performed at a temperature of 125-135°C.

[0019] In one embodiment, the heat setting and heat relaxation of step (e) may be performed at a temperature of 155-165°C.

[0020] Another embodiment of the present invention provides a polypropylene microporous membrane prepared by the preparation method.

[0021] Another embodiment of the present invention provides a microporous membrane for a secondary battery separator, wherein the microporous membrane for a secondary battery separator comprises a microporous membrane having a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6g / mol of polypropylene, the thickness of the microporous membrane for the secondary battery separator is 3-30 μm, the puncture strength is above 0.20 N / μm, and the air permeability is 1.0×10 -5 Darcy or above, the porosity is 25-60%, the average pore size is 25-50nm, and the lateral shrinkage measured after being placed at 150°C for 1 hour is less than 20%.

[0022] In one embodiment, the microporous film for a secondary battery separator may have a melt fracture temperature of 165° C. or higher.

[0023] Another embodiment of the present invention provides a secondary battery including a positive electrode, a negative electrode, and the separator according to the one embodiment.

[0024] Furthermore, as another method for achieving the above technical problem, the present invention provides a separator including the polypropylene microporous membrane as described above.

[0025] Beneficial Effects

[0026] The polypropylene microporous membrane according to the present invention can have excellent puncture strength and permeability while ensuring significantly improved heat resistance at high temperatures.

[0027] In addition, the puncture strength of the polypropylene microporous membrane according to the present invention can be 0.20 N / μm or more, and the air permeability can be 1.0×10 -5 Darcy above.

[0028] Furthermore, the transverse shrinkage of the polypropylene microporous film according to the present invention measured after being left at 150° C. for 1 hour may be 20% or less.

[0029] In addition, the present invention can provide a battery, the battery including the polypropylene microporous membrane according to one embodiment, thereby ensuring excellent battery performance while having excellent safety without smoke or fire in a high temperature environment. In detail, the present invention can provide a battery having excellent safety without smoke or fire of the battery in a high temperature hot box evaluation at 140°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a diagram showing a framework for measuring the melt fracture temperature of a microporous membrane prepared in one embodiment.

[0031] Figure 2 : is a diagram showing a state in which a microporous membrane is fixed to a frame for measuring the melt fracture temperature of a microporous membrane prepared in one embodiment with an adhesive tape. DETAILED DESCRIPTION

[0032] The embodiments described in this specification can be modified into various forms, and the technology according to one embodiment is not limited to the embodiments described below. In addition, the implementation form of one embodiment is provided to more completely explain the present invention to those skilled in the art.

[0033] Furthermore, unless otherwise specifically stated herein, singular forms used in the specification and the claims may also include plural forms.

[0034] In addition, the numerical range used in this specification includes the lower limit value and the upper limit value and all values ​​in the range, the increments logically derived from the form and width of the defined range, all values ​​defined therein, and all possible combinations of the upper and lower limits of the numerical range defined in different forms. In this specification, unless otherwise specifically defined, values ​​outside the numerical range that may be generated due to experimental errors or rounding of values ​​are also included in the defined numerical range.

[0035] Furthermore, throughout the specification, unless otherwise specifically stated to the contrary, the description “comprising” or “including” a certain constituent element means that other constituent elements may also be included, rather than excluding other constituent elements.

[0036] The present invention provides a polypropylene microporous membrane, wherein the polypropylene microporous membrane comprises a polypropylene microporous membrane having a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of polypropylene, the thickness of the polypropylene microporous membrane is 3-30 μm, the puncture strength is above 0.20 N / μm, and the air permeability is 1.0×10 -5 Darcy or above, the porosity is 25-60%, the average pore size is 25-50nm, and the lateral shrinkage measured after being placed at 150°C for 1 hour is less than 20%.

[0037] In recent years, with the high capacity and large-scale, secondary batteries need to meet more excellent battery performance and safety. For this reason, secondary battery separators need to have higher levels of heat resistance and transmittance at the same time. For this reason, polypropylene with a high melting temperature is used as the material for secondary battery separators, but the polypropylene microporous membrane prepared by the dry process has low puncture strength and excessively large and uneven pore size, so it is not suitable for use in the field of secondary batteries. In addition, the polypropylene microporous membrane prepared by the wet process also has low puncture strength, and the thermal shrinkage stability is not greatly improved compared with the prior art, so that the safety of the battery is poor in high temperature environments such as hot box evaluation, so it has the disadvantage of being unsuitable for large-scale batteries with high capacity.

[0038] As a result of repeated research, the inventors have confirmed that a polypropylene microporous membrane can be prepared, which can simultaneously achieve a puncture strength of more than 0.20 N / μm and a -5 It has an air permeability of more than Darcy, a porosity of 25-60%, an average pore size of 25-50nm, and a lateral shrinkage of less than 20% measured after being placed at 150°C for 1 hour. Therefore, it can have excellent puncture strength and permeability, and can significantly improve heat resistance at high temperatures.

[0039] In a secondary battery according to one embodiment, by including a polypropylene microporous membrane that satisfies the physical properties as described above, excellent battery performance and safety at high temperatures can be ensured at the same time. In particular, the present invention can provide a battery that can have excellent thermal safety at high temperatures without smoke or fire of the battery in a high-temperature hot-box evaluation at 140°C. The manufacturing and evaluation methods of the batteries evaluated above are as follows. The positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material are wound together with the microporous membrane of the present invention and placed in an aluminum soft pack to make a battery. Next, an electrolyte in which 1M of lithium hexafluorophosphate (LiPF6) is dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2 is injected into the interior of the battery and sealed to make a battery with a capacity of 2Ah. Next, the battery was aged and degassed, fully charged to 4.2V, placed in an oven, heated at 5°C / min, and left at 140°C for 30 minutes to confirm whether the battery smoked or caught fire. That is, the polypropylene microporous membrane of the present invention satisfies the above-mentioned physical properties at the same time, and is therefore suitable for use in high-power / high-capacity batteries.

[0040] As an embodiment, the polypropylene microporous membrane simultaneously satisfying the physical properties as described above may be prepared by using a polypropylene resin having a viscosity average molecular weight in a specific range or heat-treating at a specific temperature after extracting a diluent.

[0041] As an embodiment, the viscosity average molecular weight of the polypropylene resin contained in the polypropylene microporous membrane may be 1×10 6 g / mol to 3×10 6 g / mol, specifically 1.2×10 6 g / mol to 2.5×10 6 g / mol, more specifically 1.3×10 6 g / mol to 2.2×10 6 g / mol.

[0042] As an embodiment, the heat treatment at a specific temperature after extracting the diluent may be to heat-stretch the film obtained after extracting the diluent at a first temperature, and to heat-set and heat-relax the heat-stretched film at a second temperature higher than the first temperature.

[0043] Therefore, the polypropylene microporous membrane may have excellent puncture strength and permeability, and may have significantly improved heat resistance at high temperatures.

[0044] Hereinafter, the polypropylene microporous membrane will be described in more detail.

[0045] In one embodiment, the thickness of the polypropylene microporous membrane can be 3-30 μm, specifically 5-20 μm, and more specifically 5-15 μm. The microporous membrane of the present invention can also achieve excellent puncture strength, air permeability and thermal shrinkage at the same time at the thickness in the above range, and it is particularly found that it can have excellent battery safety in the hot box evaluation according to the evaluation method of the following embodiment. In addition, it has excellent resistance to external stress generated during the manufacture of the battery, temperature rise and dendrites that occur during the charging and discharging of the battery, and the internal resistance of the battery is low, so the charging and discharging performance of the battery can be improved.

[0046] In one embodiment, the polypropylene microporous membrane may also have a puncture strength of 0.20N / μm or more at a thickness in the above range. Specifically, the puncture strength may be 0.25N / μm or more or 0.30N / μm or more, and there is no particular limit on its upper limit, but for example, it may be 1.0N / μm or less. In a specific embodiment, the puncture strength may be 0.20-1.0N / μm, 0.25-1.0N / μm or 0.30-1.0N / μm, but is not limited thereto. By satisfying the puncture strength in the above range, it has excellent resistance to external stresses generated during the manufacture of the battery and dendrites generated during the charging and discharging of the battery, thereby ensuring the safety of the battery. In addition, the thin film of the separator for secondary batteries can be achieved, so it is suitable for application in high-capacity / high-power batteries.

[0047] In one embodiment, the polypropylene microporous membrane may have a -5 Darcy or higher air permeability, specifically, the air permeability can be 1.3×10 -5 Darcy or above, 1.5×10 -5 Darcy or above, 3.0×10 -5 Darcy or less or 5.0×10 -5 In a specific embodiment, the air permeability may be 1.0×10 -5 Darcy to 5.0×10 -5Darcy or 1.3×10 -5 Darcy to 3.0×10 -5 By satisfying the air permeability within the above range, the battery can have excellent ion conductivity, and thus the charge and discharge characteristics of the battery can be improved due to the low internal resistance of the battery.

[0048] In one embodiment, in terms of mechanical strength and ionic conductivity, the porosity of the polypropylene microporous membrane may be 25-60%, specifically 30-50% or 35-39%, but is not limited thereto.

[0049] In one embodiment, the average pore size of the polypropylene microporous membrane can be 25-50nm, specifically 25-40nm, and more specifically 25-35nm. At this time, the average pore size can be measured by using a semi-dry method. In one embodiment, the average pore size can be measured according to ASTM F316-03 and using a pore size analyzer (porometer).

[0050] In one embodiment, the transverse shrinkage of the polypropylene microporous membrane measured after being placed at 150° C. for 1 hour may be 20% or less, 15% or less, or 13% or less, and the lower limit thereof is not particularly limited, but may be, for example, 0.1%, 0.5% or 1%. In a specific embodiment, the shrinkage may be 0.1-20%, 0.5-15% or 1-13%, but is not limited thereto.

[0051] In one embodiment, the melt fracture temperature of the polypropylene microporous membrane may be above 165° C. or above 170° C., and the upper limit thereof is not particularly limited, but for example may be 250° C. In a specific embodiment, the melt fracture temperature may be 165-250° C. or 170-250° C., but is not limited thereto.

[0052] In one embodiment, the polypropylene microporous membrane may be prepared by a wet process including a sequential biaxial stretching process, thereby providing a polypropylene microporous membrane simultaneously satisfying the physical properties as described above.

[0053] Specifically, the polypropylene microporous membrane can be prepared by extruding a mixture in which a diluent is dissolved in a polypropylene resin and sequentially biaxially stretching it to form a membrane and extracting the diluent from the membrane, and can be prepared by a wet method including a conventional sequential biaxial stretching process known to those skilled in the art, without limitation as long as a microporous membrane having the physical properties as described above can be prepared.

[0054] As an embodiment, the polypropylene microporous membrane that satisfies the physical properties as described above can be prepared by using a polypropylene resin having a viscosity-average molecular weight in a specific range or heat-treating at a specific temperature after extracting a diluent. Therefore, the polypropylene microporous membrane can have excellent puncture strength and transmittance while having significantly improved heat resistance at high temperatures. By including a polypropylene microporous membrane that satisfies the physical properties as described above, the present invention can provide a battery that can ensure excellent battery performance while having excellent high temperature thermal safety without smoke or fire of the battery in a high temperature hot box evaluation at 140°C.

[0055] As an embodiment, the viscosity average molecular weight of the polypropylene resin contained in the polypropylene microporous membrane may be 1×10 6 g / mol to 3×10 6 g / mol, specifically 1.2×10 6 g / mol to 2.5×10 6 g / mol, more specifically 1.3×10 6 g / mol to 2.2×10 6 g / mol.

[0056] As an embodiment, the heat treatment at a specific temperature after extracting the diluent may be to heat-stretch the film obtained after extracting the diluent at a first temperature, and to heat-set and heat-relax the heat-stretched film at a second temperature higher than the first temperature.

[0057] Hereinafter, the method for producing a polypropylene microporous membrane of the present invention will be described.

[0058] The method for preparing a polypropylene microporous membrane according to one embodiment may include the following steps: (a) extruding a polypropylene microporous membrane having a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of a polypropylene resin and a diluent are melt-kneaded to prepare a melt; (b) the melt is extruded to form a sheet; (c) the sheet is sequentially biaxially stretched in the longitudinal and transverse directions to form a film; (d) the diluent is extracted from the stretched film and dried; and (e) the dried film is heat-stretched at a temperature at which 2-5% of the crystals of the polypropylene resin melt, and the heat-stretched film is heat-set and heat-relaxed at a temperature at which 25-60% of the crystals of the polypropylene resin melt for heat treatment.

[0059] Hereinafter, each preparation step will be described.

[0060] First, step (a) is a step of preparing a melt by melt-kneading a mixture containing a polypropylene resin and a diluent through an extruder. In order to form holes, the mixture may contain a polypropylene resin and a diluent in a weight ratio of 10 to 60:90 to 40, specifically, a polypropylene resin and a diluent in a weight ratio of 20 to 40:80 to 60, but as long as the purpose of the present invention can be achieved, there is no particular limitation. When the weight ratio within the above range is met, the melt has sufficient fluidity, so that it is easy to be formed into a uniform sheet in the subsequent steps, and sufficient orientation is achieved during the stretching process, so that mechanical strength is easily ensured, so that problems such as rupture during the stretching process can be prevented.

[0061] The polypropylene resin may have a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol, preferably 1.2×10 6 g / mol to 2.5×10 6 g / mol, more preferably 1.3×10 6 g / mol to 2.2×10 6 g / mol of polypropylene or polypropylene having a viscosity average molecular weight in the above range. By having a viscosity average molecular weight in the above range, the desired physical properties of the present invention can be achieved. The battery using the microporous membrane satisfying the above physical properties has a low initial resistance, so it can have excellent battery performance while achieving excellent thermal safety in the hot box evaluation.

[0062] In one embodiment, the melting temperature of the polypropylene resin may be above 160° C., specifically 160-170° C., but is not necessarily limited thereto. The melting temperature of the polypropylene resin may be determined by differential scanning calorimetry (DSC).

[0063] In one embodiment, the diluent may be any organic compound that forms a single phase with the polypropylene resin at the extrusion temperature. For example, the diluent may be selected from aliphatic hydrocarbons or cyclic hydrocarbons such as nonane, decane, decalin, paraffin oil, and paraffin wax, phthalic acid esters such as dibutyl phthalate and dioctyl phthalate, C10-C20 fatty acids such as palmitic acid, stearic acid, oleic acid, linoleic acid, and linolenic acid, and C10-C20 fatty alcohols such as cetyl alcohol, stearyl alcohol, and oleyl alcohol, or a combination of two or more thereof. As a specific example of the diluent, paraffin oil having a kinetic viscosity of 20-200 cSt at 40°C can be cited, but it is not limited thereto. In addition, other diluents having the same or similar kinetic viscosity at an appropriate extrusion temperature can be used. For example, a diluent having a kinetic viscosity of 1-1000 cSt or 10-500 cSt can be used.

[0064] Furthermore, the mixture may further contain any one or more conventional additives for improving specific functions, such as an oxidation stabilizer, a UV stabilizer, and an antistatic agent, within a range that the properties of the microporous membrane are not significantly reduced.

[0065] Step (b) is a step of extruding the melt to form a sheet, which can be performed without limitation by methods known to those skilled in the art. As an example, the melt can be extruded through a T-die and cooled to a temperature of 10-80°C and formed into a sheet by casting or calendaring.

[0066] The longitudinal and transverse stretch ratios in step (c) can be independently 4 times or more, 6 times or more, 10 times or less, or 15 times or less, for example, 4 to 15 times or 6 to 10 times. By making the longitudinal and transverse stretch ratios satisfy the above ranges, a polypropylene microporous membrane having the desired physical properties of the present invention can be prepared.

[0067] The stretching in step (c) can be carried out by a sequential stretching method of a roller method or a tenter method, and can be carried out at a temperature ranging from 80°C lower than the melting temperature of polypropylene to the melting temperature of polypropylene. When the stretching is carried out at a temperature in the above range, the fluidity of the polypropylene resin for effective stretching can be ensured. In detail, uniform stretching is carried out throughout the sheet, and no rupture caused by stretching occurs, so that the stretching can be carried out stably, and therefore a high-quality microporous film having uniform air permeability, puncture strength and other physical properties can be prepared throughout the film. As an example, the stretching can be carried out at 100-170°C or 110-160°C, but is not limited thereto.

[0068] Step (d) is a step of extracting the diluent from the stretched film and drying it, which is performed by extracting the diluent inside the film with an organic solvent and drying the organic solvent in the film in which the diluent is replaced with the organic solvent. The organic solvent can be used without particular limitation as long as it can extract the diluent. Specifically, in terms of high extraction efficiency and rapid drying, the organic solvent can use methyl ethyl ketone, dichloromethane, hexane, etc.

[0069] Step (d) is preferably performed at a high temperature to increase the solubility of the diluent and the organic solvent, but may be performed at a temperature below 40° C. in view of safety caused by boiling of the organic solvent.

[0070] Step (e) is a step of heat-stretching the dried film at a temperature at which 2-5% of the crystals of the polypropylene resin melt using a roller method or a tenter method, and heat-setting and heat-relaxing the heat-stretched film at a temperature at which 25-60% of the crystals of the polypropylene resin melt for heat treatment. By heat-treating at the above temperature, the desired physical properties of the present invention can be achieved. The microporous membrane having such physical properties is suitable for application in high-power / high-capacity batteries. In detail, the battery to which the microporous membrane satisfying the above physical properties is applied has a low initial resistance, and therefore can have excellent battery performance while achieving excellent thermal safety in a hot box evaluation.

[0071] In one embodiment, the temperature at which the crystals of the polypropylene resin melt to a certain level can vary according to the viscosity average molecular weight and crystallinity of the polypropylene used. In the present invention, as the polypropylene resin for preparing the polypropylene microporous membrane, a polypropylene having a viscosity average molecular weight in the above range is used, so the hot stretching of the step (e) can be carried out at a temperature of 125-135°C, specifically, at a temperature of 127-133°C. In addition, the heat setting and heat relaxation of the step (e) can be carried out at a temperature of 155-165°C, specifically, at a temperature of 157-165°C.

[0072] The heat stretching in step (e) can be performed, for example, in the longitudinal or transverse direction. In terms of heat shrinkage, the heat stretching can be performed in the transverse direction to 120-160% or 130-150% of the width in the transverse direction before heat stretching.

[0073] The thermal relaxation in step (e) may be performed in the longitudinal direction or the transverse direction. In terms of the thermal shrinkage rate, the thermal relaxation may be performed in the transverse direction to 80-99% or 90-99% of the transverse width before thermal relaxation.

[0074] The present invention provides a diaphragm comprising the polypropylene microporous membrane as described above, which can be used for all known energy storage devices without any particular limitation. As a non-limiting example, a diaphragm for a lithium secondary battery can be cited.

[0075] Hereinafter, the embodiments and experimental examples will be specifically illustrated and described. However, the following embodiments and experimental examples are only illustrative of a part, and the technology described in this specification is not limited thereto.

[0076] [Measurement methods of physical properties]

[0077] 1. Viscosity average molecular weight (g / mol)

[0078] The viscosity average molecular weight (Mv) of polypropylene was measured at 165° C. using the Crystex QC model of Polymerchar according to ISO 16152:2022 and calculated by the Margolies equation of the following mathematical formula 1. The intrinsic viscosity was measured by using 1,2,4-trichlorobenzene (TCB) as a solvent.

[0079] [Mathematical formula 1]

[0080] Mv=5.37×10 4 ×[η] 1.49

[0081] 2. Thickness of microporous membrane (μm)

[0082] The thickness of the microporous film was measured using a contact thickness gauge with a thickness accuracy of 0.1 μm. The measurement was performed using a TESA Mu-Hite Electronic Height Gauge manufactured by TESA and a measuring pressure of 0.63 N.

[0083] 3.Puncture strength (N / μm)

[0084] The puncture strength was measured by installing a pin tip with a diameter of 1.0 mm and a radius of curvature of 0.5 mm in a Universal Test Machine (UTM) 3345 from INSTRON and pressing the microporous membrane at a speed of 120 mm / min. At this time, the puncture strength was calculated by dividing the load (N) at the time of rupture of the microporous membrane by the thickness (μm) of the microporous membrane.

[0085] 4. Air permeability (Darcy)

[0086] The air permeability is measured by using a pore size analyzer (Porometer; CFP-1500-AEL of Porous Materials, Inc. (PMI)). Generally, the air permeability is expressed as a Gurley number, but the Gurley number does not correct the effect of thickness, so it is difficult to know the relative permeability according to the pore structure. In order to solve this problem, the air permeability of the present invention is measured by using the Darcy permeability constant calculated by the following mathematical formula 2. Nitrogen is used as the gas, and the average value of the Darcy permeability constant measured in the region of 100-200 psi is calculated.

[0087] [Mathematical formula 2]

[0088] Darcy transmittance constant (C) = (8F·T·V) / (πD 2 (P 2 -1))

[0089] F = flow rate (cc / cm2)

[0090] T = thickness of sample (mm)

[0091] V = viscosity of the gas (at 20°C, N2 is 0.185 cP)

[0092] D = diameter of sample (mm)

[0093] P = Pressure (psi)

[0094] 5. Transverse shrinkage (%)

[0095] A 15 cm×15 cm microporous film with longitudinal and transverse directions marked with a length of 10 cm was placed in an oven (DKN612 manufactured by Yamato) at 150° C. for 1 hour, and then the change in length was measured and the transverse shrinkage was calculated using the following formula 3.

[0096] [Mathematical formula 3]

[0097] Transverse shrinkage (%) = {(transverse length before heating - transverse length after heating) / transverse length before heating} × 100

[0098] 6. Average pore size (nm)

[0099] The average pore size was measured according to ASTM F316-03 using a porometer (PMI CFP-1500-AEL). The average pore size was measured by a semi-dry method (ASTM F316-03), and Galwick liquid (surface tension: 15.9 dyne / cm) provided by PMI was used to measure the pore size.

[0100] 7. Melt Fracture Temperature

[0101] For the melt fracture temperature of microporous membrane, Figure 2 As shown, a microporous membrane 12 (5 cm x 5 cm) was fixed on a plate with a polyimide tape 14. Figure 1 The microporous film is placed on a frame 10 (outer profile: 7.5 cm×7.5 cm, inner diameter: 2.5 cm×2.5 cm) shown in the figure, and then placed in a hot air oven (convection oven) maintained at a set temperature for 10 minutes, and then the microporous film is measured by observing whether it is broken. The highest temperature at which the microporous film does not break even after 10 minutes is defined as the melt fracture temperature.

[0102] 8. Initial resistance test

[0103] The initial resistance test was performed by using a battery assembled using a polypropylene microporous membrane as a separator. Specifically, the positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material were wound together with the prepared microporous membrane and placed in an aluminum soft pack, and then injected with an electrolyte containing 1M lithium hexafluorophosphate (LiPF6) dissolved in a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2 and sealed, thereby assembling a battery with a capacity of 2Ah. After aging and degassing the assembled battery, it was fully charged to 4.2V and the initial resistance (mΩ) was measured.

[0104] When the initial resistance is 50 mΩ or less, it is confirmed that 20% or more of the capacity is maintained in a discharge test at a 2C rate (C-rate), so the initial resistance value becomes an evaluation index for power characteristics.

[0105] 9. Hot box evaluation

[0106] The hot box evaluation is carried out by using a battery assembled using a polypropylene microporous membrane as a separator. Specifically, the positive electrode using NCM 622 (Ni: Co: Mn = 6: 2: 2) as the active material and the negative electrode using graphite carbon as the active material are wound together with the prepared microporous membrane and placed in an aluminum soft pack, and then injected into a solution containing ethylene carbonate, ethyl methyl carbonate and diethyl carbonate in a volume ratio of 3: 5: 2. 1M of lithium hexafluorophosphate (LiPF6) is dissolved in the electrolyte and sealed to assemble a battery with a capacity of 2Ah. After aging and degassing, the assembled battery is fully charged to 4.2V, placed in an oven, heated at 5°C / min, and placed for 30 minutes after reaching 140°C to measure the changes in the battery.

[0107] If the battery emits smoke or catches fire after being placed at 140°C for 30 minutes, it is judged as a failure. If the battery voltage / current does not change and no smoke or fire occurs, it is judged as a pass.

[0108] 10. Analysis of thermal properties of films

[0109] The phenomenon of crystal melting of the polypropylene resin according to temperature was analyzed using a differential scanning calorimeter (DSC) Discovery DSC250 manufactured by TA Instruments under the conditions of a sample weight of 5 mg and a scanning speed of 10° C. / min.

[0110] The temperature at which n% of the crystals of polypropylene resin melt (T n ) is measured by calculating the temperature at a position representing n% of the total heat of fusion. In the present invention, the temperatures T2, T5, T6, T7, T8, T9, T10, T11, T12, T13, T14, T15, T16, T17, T18, T19, T20, T21, T22, T30, T31, T40, T52, T63, T74, T85, T96, T10, T11, T12, T13, T14, T15 25 and T 60 The measurements were performed respectively and are shown in Table 1.

[0111] 11. Porosity (%)

[0112] The porosity is calculated using the following mathematical formula: Specifically, a sample with a width of A cm (e.g., 30 cm), a length of B cm (e.g., 20 cm), and a thickness of T cm (e.g., 0.0003-0.002 cm) is prepared and the mass is measured, and the porosity is calculated by the ratio of the mass of the same volume of resin to the mass of the microporous membrane.

[0113] Porosity (%) = 100 × {1-M / (A × B × T × ρ)}

[0114] In the above formula, M is the mass of the microporous membrane (g), and ρ is the density of the polypropylene resin forming the microporous membrane (g / cm 3 ).

[0115] <Example 1>

[0116] Using a twin-screw extruder, a 30:70 weight ratio of 1.5×10 6 A mixture of a polypropylene resin having a melting temperature of 165° C. and a paraffin oil having a dynamic viscosity of 80 cSt at 40° C. was melt-kneaded to prepare a melt. The melting temperature was measured using a differential scanning calorimeter (DSC) Discovery DSC250 provided by TA Instruments, and was measured under the conditions of a sample weight of 5 mg and a scanning speed of 10° C. / min.

[0117] The melt was continuously extruded through a T-die, and a sheet having a width of 300 mm and an average thickness of 1100 μm was prepared using a casting roll set at 30° C. The sheet was longitudinally stretched to 6 times by a roll method at a stretching temperature of 115° C., then guided to a tenter and transversely stretched to 6 times at a stretching temperature of 140° C.

[0118] Paraffin oil was extracted from the film after longitudinal stretching and transverse stretching at 25°C using dichloromethane, and the film from which the paraffin oil had been extracted was dried at 60°C.

[0119] The dried film was heat-stretched to 145% in the transverse direction at 130° C., which is a temperature at which 3% of the crystals of the polypropylene resin melt, using a tenter-type heat-setting device. Then, it was heat-set for 10 seconds at 160° C., which is a temperature at which 35% of the crystals of the polypropylene resin melt, and heat-relaxed (shrunk) to 93% of the width before the heat-relaxation process, thereby preparing a microporous film with a thickness of 12.8 μm.

[0120] The physical properties of the finally prepared microporous membrane and the performance of the battery using the microporous membrane are shown in Table 2 below.

[0121] <Example 2 to Example 3 and Comparative Example 1 to Comparative Example 6>

[0122] A polypropylene microporous membrane was prepared by the same method as in Example 1, except that the viscosity average molecular weight (PP Mv) of the polypropylene resin used, the longitudinal / transverse stretching ratio and the heat treatment temperature were changed to the conditions described in Table 1. The physical properties of the finally prepared microporous membrane and the performance of the battery using the microporous membrane are shown in Table 2 below.

[0123] [Table 1]

[0124]

[0125] [Table 2]

[0126]

[0127]

[0128] Referring to Tables 1 and 2, the microporous membrane of the embodiment satisfies all the physical properties expected by the present invention, so the initial resistance of the battery using the microporous membrane is below 50 mΩ and passes the hot box evaluation, thus achieving excellent battery performance and safety in a high temperature environment.

[0129] The microporous membrane of Comparative Example 1 was prepared by using a porous membrane having a thickness of less than 1.0×10 6 g / mol, the polypropylene resin is prepared, as a result, the entanglement between chains is less, and thus the film is broken during the heat stretching in the heat treatment step.

[0130] The microporous membrane of Comparative Example 2 was prepared by using a microporous membrane having a thickness of more than 3.0×10 6 g / mol of polypropylene resin with a viscosity average molecular weight of 1.3 g / mol is used for preparation. As a result, the mixing between the resin and the diluent is uneven, so a sheet with uneven thickness is obtained, and there is a disadvantage of uneven product quality.

[0131] For the microporous membranes of Comparative Examples 3 and 4, the heat stretching in the heat treatment step was performed at a temperature higher than the temperature (T5) at which 5% of the crystals of the membrane introduced into the heat setting device melted, and as a result, the air permeability, porosity and average pore size were less than 1.0×10 -5 Darcy, less than 25%, less than 24nm, so although the thermal safety of the battery using the microporous membrane is the same as that of the present invention, the initial resistance is more than 55mΩ, which has the disadvantage of poor battery performance.

[0132] For the microporous membrane of Comparative Example 5, the heat setting and heat relaxation of the heat treatment step were performed at a temperature (T 25 ) is carried out at a lower temperature. As a result, although the physical properties such as air permeability are met, a lateral shrinkage rate of 25.1% is exhibited. Therefore, the battery using this microporous membrane has the disadvantage of greatly reduced safety in a high temperature environment.

[0133] For the microporous membrane of Comparative Example 6, the heat setting and heat relaxation of the heat treatment step were performed at a temperature lower than the temperature at which 60% of the crystals of the membrane introduced into the heat setting device melted (T 60 ) at a higher temperature, the results showed that the air permeability, porosity and average pore size were less than 0.2×10 -5Darcy, less than 16%, less than 19 nm, so although the thermal safety of the battery using the microporous membrane is the same as that of the present invention, the initial resistance is 65 mΩ, which has the disadvantage of poor battery performance.

[0134] As described above, in this specification, the present invention is described through specific content and limited embodiments, but this is only provided to help a more comprehensive understanding of the present invention. The present invention is not limited to the above embodiments, and those skilled in the art can make various modifications and variations from these descriptions.

Claims

1. A polypropylene microporous membrane, the polypropylene microporous membrane comprising a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of polypropylene, the thickness of the polypropylene microporous membrane is 3-30 μm, the puncture strength is above 0.20 N / μm, and the air permeability is 1.0×10 -5 Darcy or above, the porosity is 25-60%, the average pore size is 25-50nm, and the lateral shrinkage measured after being placed at 150°C for 1 hour is less than 20%.

2. The polypropylene microporous membrane according to claim 1, wherein The melt fracture temperature of the polypropylene microporous membrane is above 165°C.

3. The polypropylene microporous membrane according to claim 1, wherein The transverse shrinkage of the polypropylene microporous membrane is less than 15%.

4. The polypropylene microporous membrane according to claim 1, wherein The polypropylene microporous membrane is prepared by a wet method including a sequential biaxial stretching process.

5. A method for preparing a polypropylene microporous membrane, comprising the following steps: (a) A mixture containing a viscosity average molecular weight of 1×10 6 g / mol to 3×10 6 g / mol of a polypropylene resin and a diluent are melt-kneaded to prepare a melt; (b) extruding the melt to form a sheet; (c) sequentially biaxially stretching the sheet in the longitudinal and transverse directions to form a film; (d) extracting the diluent from the stretched film and drying it; and (e) heat-stretching the dried film at a temperature at which 2-5% of the crystals of the polypropylene resin melt, and heat-setting and heat-relaxing the heat-stretched film at a temperature at which 25-60% of the crystals of the polypropylene resin melt for heat treatment.

6. The method for preparing a polypropylene microporous membrane according to claim 5, wherein: The heat stretching in step (e) is performed at a temperature of 125-135°C.

7. The method for preparing a polypropylene microporous membrane according to claim 5, wherein: The heat setting and heat relaxation of step (e) are performed at a temperature of 155-165°C. 8 . A separator comprising the polypropylene microporous membrane according to claim 1 .

9. A microporous membrane for a secondary battery separator, the microporous membrane for a secondary battery separator comprising a 6 g / mol to 3×10 6 g / mol of polypropylene, the thickness of the microporous membrane for the secondary battery separator is 3-30 μm, the puncture strength is above 0.20 N / μm, and the air permeability is 1.0×10 -5 Darcy or above, the porosity is 25-60%, the average pore size is 25-50nm, and the lateral shrinkage measured after being placed at 150°C for 1 hour is less than 20%.

10. The microporous membrane for a secondary battery separator according to claim 9, wherein The microporous film for a secondary battery separator has a melt fracture temperature of 165° C. or higher. 11 . A polypropylene microporous membrane, prepared by the method for preparing a polypropylene microporous membrane according to any one of claims 5 to 7. 12 . A secondary battery comprising a positive electrode, a negative electrode and the separator according to claim 8 .