Epoxy resin composition for high-voltage insulator pouring as well as preparation method and application of epoxy resin composition
Through the epoxy resin composition with a specific ratio, the problems of insufficient brittleness and heat resistance of the epoxy resin cured product are solved, and a high-pressure insulator filling material with excellent mechanical properties and long-term strength stability are formed, which is suitable for medium and high-pressure equipment.
Patent Information
- Application Number
- CN202411224831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
The cured epoxy resins have problems such as high brittleness, insufficient toughness, poor heat aging resistance, poor low temperature properties and easy cracking, which affects its application in high-pressure insulator filling.
Specific raw material ratios are adopted, including bisphenol A type epoxy resin, low viscosity phenolic epoxy resin, aromatic low viscosity active diluent, alumina, vapor phase silica, liquid anhydride, solid anhydride, high temperature stabilizer and The toughener forms a high-pressure insulator infusion epoxy resin composition through specific mixing and curing conditions, reducing the crosslinking density and forming an effective three-dimensional network structure.
It improves the mechanical properties, toughness and heat resistance of the composition, is suitable for insulating materials for medium and high-voltage equipment, has excellent mechanical properties and long-term strength stability, and is suitable for insulators, medium-voltage switches and other components.
Smart Images

Figure BDA0005024130020000021 
Figure BDA0005024130020000022 
Figure BDA0005024130020000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulator potting materials, and more specifically to an epoxy resin composition for high-voltage insulator potting and a preparation method thereof. Background Art
[0002] With the comprehensive development of my country's high-voltage flexible transmission technology, epoxy resin potting has entered a golden age along with the development of insulating materials. The potting of high-voltage insulators mainly adopts epoxy potting with good insulating properties. The epoxy resin used has excellent mechanical properties and long-term strength stability, and is superior in high-temperature environment resistance. Its insulation, thermal stability and crack resistance are one of the key factors to ensure the safety and stability of insulators.
[0003] Since the epoxy resin molecular structure contains unique active groups and polar groups such as epoxy groups, hydroxyl groups and ether bonds, epoxy resin cured products have good dielectric properties, mechanical properties, bonding properties and corrosion resistance. Its cured products have small shrinkage and linear expansion coefficients, stable dimensions and good processability. In addition, due to the flexibility and diversity of epoxy resin formula design, it can be obtained to meet almost all performance requirements and can be processed into coatings, composite materials and adhesives, etc. It is widely used in various fields such as anti-corrosion coatings, electrical insulation, wind blades, new energy vehicles, photovoltaic power generation, military industry, aerospace, etc.
[0004] However, epoxy resin cured products are spatial three-dimensional network structures with a high degree of cross-linking. The molecular chains are not easy to slide and have large internal stress. After curing, they are generally brittle, lack toughness, have poor heat aging resistance, poor low-temperature resistance, and are prone to cracking. Summary of the invention
[0005] Based on the above technical problems existing in the prior art, one of the purposes of the present invention is to provide an epoxy resin composition for high-voltage insulation potting, which adopts a specific raw material ratio so that the composition has higher mechanical properties and heat resistance.
[0006] In order to achieve the above object, the technical solution of the present invention is as follows:
[0007] An epoxy resin composition for high-voltage insulator potting includes a component A and a component B. The raw materials of the component A include, by weight:
[0008]
[0009] The raw materials of the B component include, by weight:
[0010]
[0011] In some embodiments, the bisphenol A epoxy resin has an epoxy equivalent of 170 g / eq to 210 g / eq, and an average viscosity of the bisphenol A epoxy resin at 25° C. is less than 12,000 mPa·s. Preferably, the bisphenol A epoxy resin is at least one of CYD-128, CYD-127, and E39D.
[0012] In some embodiments, the low viscosity novolac epoxy resin has an epoxy equivalent of 160 g / eq to 180 g / eq, and a viscosity of the low viscosity novolac epoxy resin at 25° C. of 3,500 to 6,000 mPa·s.
[0013] In some embodiments, the active diluent is an aromatic glycidyl ether diluent; preferably, it is at least one of phenol glycidyl ether, cresol glycidyl ether, p-tert-butylphenol glycidyl ether, phenylphenol glycidyl ether, and resorcinol diglycidyl ether.
[0014] In some embodiments, the coupling agent is KH560.
[0015] In some embodiments, the alumina is electrical grade with an average particle size of 100 to 2,000 mesh.
[0016] In some embodiments, the thixotropic agent is fumed silica.
[0017] In some embodiments, the first curing agent is at least one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, and methylnadic anhydride.
[0018] In some embodiments, the second curing agent is at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride, and nadic anhydride.
[0019] In some embodiments, the high temperature stabilizer is at least one of 2,6-di-tert-butyl-p-cresol (BHT) and neopentyl glycol (NPG).
[0020] In some embodiments, the toughening agent is a polyether polyol having an average viscosity of less than 450 mPa·s at 25° C. and a hydroxyl value of less than 550 mgKOH / g; preferably, the polyether polyol is a polymer of polyethylene glycol and polypropylene glycol, and preferably at least one of DE-200, DE-300, DE-400, DE-600, DP-200, DP-400, DP-410, DP-450, DP-500, DP-750, DP-1000, DP-2000, DP-200, and DP-400 of Guodu Chemical.
[0021] In some embodiments, the first accelerator is at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylbenzylamine and triethylamine.
[0022] In some embodiments, the second accelerator is an acetylacetonate accelerator; preferably, the acetylacetonate accelerator is at least one of aluminum acetylacetonate, chromium acetylacetonate, titanium acetylacetonate, and cobalt acetylacetonate.
[0023] In some embodiments, the mass ratio of the A component to the B component is 100:20-40.
[0024] A second object of the present invention is to provide a method for preparing the epoxy resin polymer for high voltage insulator potting according to any of the above embodiments, the method comprising the following steps:
[0025] (1) Preparation of component A: bisphenol A epoxy resin, low viscosity novolac epoxy resin, reactive diluent and coupling agent are uniformly mixed, and then aluminum oxide and thixotropic agent are added. The mixture is placed in a disperser and heated to high speed for mixing. After cooling to room temperature and vacuum degassing, component A is obtained.
[0026] Preparation of component B: adding the first curing agent, the second curing agent, the high temperature stabilizer, the toughening agent and the first accelerator into a stirring kettle, heating for reaction, cooling to room temperature, adding the second accelerator and vacuum degassing to obtain component B;
[0027] (2) Component A and component B obtained in step (1) are mixed and stirred to obtain the epoxy resin composition for high voltage insulator potting.
[0028] In some embodiments, during the preparation of component A, the mixing temperature is 90-110°C, the high-speed shear dispersion time is 2-4 hours, and the rotation speed is 1000rpm-2000rpm; during the preparation of component B, the heating reaction temperature is 100-120°C, the reaction time is 6-8 hours, and the stirring speed is 500rpm-1000rpm.
[0029] A third object of the present invention is to provide an insulating material, which is obtained by curing the epoxy resin polymer of any of the above embodiments.
[0030] In some embodiments, the curing conditions are: curing at a temperature of 160-200° C. for 4-8 hours, and then curing at a temperature of 100-140° C. for 8-12 hours.
[0031] In some embodiments, the insulating material can be applied to components related to medium and high voltage equipment, including but not limited to indoor electrical insulators, medium voltage switches, bushings, etc.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention uses bisphenol A epoxy resin as a raw material, and cooperates with low-viscosity phenolic epoxy resin and aromatic low-viscosity active diluent, so that the composition has excellent strength and toughness, and the resin has a large number of active hydroxyl groups, which is conducive to improving the heat resistance and crack resistance of the composition; then liquid anhydride and solid anhydride are used as the main curing agent, and a certain thermal stabilizer and toughening agent are used, while reducing the cost of raw materials, the crosslinking density of the epoxy resin cured product can be greatly reduced, its cohesion can be reduced, and the temperature shock resistance of the composition can be improved. In addition, through the specific ratio of bisphenol A epoxy resin, low-viscosity phenolic epoxy resin, aromatic low-viscosity active diluent and liquid anhydride, solid anhydride, high-temperature stabilizer and toughening agent, and then with different compositions of the first accelerator and the second accelerator, an effective three-dimensional network structure is formed, and the toughening agent can further form an effective IPN toughening effect with the epoxy resin, which can further improve the toughness and strength, so that the obtained high-voltage insulator infusion epoxy resin composition has excellent mechanical properties and long-term strength stability, and excellent high temperature environment resistance performance.
[0034] In addition, the insulating material obtained by curing the polyurethane composition of the present invention under specific curing conditions exhibits excellent mechanical properties and can be widely used in components of medium and high voltage equipment, including but not limited to insulators, medium voltage switches, bushings, etc. DETAILED DESCRIPTION
[0035] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0037] Example 1
[0038] An epoxy resin composition for high-voltage insulator potting comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 100:20; wherein:
[0039] The raw materials of component A include the following components by weight:
[0040]
[0041] The raw materials of component B include the following components by weight:
[0042]
[0043]
[0044] In this embodiment, the preparation of component A and component B includes the following steps:
[0045] (1) CYD-128, low viscosity phenolic epoxy resin and phenol glycidyl ether were mixed at 90° C., 0.5 parts of KH560, 150 parts of 100-mesh alumina and 1 part of fumed silica were added, and the mixture was added to a disperser and mixed and dispersed at 1000 rpm for 2 h. The mixture was cooled to room temperature and vacuum degassed to obtain component A;
[0046] (2) adding methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, 2,6-di-tert-butyl-p-cresol (BHT), polyether polyol DP-400 and DMP-30 into a stirred tank and heating at 100° C. for 6 h, cooling to room temperature, adding aluminum acetylacetonate and vacuum degassing to obtain composition B;
[0047] (3) Accurately weigh 100 g of component A prepared in step (1) and 20 g of component B prepared in step (2), stir for 20 min to mix evenly, and then degas and cure to obtain an epoxy resin composition; the properties of the epoxy resin composition are tested, and the test results are shown in Table 1.
[0048] Example 2
[0049] An epoxy resin composition for high-voltage insulator potting comprises component A and component B in a mass ratio of 100:40; wherein:
[0050] Component A includes the following components by weight:
[0051]
[0052]
[0053] Component B is mainly composed of the following components in parts by mass:
[0054]
[0055] In this embodiment, the preparation of component A and component B includes the following steps:
[0056] (1) CYD-127, low viscosity novolac epoxy resin and cresol glycidyl ether were mixed uniformly at 110° C., KH560, 300 parts of 2,000 mesh alumina and fumed silica were added, and the mixture was added to a disperser and mixed and dispersed at 2,000 rpm for 4 hours. The mixture was cooled to room temperature and vacuum degassed to obtain component A;
[0057] (2) adding methyl hexahydrophthalic anhydride, hexahydrophthalic anhydride and neopentyl glycol (NPG), 20 parts of polyether polyol DP-2000 and N,N-dimethylbenzylamine into a stirred tank, heating at 120° C. for 8 hours, cooling to room temperature, adding chromium acetylacetonate and vacuum degassing to obtain composition B;
[0058] (3) Accurately weigh 100 g of the component A prepared in the above step (1) and 40 g of the component B prepared in the above step (2), stir for 20 min to mix evenly, and then degas and cure to obtain an epoxy resin composition; the properties of the epoxy resin composition are tested, and the test results are shown in Table 1.
[0059] Example 3
[0060] An epoxy resin composition for high-voltage insulator potting comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 100:30; wherein:
[0061] The raw materials of component A include the following components by weight:
[0062]
[0063] The raw materials of component B include the following components by weight:
[0064]
[0065] In this embodiment, the preparation of component A and component B includes the following steps:
[0066] (1) E-39D, low viscosity phenolic epoxy resin and resorcinol diglycidyl ether were mixed uniformly at 100° C., KH560, 1000 mesh alumina and fumed silica were added, and the mixture was added to a disperser for mixing and dispersing at 1500 rpm for 3 h. The mixture was cooled to room temperature and vacuum degassed to obtain component A;
[0067] (2) adding methyl nadic anhydride, nadic anhydride and 2,6-di-tert-butyl-p-cresol (BHT), neopentyl glycol (NPG), polyether polyol DE-600 and triethylamine into a stirred tank, heating at 110° C. for 7 h, cooling to room temperature, adding cobalt acetylacetonate and vacuum degassing to obtain composition B;
[0068] (3) Accurately weigh 100 g of the component A prepared in the above step (1) and 30 g of the component B prepared in the above step (2), stir for 20 min to mix evenly, and then degas and cure to obtain an epoxy resin composition; the properties of the epoxy resin composition are tested, and the test results are shown in Table 1.
[0069] Table 1 Performance test results of the epoxy resin composition for high voltage insulator potting obtained in each embodiment
[0070]
[0071]
[0072] It can be seen from Table 1 that under different processing conditions, the epoxy resin compositions for high-voltage insulator potting prepared in Examples 1-3 of the present invention have good mechanical strength and insulation properties, can be widely used in the manufacture of indoor electrical insulators, medium-voltage switches, bushings and other insulating parts, are suitable for insulation potting of medium- and high-voltage equipment switches and other components, and have the advantages of simple preparation, high use value and good application prospects.
[0073] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0074] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An epoxy resin composition for high voltage insulator potting, characterized in that: It comprises component A and component B, wherein the raw materials of component A are calculated by weight and include: The raw materials of the B component include, by weight:
2. The epoxy resin composition for high voltage insulator potting according to claim 1, characterized in that: The bisphenol A epoxy resin has an epoxy equivalent of 170 g / eq to 210 g / eq, and an average viscosity of the bisphenol A epoxy resin at 25° C. is less than 12,000 mPa·s.
3. The epoxy resin composition for high voltage insulator potting according to claim 1, characterized in that: The low-viscosity novolac epoxy resin has an epoxy equivalent of 160 g / eq to 180 g / eq, and a viscosity of the low-viscosity novolac epoxy resin at 25° C. of 3,500 to 6,000 mPa·s.
4. The epoxy resin composition for high voltage insulator potting according to claim 1, characterized in that: The active diluent is an aromatic glycidyl ether diluent; and / or, the coupling agent is KH560; and / or, the alumina is electrical grade with an average particle size of 100 to 2,000 meshes; and / or, the thixotropic agent is fumed silica.
5. The epoxy resin composition for high voltage insulator potting according to claim 1, characterized in that: The first curing agent is at least one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride and methylnadic anhydride; the second curing agent is at least one of tetrahydrophthalic anhydride, hexahydrophthalic anhydride and nadic anhydride.
6. The epoxy resin composition for high voltage insulator potting according to claim 1, characterized in that: The high temperature stabilizer is at least one of 2,6-di-tert-butyl-p-cresol (BHT) and neopentyl glycol (NPG); and / or the toughening agent is a polyether polyol having an average viscosity of less than 450 mPa·s and a hydroxyl value of less than 550 mgKOH / g at 25° C.; and / or the first accelerator is at least one of 2,4,6-tris(dimethylaminomethyl)phenol, N,N-dimethylbenzylamine and triethylamine; and / or the second accelerator is an acetylacetonate accelerator.
7. The method for preparing the epoxy resin composition for high voltage insulator potting according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Preparation of component A: bisphenol A epoxy resin, low viscosity novolac epoxy resin, reactive diluent and coupling agent are uniformly mixed, and then aluminum oxide and thixotropic agent are added. The mixture is placed in a disperser and heated to high speed for mixing. After cooling to room temperature and vacuum degassing, component A is obtained. Preparation of component B: adding the first curing agent, the second curing agent, the high temperature stabilizer, the toughening agent and the first accelerator into a stirring kettle, heating for reaction, cooling to room temperature, adding the second accelerator and vacuum degassing to obtain component B; (2) Component A and component B obtained in step (1) are mixed and stirred to obtain the epoxy resin composition for high voltage insulator potting.
8. The method for preparing the epoxy resin composition for high voltage insulator potting according to claim 7, characterized in that: In step (1), during the preparation of component A, the mixing temperature is 90-110° C., the high-speed shear dispersion time is 2-4 h, and the rotation speed is 1000 rpm-2000 rpm; during the preparation of component B, the heating reaction temperature is 100-120° C., the reaction time is 6-8 h, and the stirring speed is 500 rpm-1000 rpm.
9. An insulating material, characterized in that: The epoxy resin composition according to any one of claims 1 to 6 is cured.
10. The insulating material according to claim 9, characterized in that The curing conditions are: curing at a temperature of 160-180°C for 4-8 hours, and then curing at a temperature of 100-140°C for 8-12 hours.
Citation Information
Cited By
High-toughness low-viscosity epoxy resin and preparation method thereof
CN121427256A
Heat-resistant high-insulation VPI impregnating resin as well as preparation method and application thereof
CN122188340A