Preparation method and application of corrosion-resistant on-bridge tube box bracket
By using composite materials of polypropylene resin, thermoplastic polyurethane elastomer, passivation fiber and nanocarbon powder, the corrosion-resistant bridge tube box bracket is prepared, and the problem of insufficient tensile strength and corrosion resistance of the bridge tube box bracket is solved, and the problem of insufficient tensile strength and corrosion resistance of the bridge tube box bracket is realized. Efficient material performance improvement.
Patent Information
- Application Number
- CN202411245229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
The bridge pipe box bracket needs to have high tensile strength and corrosion resistance to resist loads and harsh environment erosion. The existing technology is difficult to meet both needs at the same time.
The corrosion-resistant bridge upper tube box bracket is prepared by intensive and extruded processes using polypropylene resin, thermoplastic polyurethane elastomer, passivation fiber and nanocarbon powder composite materials. The passivation fibers are enhanced by high-temperature firing and pickling treatment. Capability, nanocarbon powder improves the tensile strength and corrosion resistance of the material by forming physical crosslinking points.
The tensile strength and corrosion resistance of the composite material are significantly improved, and the tensile strength loss rate of the material in salt spray environment is low, extending its service life.
Smart Images

Figure CN118994784A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite material brackets, and particularly relates to a preparation method and application of a corrosion-resistant bridge pipe box bracket. Background Art
[0002] The bridge pipe box bracket is an important part of the bridge structure. It is mainly used to support and fix the pipeline facilities on the bridge, such as drainage, water supply, gas, electricity and communication pipelines, etc. The design, material selection and manufacturing process of these brackets are crucial to the safe operation of the bridge.
[0003] The pipe box bracket on the bridge needs to have sufficient tensile strength to withstand various loads and environmental influences, such as wind loads, temperature changes, and earthquakes. At the same time, due to the high humidity on the bridge, the pipe box bracket on the bridge also needs to have good corrosion resistance to resist erosion in harsh environments (such as moisture and salt spray), thereby enhancing environmental adaptability and extending service life. Summary of the invention
[0004] In order to solve the problems existing in the background technology, the present invention provides a preparation method and application of a corrosion-resistant bridge pipe box bracket, which improves the tensile strength of the product and the corrosion resistance.
[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for preparing a corrosion-resistant bridge pipe box bracket, comprising the following steps:
[0006] S1. Mix 40-45 parts of polypropylene resin, 9-11 parts of thermoplastic polyurethane elastomer, 3-4 parts of copolyester hot melt rubber particles, 1-1.5 parts of antioxidant and 0.5-1 parts of lubricant by weight to obtain a base material;
[0007] S2, putting the base material obtained in S1 into an internal mixer, and then putting 7-9 parts of passivated fiber and 4-5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 40-50r / min, the internal mixing temperature is 170-180°C, and the internal mixing time is 8-10min; then, the rotor speed of the internal mixer is 55-60r / min, the internal mixing temperature is 200-215°C, and the internal mixing time is 4-6min; finally, the rotor speed of the internal mixer is 65-70r / min, the internal mixing temperature is 240-245°C, and the internal mixing time is 1-2min; to obtain the internal mixing material;
[0008] S3, feeding the mixed material obtained in S2 into a twin-screw extruder, and extruding and granulating at 215-245° C. to obtain a composite material;
[0009] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 225-245°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0010] Furthermore, the preparation method of the passivated fiber is as follows:
[0011] A1. Put the glass fiber into a high temperature resistance furnace, burn it at 300-340℃ for 30-40min, discharge it, and cool it naturally to room temperature to obtain the fired fiber;
[0012] A2. Immerse the fired fiber obtained in A1 in an acid washing solution, perform ultrasonic cleaning for 35-45 minutes, filter out, wash with water until neutral, and dry to obtain a passivated fiber.
[0013] Furthermore, in A1, the specification of the glass fiber is 3MM.
[0014] Furthermore, in A2, the pickling solution is a hydrofluoric acid solution with a mass concentration of 5-6%.
[0015] Furthermore, in A2, the ultrasonic cleaning frequency is 50-70 KHz.
[0016] Furthermore, the average particle size of the nano carbon powder is 20 nm.
[0017] Furthermore, the antioxidant includes a phenolic antioxidant or an amine antioxidant.
[0018] Furthermore, the lubricant includes a fatty acid lubricant or a fatty acid ester lubricant.
[0019] In a second aspect, the present invention provides an application of a corrosion-resistant bridge pipe box bracket, wherein the corrosion-resistant bridge pipe box bracket is prepared by the above-mentioned preparation method, and the corrosion-resistant bridge pipe box bracket is used to support and fix pipeline facilities on the bridge.
[0020] This application has the following beneficial effects:
[0021] 1. The passivated fiber of the present invention is made of glass fiber after high-temperature calcination and acid washing. The glass fiber itself has higher strength and modulus than most resins. After sintering and acid washing, it can enhance the bonding ability with polypropylene resin, further improving the tensile strength and corrosion resistance of the composite material.
[0022] The urethane groups in the thermoplastic polyurethane elastomer can form a stronger physical or chemical bond with the functional groups on the surface of the nano-carbon powder, making it a material with a strong anchoring ability for the nano-carbon powder in the hot melt state, effectively preventing the nano-carbon powder from being adsorbed by the passivated fiber, thereby avoiding a negative impact on the bonding effect between the passivated fiber and the polypropylene resin.
[0023] At the same time, nano-carbon powder has a very high specific surface area, which enables it to form a large number of physical cross-linking points in the resin matrix. These cross-linking points can effectively transfer stress, so that the material can better distribute internal stress when subjected to external force, reduce local stress concentration, and thus improve the overall tensile strength of the material; nano-carbon powder has high chemical stability and is not easy to react with corrosive media, and evenly dispersed nano-carbon powder can effectively fill the tiny pores and defects in the matrix and reduce the penetration path of corrosive media. This densification effect can significantly improve the corrosion resistance of the material.
[0024] 2. Thermoplastic polyurethane elastomer has high elasticity and can absorb and disperse energy when subjected to force, reduce stress concentration inside the material, avoid the generation and expansion of cracks, and thus achieve the effect of improving tensile strength and corrosion resistance.
[0025] Copolyester hot melt particles can form a stronger interface bond with polypropylene resin, thermoplastic polyurethane elastomer, passivated fiber and nano carbon powder, thereby improving the tensile strength and corrosion resistance of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 , a comparative trend chart of tensile strength test data of products obtained in Examples 1-5 of the present invention and Comparative Examples 1-5;
[0027] Figure 2 , a trend chart comparing the tensile strength loss rate test data of the products obtained in Examples 1-5 of the present invention and Comparative Examples 1-5 after being treated with salt spray corrosion. DETAILED DESCRIPTION
[0028] The present application is further described in detail below with reference to the embodiments.
[0029] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.
[0030] Example 1: (1) Preparation of passivated fibers, the preparation method is as follows:
[0031] A1. Put the glass fiber into a high temperature resistance furnace, burn it at 320℃ for 35min, discharge it, and cool it naturally to room temperature to obtain the fired fiber.
[0032] A2. Immerse the fired fiber obtained in A1 in an acid washing solution, ultrasonically clean it for 40 minutes, filter it out, wash it with water until it is neutral, and dry it to obtain a passivated fiber.
[0033] Among them, the glass fiber (AB-61), specification 3MM, was purchased from Shijiazhuang Anbai Mining Co., Ltd. The pickling solution was a hydrofluoric acid solution with a mass concentration of 6%; the mass ratio of the fired fiber to the pickling solution was 1:5. The ultrasonic cleaning frequency was 60KHz.
[0034] (2) A method for preparing a corrosion-resistant bridge pipe box bracket, comprising the following steps:
[0035] S1. According to weight, 44 parts of polypropylene resin, 10 parts of thermoplastic polyurethane elastomer, 3.5 parts of copolyester hot melt rubber particles, 1.2 parts of antioxidant and 0.8 parts of lubricant are mixed to obtain a base material. Among them, polypropylene resin (T30S) is from Daqing Refining and Chemical, purchased from Ningbo Jinchi Plastic Co., Ltd. BASF 1180A thermoplastic polyurethane elastomer from Germany was purchased from Shanghai Enyan Engineering Plastics Co., Ltd. Copolyester PES hot melt rubber particles were purchased from Qidong Huading Hot Melt Adhesive Co., Ltd. The antioxidant is BASF BASFIrganox EasyGaLes 1010 antioxidant. The lubricant is tall oil fatty acid, purchased from Dezhou Chengyan New Materials Co., Ltd.
[0036] S2, put the base material obtained in S1 into an internal mixer, and then put 8 parts of passivated fiber and 4.5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 45r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9min; then, the rotor speed of the internal mixer is 57r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5min; finally, the rotor speed of the internal mixer is 68r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5min; and the internal mixing material is obtained. Among them, the nano carbon powder (average particle size 20nm, purity 99.9%) was purchased from Shanghai Yaotian New Material Technology Co., Ltd.
[0037] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0038] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0039] The corrosion-resistant bridge pipe box bracket prepared by the above preparation method is suitable for supporting and fixing pipeline facilities on the bridge, such as drainage, water supply, gas, electricity and communication pipelines.
[0040] Example 2: The difference between this example and Example 1 is that: (1) a passivated fiber is prepared by the following method:
[0041] A1. Put the glass fiber into a high temperature resistance furnace, burn it at 300℃ for 30min, discharge it, and cool it naturally to room temperature to obtain the fired fiber.
[0042] A2. Immerse the fired fiber obtained in A1 in an acid washing solution, ultrasonically clean it for 35 minutes, filter it out, wash it with water until it is neutral, and dry it to obtain a passivated fiber.
[0043] Example 3: The difference between this example and Example 1 is that: (1) a passivated fiber is prepared by the following method:
[0044] A1. Put the glass fiber into a high temperature resistance furnace, burn it at 340℃ for 40min, discharge it, and cool it naturally to room temperature to obtain the fired fiber.
[0045] A2. Immerse the fired fiber obtained in A1 in an acid washing solution, perform ultrasonic cleaning for 45 minutes, filter out, wash with water until neutral, and dry to obtain a passivated fiber.
[0046] Embodiment 4: The difference between this embodiment and embodiment 1 is that: (2) A method for preparing a corrosion-resistant bridge pipe box bracket comprises the following steps:
[0047] S1. Mix 40 parts of polypropylene resin, 9 parts of thermoplastic polyurethane elastomer, 3 parts of copolyester hot melt rubber particles, 1 part of antioxidant and 0.5 parts of lubricant by weight to obtain a base material.
[0048] S2. Put the base material obtained in S1 into an internal mixer, and then put 7 parts of passivated fiber and 4 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 40r / min, the internal mixing temperature is 170°C, and the internal mixing time is 8min; then, the rotor speed of the internal mixer is 55r / min, the internal mixing temperature is 200°C, and the internal mixing time is 4min; finally, the rotor speed of the internal mixer is 65r / min, the internal mixing temperature is 240°C, and the internal mixing time is 1min; the internal mixing material is obtained.
[0049] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0050] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0051] Embodiment 5: The difference between this embodiment and embodiment 1 is that: (2) A method for preparing a corrosion-resistant bridge pipe box bracket comprises the following steps:
[0052] S1. Mix 45 parts of polypropylene resin, 11 parts of thermoplastic polyurethane elastomer, 4 parts of copolyester hot melt rubber particles, 1.5 parts of antioxidant and 1 part of lubricant by weight to obtain a base material.
[0053] S2. Put the base material obtained in S1 into an internal mixer, and then put 9 parts of passivated fiber and 5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 50r / min, the internal mixing temperature is 180°C, and the internal mixing time is 10min; then, the rotor speed of the internal mixer is 60r / min, the internal mixing temperature is 215°C, and the internal mixing time is 6min; finally, the rotor speed of the internal mixer is 70r / min, the internal mixing temperature is 245°C, and the internal mixing time is 2min; and the internal mixing material is obtained.
[0054] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0055] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0056] Comparative Example 1: The difference between this comparative example and Example 1 is that the thermoplastic polyurethane elastomer, copolyester hot melt rubber particles, passivated fibers and nano-carbon powder are deleted.
[0057] Specifically, a method for preparing a corrosion-resistant bridge pipe box bracket includes the following steps:
[0058] S1. Mix 57.5 parts of polypropylene resin, 1.2 parts of antioxidant and 0.8 parts of lubricant by weight to obtain a base material.
[0059] S2. The base material obtained in S1 is put into an internal mixer; first, the rotor speed of the internal mixer is 45 r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9 min; then, the rotor speed of the internal mixer is 57 r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5 min; finally, the rotor speed of the internal mixer is 68 r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5 min; and the internal mixing material is obtained.
[0060] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0061] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0062] Comparative Example 2: The difference between this comparative example and Example 1 is that the thermoplastic polyurethane elastomer, copolyester hot melt particles and nano-carbon powder are deleted.
[0063] Specifically, a method for preparing a corrosion-resistant bridge pipe box bracket includes the following steps:
[0064] S1. Mix 57.5 parts of polypropylene resin, 1.2 parts of antioxidant and 0.8 parts of lubricant by weight to obtain a base material.
[0065] S2. Put the base material obtained in S1 into an internal mixer, and then put 8 parts of the passivated fiber into the internal mixer; first, the rotor speed of the internal mixer is 45r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9min; then, the rotor speed of the internal mixer is 57r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5min; finally, the rotor speed of the internal mixer is 68r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5min; the internal mixing material is obtained.
[0066] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0067] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0068] Comparative Example 3: The difference between this comparative example and Example 1 is that the copolyester hot melt adhesive particles and nano carbon powder are deleted.
[0069] Specifically, a method for preparing a corrosion-resistant bridge pipe box bracket includes the following steps:
[0070] S1. Mix 47.5 parts of polypropylene resin, 10 parts of thermoplastic polyurethane elastomer, 1.2 parts of antioxidant and 0.8 parts of lubricant by weight to obtain a base material.
[0071] S2. Put the base material obtained in S1 into an internal mixer, and then put 8 parts of the passivated fiber into the internal mixer; first, the rotor speed of the internal mixer is 45r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9min; then, the rotor speed of the internal mixer is 57r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5min; finally, the rotor speed of the internal mixer is 68r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5min; the internal mixing material is obtained.
[0072] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0073] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0074] Comparative Example 4: The difference between this comparative example and Example 1 is that the thermoplastic polyurethane elastomer and copolyester hot melt rubber particles are deleted.
[0075] Specifically, a method for preparing a corrosion-resistant bridge pipe box bracket includes the following steps:
[0076] S1. Mix 57.5 parts of polypropylene resin, 1.2 parts of antioxidant and 0.8 parts of lubricant by weight to obtain a base material.
[0077] S2. Put the base material obtained in S1 into an internal mixer, and then put 8 parts of passivated fiber and 4.5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 45r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9min; then, the rotor speed of the internal mixer is 57r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5min; finally, the rotor speed of the internal mixer is 68r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5min; the internal mixing material is obtained.
[0078] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0079] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0080] Comparative Example 5: The difference between this comparative example and Example 1 is that the copolyester hot melt adhesive particles are deleted.
[0081] Specifically, a method for preparing a corrosion-resistant bridge pipe box bracket includes the following steps:
[0082] S1. Mix 47.5 parts of polypropylene resin, 10 parts of thermoplastic polyurethane elastomer, 1.2 parts of antioxidant and 0.8 parts of lubricant by weight to obtain a base material.
[0083] S2. Put the base material obtained in S1 into an internal mixer, and then put 8 parts of passivated fiber and 4.5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 45r / min, the internal mixing temperature is 176°C, and the internal mixing time is 9min; then, the rotor speed of the internal mixer is 57r / min, the internal mixing temperature is 207°C, and the internal mixing time is 5min; finally, the rotor speed of the internal mixer is 68r / min, the internal mixing temperature is 242°C, and the internal mixing time is 1.5min; the internal mixing material is obtained.
[0084] S3. The mixed material obtained in S2 is fed into a twin-screw extruder, and the temperatures of each zone of the twin-screw extruder are set to 215°C, 220°C, 230°C, 240°C, 240°C, 245°C, 240°C, 230°C, and 220°C in sequence, the die head temperature is 210°C, and the screw speed is 120rpm, and extrusion granulation is carried out to obtain a composite material.
[0085] S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 240°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
[0086] Test example: Test object: Composite materials / products were prepared according to Examples 1-5 and Comparative Examples 1-5.
[0087] Test items: 1. Tensile strength; 2. Corrosion resistance.
[0088] Test basis / method: 1. Tensile strength: Tested in accordance with GB / T1040-1992;
[0089] 2. Corrosion resistance: It is characterized by the tensile strength loss rate. The smaller the tensile strength loss rate, the stronger the corrosion resistance. Tensile strength loss rate = (tensile strength measured on the sample before salt spray treatment - tensile strength measured on the sample after salt spray treatment) / tensile strength measured on the sample before salt spray treatment * 100%. Among them, the sample before salt spray treatment and the sample after salt spray treatment are two different samples of the same test object. Salt spray treatment method: The sample is exposed and placed in a salt spray test chamber at an inclination angle of 15°-30°. The salt solution in the salt spray test chamber is a sodium chloride solution with a mass fraction of 8%, the temperature is 45°C, the relative humidity is 95%, and the placement (treatment) time is 7 days.
[0090] Test results: See Table 1.
[0091] Table 1. Test data of the experimental example
[0092]
[0093] Result analysis: Analyze examples 1-5 and combine the data in Table 1 and Figure 1-2It can be seen that the tensile strength of the composite material / product prepared by the present invention is as high as 147.6 MPa or more, and the corrosion resistance is strong. The tensile strength loss rate after 7 days of salt spray treatment is as low as less than 3.97%.
[0094] Analyze Example 1 and Comparative Examples 1-5 and combine the data in Table 1 and Figure 1 The specific analysis is as follows: From the comparison between Comparative Example 1 and Comparative Example 2, it can be seen that adding passivated fibers to the base polypropylene resin can improve the tensile strength of the obtained composite material / product; combined with the comparison with Comparative Example 3, it can be seen that adding thermoplastic polyurethane elastomer can further improve the tensile strength of the obtained composite material / product.
[0095] From the comparison of Comparative Examples 2 and 4, it can be seen that when only the base polypropylene resin and the passivated fiber are present, the addition of nano-carbon powder will cause the tensile strength of the obtained composite material / product to decrease instead of increase; from the comparison of Comparative Examples 3 and 5, it can be seen that when the base polypropylene resin, the passivated fiber and the thermoplastic polyurethane elastomer are present, the addition of nano-carbon powder can improve the tensile strength of the obtained composite material / product. This shows that in this system, when the thermoplastic polyurethane elastomer is present, the addition of nano-carbon powder can play a role in improving the tensile strength; if there is no participation of the thermoplastic polyurethane elastomer, the addition of nano-carbon powder will lead to a decrease in tensile strength.
[0096] From the comparison between Example 1 and Comparative Example 5, it can be seen that the addition of copolyester hot melt adhesive particles can improve the tensile strength of the obtained composite material / product.
[0097] Analyze Example 1 and Comparative Examples 1-5 and combine the data in Table 1 and Figure 2 The specific analysis content is as follows: From the comparison between Comparative Example 1 and Comparative Example 2, it can be seen that adding passivated fiber to the base polypropylene resin can improve the (salt spray) corrosion resistance of the obtained composite material / product; combined with the comparison with Comparative Example 3, it can be seen that adding thermoplastic polyurethane elastomer can further improve the (salt spray) corrosion resistance of the obtained composite material / product.
[0098] From the comparison of Comparative Examples 2 and 4, it can be seen that when only the base polypropylene resin and the passivation fiber are present, the addition of nano-carbon powder will cause the (salt spray) corrosion resistance of the obtained composite material / product to decrease instead of increase; from the comparison of Comparative Examples 3 and 5, it can be seen that when the base polypropylene resin, the passivation fiber and the thermoplastic polyurethane elastomer are present, the addition of nano-carbon powder can improve the (salt spray) corrosion resistance of the obtained composite material / product. This shows that in this system, when the thermoplastic polyurethane elastomer is present, the addition of nano-carbon powder can play a role in improving the (salt spray) corrosion resistance; if there is no participation of the thermoplastic polyurethane elastomer, the addition of nano-carbon powder will lead to a decrease in the (salt spray) corrosion resistance.
[0099] The inventors said that this is because the hot-melt polypropylene resin has insufficient anchoring ability for nano-carbon powder, which causes the added nano-carbon powder to be easily adsorbed by the passivated fibers. This adsorption affects the bonding between the passivated fibers and the polypropylene resin, resulting in a decrease in the tensile strength and corrosion resistance of the resulting composite material / product.
[0100] From the comparison between Example 1 and Comparative Example 5, it can be seen that the addition of copolyester hot melt particles can improve the (salt spray) corrosion resistance of the obtained composite material / product.
[0101] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0102] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a corrosion-resistant bridge pipe box bracket, characterized in that: The steps include: S1. Mix 40-45 parts of polypropylene resin, 9-11 parts of thermoplastic polyurethane elastomer, 3-4 parts of copolyester hot melt rubber particles, 1-1.5 parts of antioxidant and 0.5-1 parts of lubricant by weight to obtain a base material; S2, putting the base material obtained in S1 into an internal mixer, and then putting 7-9 parts of passivated fiber and 4-5 parts of nano carbon powder into the internal mixer; first, the rotor speed of the internal mixer is 40-50r / min, the internal mixing temperature is 170-180°C, and the internal mixing time is 8-10min; then, the rotor speed of the internal mixer is 55-60r / min, the internal mixing temperature is 200-215°C, and the internal mixing time is 4-6min; finally, the rotor speed of the internal mixer is 65-70r / min, the internal mixing temperature is 240-245°C, and the internal mixing time is 1-2min; to obtain the internal mixing material; S3, feeding the mixed material obtained in S2 into a twin-screw extruder, and extruding and granulating at 215-245° C. to obtain a composite material; S4. The composite material obtained in S3 is fed into an injection molding machine, melted at 225-245°C, injected into a mold, and cooled to obtain a corrosion-resistant bridge pipe box bracket.
2. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 1, characterized in that: The preparation method of the passivated fiber is as follows: A1. Put the glass fiber into a high temperature resistance furnace, burn it at 300-340℃ for 30-40min, discharge it, and cool it naturally to room temperature to obtain the fired fiber; A2. Immerse the fired fiber obtained in A1 in an acid washing solution, perform ultrasonic cleaning for 35-45 minutes, filter out, wash with water until neutral, and dry to obtain a passivated fiber.
3. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 2 is characterized in that: In A1, the specification of the glass fiber is 3MM.
4. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 2, characterized in that: In A2, the pickling solution is a hydrofluoric acid solution with a mass concentration of 5-6%.
5. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 2, characterized in that: In A2, the ultrasonic cleaning frequency is 50-70KHz.
6. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 1, characterized in that: The average particle size of the nano carbon powder is 20 nm.
7. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 1, characterized in that: The antioxidant includes a phenolic antioxidant or an amine antioxidant.
8. The method for preparing the corrosion-resistant bridge pipe box bracket according to claim 1, characterized in that: The lubricant includes a fatty acid lubricant or a fatty acid ester lubricant.
9. An application of a corrosion-resistant bridge pipe box bracket, characterized in that: The corrosion-resistant bridge pipe box bracket is prepared by the preparation method described in any one of claims 1 to 8, and the corrosion-resistant bridge pipe box bracket is used to support and fix the pipeline facilities on the bridge.