Polymer foam with bimodal cellular structure and preparation method thereof

By introducing poor compatibility nucleating agents and elastomers to control the distribution of nucleating agents, the directional design of polymer foam with bimodal cell structure and the preparation of one-step foaming method are realized, and the complex process in the prior art is solved and the problem of low production efficiency meets the needs of different pore sizes and is suitable for large-scale production.

CN118994884AActive Publication Date: 2024-11-22NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202411361618.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-22
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

In the prior art, polymer foams that prepare bimodal cell structures have complex processes and low production efficiency, which cannot meet the needs of different pore sizes.

Method used

By introducing a nucleating agent with poor compatibility with the elastomer, the average particle size, content and distribution of the nucleating agent are controlled, and the orientation design of the bimodal pore structure is achieved. A one-step foaming method is used to prepare a bimodal pore structure with a bimodal pore structure polymer foam.

Benefits of technology

The pore size control of polymer foam is achieved, meets different application needs, has a simple process and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994884A_ABST
    Figure CN118994884A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer foam with a bimodal cellular structure, the main raw materials comprise a nucleating agent and an elastomer, the nucleating agent is an alloy formed by one simple substance, a metal oxide or a plurality of simple substances of gallium, mercury, indium, tin, copper, iron, calcium, magnesium, barium, nickel, cobalt, lead and bismuth, the elastomer is at least one of thermoplastic polyurethane, ethylene vinyl acetate, a thermoplastic polyester elastomer, polyether block polyamide, a styrene-ethylene-butylene-styrene block copolymer, an ethylene-octene copolymer, ethylene propylene diene monomer, natural rubber, silicone rubber and nitrile rubber, and the average particle size of the nucleating agent is 1-500 [mu] m. The content of the nucleating agent is not more than 15 vol%. By controlling the particle size and content of the nucleating agent, the pore diameter of the polymer foam is regulated and controlled, different application requirements are met, and the application range is wide. The invention also discloses a preparation method of the polymer foam with the bimodal cellular structure, and the preparation method is simple in process and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer foams, and in particular to a polymer foam with a bimodal pore structure and a preparation method thereof. Background Art

[0002] Bimodal pore structure polymer foam is a foam material with a bimodal pore size distribution. Due to its unique microstructure, it has been widely used in the industrial field. Compared with traditional foam materials with uniform pore structure, polymer microfoam with bimodal pore structure exhibits superior physical and mechanical properties by forming a dual structure combining large pores and small pores inside the material. Large pores help to reduce the weight of the material and improve the energy absorption effect of the material, while small pores can improve the structural strength and thermal insulation performance of the material. By optimizing the size distribution of the pores, the foam with a bimodal pore structure can significantly improve its mechanical strength and durability while keeping the material lightweight. In addition, this bimodal pore structure also enables the foam material to exhibit better energy absorption and cushioning performance under dynamic impact loads. Therefore, in application scenarios that require high-performance and multifunctional materials, foam with a bimodal pore structure has become an ideal choice.

[0003] At present, the methods for preparing polymer foams with bimodal pore materials are mainly physical foaming and chemical foaming. The physical foaming method first allows the gas to reach a dissolution equilibrium inside the polymer, and then causes thermodynamic instability of the system by rapid pressure relief or temperature increase, thereby achieving a transition from homogeneous to heterogeneous phases, inducing nucleated pore growth, and finally the polymer forms a porous structure, which includes rapid pressure relief foaming and temperature increase foaming. The chemical foaming method is similar to the physical foaming method, both of which reduce the solubility of the gas in the polymer, then the bubbles nucleate and the pores grow, but the gas source of the chemical foaming is obtained by chemical reactions between different reagents. However, the current preparation methods mostly use a multi-step method to prepare polymer foams with a bimodal pore structure, which is complex in process and low in production efficiency, which limits the large-scale application of polymer foams with a bimodal pore structure.

[0004] Publication No. CN105385024A discloses a polypropylene foam with bimodal distribution and a preparation method thereof, wherein the polypropylene foam with bimodal distribution is composed of porous inorganic particles and a matrix resin, and has large pores with an average diameter of 15 μm-50 μm and small pores with an average diameter of 1 μm-10 μm, wherein the porous inorganic particles are a mixture of one or more of activated carbon, porous alumina, porous silica gel, molecular sieve, and porous silica. However, the pore sizes of the obtained polypropylene foam are not obviously different, but are relatively close, and cannot meet the requirements of different pore sizes.

[0005] Publication No. CN114702720A discloses a polybutene foam and its preparation method, preform and application. The preparation method includes the following steps: (1) annealing the polybutene resin to obtain a preform; the annealing method includes supercritical CO2 annealing or normal temperature and pressure annealing; supercritical CO2 annealing includes: in the presence of supercritical CO2, the polybutene resin is kept warm and pressurized, and the pressure is released to obtain; the pressure release rate is 0.1-1 MPa / min; normal temperature and pressure annealing includes: melting the polybutene resin, cooling it at normal temperature and pressure to obtain; (2) in the presence of supercritical CO2, the preform is kept warm and pressurized, and the pressure is released to obtain; wherein the pressure release rate is 5-300 MPa / s. However, the polybutene resin needs to be cooled and annealed first, and the process is complicated. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a polymer foam with a bimodal pore structure, into which a nucleating agent with poor compatibility with elastomer is introduced, and by controlling the average particle size, content and distribution of the nucleating agent, the bimodal pore structure can be directional designed.

[0007] A polymer foam with a bimodal pore structure, wherein the main raw materials are composed of a nucleating agent and an elastomer, wherein the nucleating agent is a single substance selected from gallium, mercury, indium, tin, copper, iron, calcium, magnesium, barium, nickel, cobalt, lead, and bismuth, a metal oxide, or an alloy formed by multiple single substances; the elastomer is at least one selected from thermoplastic polyurethane, ethylene vinyl acetate, thermoplastic polyester elastomer, polyether block polyamide, styrene-ethylene-butylene-styrene block copolymer, ethylene octene copolymer, ethylene propylene diene monomer rubber, natural rubber, silicone rubber, and nitrile rubber; the average particle size of the nucleating agent is 1-500 μm, and the content of the nucleating agent does not exceed 15 vol%.

[0008] In the present invention, a nucleating agent is dispersed in an elastomer, and after blending and foaming, a polymer foam having a bimodal cell structure is obtained. For a nucleating agent with a flat surface, due to the poor compatibility between the nucleating agent and the elastomer, there is an obvious interface between the two, and the existence of this interface will significantly reduce the Gibbs free energy barrier required to be overcome for bubble nucleation. For a nucleating agent with an uneven surface and a structure with many bumps and depressions, microcavities exist on the surface of the nucleating agent particles, and bubbles are more likely to be generated in these microcavities and weakly bonded places on the solid-solid interface.

[0009] During physical or chemical foaming, bubble nucleation occurs preferentially on the surface of the nucleating agent, and heterogeneous nucleation occurs at the site of the nucleating agent. The presence of heterogeneous nucleation sites does not exclude homogeneous nucleation, and homogeneous nucleation can also occur in areas far away from the influence of heterogeneous nucleation points. The bubbles of heterogeneous nucleation occurring at the nucleating agent site are larger than those of homogeneous nucleation. The bubbles of heterogeneous nucleation grow into large pores, and the bubbles of homogeneous nucleation in the matrix grow into small pores. After foaming, a polymer foam with a bimodal pore structure is obtained.

[0010] In the present invention, homogeneous nucleation and heterogeneous nucleation can occur simultaneously after the nucleating agent and the elastomer are mixed. By adjusting the proportion of the nucleating agent in the elastomer, the size of the bimodal pores can be directionally designed. When the proportion of the nucleating agent increases, the pore sizes of the obtained polymer foam gradually approach each other, and a polymer foam with a uniform pore structure will be formed. Therefore, when the proportion of the nucleating agent does not exceed 15%, the internal pore structure of the obtained polymer foam shows a significant coexistence of large and small pores.

[0011] Preferably, the nucleating agent is a gallium-indium-tin alloy, the elastomer is a thermoplastic polyurethane, and the content of the nucleating agent does not exceed 10 vol%.

[0012] Preferably, the gallium indium tin alloy is dispersed in the thermoplastic polyurethane as a nucleating agent, and the compatibility between the two is poor. During physical or chemical foaming, bubble nucleation occurs preferentially on the surface of the gallium indium tin alloy, and heterogeneous nucleation occurs at the site of the gallium indium tin alloy. When the gallium indium tin alloy accounts for no more than 10 vol%, the obtained polymer foam has a clear difference in pore size and has a clear bimodal pore structure.

[0013] Preferably, the nucleating agent is copper, the elastomer is thermoplastic polyurethane, the average particle size of the nucleating agent is 1-100 μm, and the content of the nucleating agent does not exceed 10 vol%.

[0014] Preferably, in the polymer foam having a bimodal pore structure, the pore diameter of large pores is between 40-1000 μm, the pore diameter of small pores is between 1-100 μm, and the large pores account for 5-90%.

[0015] The present invention also provides a method for preparing a polymer foam with a bimodal pore structure. The polymer foam with a bimodal pore structure is prepared by one-step foaming, and the process is simple and suitable for large-scale production.

[0016] A method for preparing a polymer foam having a bimodal pore structure comprises the following steps:

[0017] (1) uniformly mixing the elastomer and the nucleating agent to obtain a composite material;

[0018] (2) The composite material obtained in step (1) is subjected to a physical foaming method or a chemical foaming method to prepare a polymer foam having a bimodal pore structure.

[0019] Preferably, the physical foaming method is a temperature rising foaming method or a rapid pressure relief foaming method.

[0020] Further preferably, the temperature-increasing foaming method comprises the steps of subjecting the composite material obtained in step (1) to room temperature saturation treatment in a high-pressure fluid, immersing the composite material in heated glycerol, and cooling and shaping the composite material to obtain a polymer foam having a bimodal pore structure.

[0021] Preferably, at room temperature, the composite material obtained by blending the elastomer and the nucleating agent is saturated and immersed in heated glycerol. As the temperature rises suddenly, the entire system quickly becomes an oversaturated system, the gas dissolved in the composite material is concentrated to form nuclei, and the gas molecules begin to gradually diffuse to the nucleus, causing the pores to grow, thereby obtaining a polymer foam with a bimodal pore structure.

[0022] More preferably, the glycerol temperature is 100-160° C., and the soaking time is 5-30 seconds.

[0023] The temperature and immersion time of glycerol are the foaming temperature and foaming time of the polymer foam respectively. When the foaming temperature increases and the foaming time prolongs, the surface tension of the elastomer decreases and the bubbles grow more easily. Therefore, the pore size of the macropores in the foam increases, the foaming ratio increases, and the density of the polymer foam decreases.

[0024] Further preferably, the rapid pressure relief method comprises saturating the composite material obtained in step (1) in a high-pressure fluid, and after saturation, rapidly releasing the pressure, cooling and shaping to obtain a polymer foam having a bimodal pore structure.

[0025] More preferably, the saturation temperature is 120-160° C., the saturation pressure is 10-16 MPa, and the saturation time is 0.5-1 h.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) In the present invention, metal, metal oxide or alloy is introduced as a nucleating agent. Due to the difference in compatibility between the nucleating agent and the elastomer, homogeneous nucleation and heterogeneous nucleation can occur simultaneously, and after foaming, a polymer foam with a bimodal pore structure can be obtained;

[0028] (2) In the present invention, the particle size and content of the nucleating agent are controlled to achieve pore size control of the polymer foam, thereby meeting different application requirements and having a wide range of applications;

[0029] (3) The method adopted in the present invention is a conventional physical foaming method and a chemical foaming method, both of which only require one step of foaming to prepare a polymer foam with a bimodal pore structure, and the process is simple and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a scanning electron microscope (SEM) image of the polymer foam with a bimodal pore structure obtained in Example 1.

[0031] Figure 2 This is a cell size distribution diagram of the polymer foam with a bimodal cell structure obtained in Example 1.

[0032] Figure 3 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 2.

[0033] Figure 4 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 3.

[0034] Figure 5 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 4.

[0035] Figure 6 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 5.

[0036] Figure 7 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 6.

[0037] Figure 8 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 7.

[0038] Fig. 9 This is a SEM image of the polymer foam with a bimodal cell structure obtained in Example 8.

[0039] Fig.10 This is the SEM image of the polymer foam obtained in Comparative Example 1. DETAILED DESCRIPTION

[0040] The present invention will be further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited to the following examples.

[0041] The raw materials used in the present invention are all commercially available.

[0042] Example 1

[0043] (1) 35.7984 g of thermoplastic polyurethane (BASF, brand 1190A) was dissolved in 100.24 mL of dimethylacetamide to obtain a thermoplastic polyurethane solution. 0.32 mL of gallium indium tin alloy (Ga68.5In21.5Sn10) with an average particle size of 17 μm was taken and mixed evenly with the thermoplastic polyurethane solution. The mixture was poured into a mold, and the dimethylacetamide solution was removed by vacuum to obtain a thermoplastic polyurethane / gallium indium tin alloy composite material with a thickness of 1.1 mm, wherein the content of the gallium indium tin alloy was 1 vol%.

[0044] (2) The thermoplastic polyurethane / gallium indium tin alloy composite material obtained in step (1) was placed in an autoclave for saturation treatment, with a saturation pressure of 4 MPa, a saturation temperature of 23° C., and a saturation time of 48 h. The saturated sample was immersed in glycerol at 150° C. for 25 seconds, and the pores were quickly cooled with water to obtain a polymer foam with a bimodal pore structure. The scanning electron microscope (SEM) image of the polymer foam is shown in FIG. Figure 1 shown.

[0045] like Figure 1 As shown, the internal cell structure of the polymer foam shows the coexistence of large and small cells.

[0046] Figure 2 The cell size distribution diagram of the polymer foam with a bimodal cell structure obtained in Example 1 is as follows: Figure 2 As shown, the polymer foam obtained in Example 1 has a bimodal pore structure, the average pore size of large pores is 99.36 μm, the average pore size of small pores is 11.53 μm, and the large pores account for 49%.

[0047] Example 2

[0048] The preparation process is the same as that of Example 1, except that the content of the gallium-indium-tin alloy is 5 vol%. The scanning electron microscope (SEM) image of the obtained polymer foam with a bimodal cell structure is as follows: Figure 2 The polymer foam obtained in Example 2 has a bimodal cell structure, the average cell size of large cells is 87.35 μm, the average cell size of small cells is 14.82 μm, and the large cells account for 75%.

[0049] Example 3

[0050] The preparation process is the same as that of Example 1, except that the saturated sample is immersed in glycerol at 150°C for 8 seconds. The scanning electron microscope (SEM) image of the obtained polymer foam with a bimodal pore structure is as follows: Figure 3 The polymer foam obtained in Example 3 has a bimodal cell structure, the average cell size of large cells is 61.73 μm, the average cell size of small cells is 12.12 μm, and the large cells account for 49%.

[0051] Example 4

[0052] The preparation process is the same as that of Example 1, except that the saturated sample is immersed in glycerol at 130°C for 25 seconds. The scanning electron microscope (SEM) image of the obtained polymer foam with a bimodal pore structure is as follows: Figure 4 The polymer foam obtained in Example 4 has a bimodal cell structure, the average cell size of large cells is 58.13 μm, the average cell size of small cells is 12.32 μm, and the large cells account for 46%.

[0053] Example 5

[0054] (1) 20 g of thermoplastic polyurethane and 3.2220 g of copper powder with an average particle size of 40 μm were mixed uniformly by an internal mixer, and the mixed materials were pressed into a thermoplastic polyurethane / copper composite material with a thickness of 1.1 mm, wherein the copper content was 2 vol%.

[0055] (2) The thermoplastic polyurethane / copper composite material obtained in step (1) is placed in an autoclave for saturation treatment, with a saturation pressure of 4 MPa, a saturation temperature of 23° C., and a saturation time of 48 h. The saturated sample is immersed in glycerol at 150° C. for 25 seconds, and the pores are quickly cooled with water to form a polymer foam with a bimodal pore structure. The scanning electron microscope (SEM) image of the polymer foam is as follows: Figure 5 The polymer foam obtained in Example 5 has a bimodal cell structure, the average cell size of large cells is 98.15 μm, the average cell size of small cells is 35.62 μm, and the large cells account for 60%.

[0056] Example 6

[0057] (1) 35.7984 g of thermoplastic polyurethane was dissolved in 100.24 mL of dimethylacetamide to obtain a thermoplastic polyurethane solution. 0.32 mL of gallium indium tin alloy (Ga68.5In21.5Sn10) with an average particle size of 17 μm was mixed evenly with the thermoplastic polyurethane solution, poured into a mold, and the dimethylacetamide solution was removed by vacuum to obtain a thermoplastic polyurethane / gallium indium tin alloy composite material with a thickness of 1.1 mm, wherein the content of the gallium indium tin alloy was 1 vol%.

[0058] (2) The thermoplastic polyurethane / gallium indium tin alloy composite material obtained in step (1) is placed in an autoclave for saturation treatment, with a saturation pressure of 12 MPa, a saturation temperature of 140° C., and a saturation time of 30 min. The saturated sample is quickly depressurized within 2 seconds, and a polymer foam having a bimodal pore structure is obtained after cooling and shaping. The scanning electron microscope (SEM) image of the obtained polymer foam having a bimodal pore structure is as follows: Figure 6The polymer foam obtained in Example 6 has a bimodal cell structure, the average cell size of large cells is 56.36 μm, the average cell size of small cells is 11.29 μm, and the large cells account for 9%.

[0059] Example 7

[0060] The preparation process is the same as that of Example 6, except that the content of the gallium-indium-tin alloy is 5 vol%. The scanning electron microscope (SEM) image of the obtained polymer foam with a bimodal cell structure is as follows: Figure 7 The polymer foam obtained in Example 7 has a bimodal cell structure, the average cell size of large cells is 45.52 μm, the average cell size of small cells is 6.67 μm, and the large cells account for 35%.

[0061] Example 8

[0062] The preparation process is the same as that of Example 6, except that the content of the gallium-indium-tin alloy is 10 vol%. The scanning electron microscope (SEM) image of the obtained polymer foam with a bimodal cell structure is as follows: Figure 8 The polymer foam obtained in Example 8 has a bimodal cell structure, the average cell size of large cells is 54.60 μm, the average cell size of small cells is 12.60 μm, and the large cells account for 68%.

[0063] Comparative Example 1

[0064] The preparation process is the same as that of Example 1, except that no nucleating agent is added.

[0065] (1) 10 g of thermoplastic polyurethane was dissolved in 28 mL of dimethylacetamide to obtain a thermoplastic polyurethane solution. The thermoplastic polyurethane solution was poured into a mold, and the dimethylacetamide solution was removed by vacuum to obtain a thermoplastic polyurethane material with a thickness of 1.1 mm.

[0066] (2) The thermoplastic polyurethane / gallium indium tin alloy composite material obtained in step (1) was placed in an autoclave for saturation treatment, with a saturation pressure of 4 MPa, a saturation temperature of 23° C., and a saturation time of 48 h. The saturated sample was immersed in glycerol at 150° C. for 25 seconds, and a polymer foam was obtained after cooling and shaping. The scanning electron microscope (SEM) image of the polymer foam is shown in FIG. Fig. 9 shown.

[0067] Fig. 9 This is a scanning electron microscope image of the polymer foam obtained in Comparative Example 1. Since no nucleating agent is added, the polymer foam obtained by the temperature rising foaming method presents a uniform single-peak cell structure, and the average cell size is 24.58 μm.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polymer foam with a bimodal cell structure, the main raw materials of which are composed of a nucleating agent and an elastomer, characterized in that: The nucleating agent is a single substance selected from gallium, mercury, indium, tin, copper, iron, calcium, magnesium, barium, nickel, cobalt, lead, and bismuth, a metal oxide, or an alloy formed by multiple single substances; the elastomer is at least one selected from thermoplastic polyurethane, ethylene vinyl acetate, thermoplastic polyester elastomer, polyether block polyamide, styrene-ethylene-butylene-styrene block copolymer, ethylene octene copolymer, ethylene propylene diene monomer rubber, natural rubber, silicone rubber, and nitrile rubber; the average particle size of the nucleating agent is 1-500 μm, and the content of the nucleating agent does not exceed 15 vol%.

2. The polymer foam having a bimodal cell structure according to claim 1, characterized in that The nucleating agent is gallium-indium-tin alloy, the elastomer is thermoplastic polyurethane, and the content of the nucleating agent does not exceed 10 vol%.

3. The polymer foam having a bimodal cell structure according to claim 1, characterized in that The nucleating agent is copper, the elastomer is thermoplastic polyurethane, the average particle size of the nucleating agent is 1-100 μm, and the content of the nucleating agent does not exceed 10 vol%.

4. The polymer foam having a bimodal cell structure according to claim 1, characterized in that In the polymer foam with a bimodal pore structure, the pore diameter of large pores is 40-1000 μm, the pore diameter of small pores is 1-100 μm, and the proportion of large pores is 5-90%.

5. The method for preparing a polymer foam having a bimodal pore structure according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing the elastomer and the nucleating agent uniformly to obtain a composite material; (2) The composite material obtained in step (1) is subjected to a physical foaming method or a chemical foaming method to prepare a polymer foam having a bimodal pore structure.

6. The method for preparing a polymer foam according to claim 5, characterized in that: The physical foaming method is a temperature-raising foaming method or a rapid pressure-releasing foaming method.

7. The method for preparing a polymer foam according to claim 6, characterized in that: The steps of the temperature-increasing foaming method are as follows: subjecting the composite material obtained in step (1) to room temperature saturation treatment in a high-pressure fluid, immersing it in heated glycerol, and cooling and shaping it to obtain a polymer foam with a bimodal pore structure.

8. The method for preparing a polymer foam according to claim 7, characterized in that: The glycerin temperature is 100-160° C., and the soaking time is 5-30 seconds.

9. The method for preparing a polymer foam according to claim 6, characterized in that: The rapid pressure relief method comprises the steps of saturating the composite material obtained in step (1) in a high-pressure fluid, and after saturation, rapidly releasing the pressure, cooling and shaping to obtain a polymer foam with a bimodal pore structure.

10. The method for preparing a polymer foam having a bimodal cell structure according to claim 9, characterized in that: The saturation temperature is 120-160° C., the saturation pressure is 10-16 MPa, and the saturation time is 0.5-1 h.

Citation Information

Patent Citations

  • Bimodal distribution type polypropylene foaming material and preparing method thereof

    CN105385024A

  • Polybutylene foaming material and preparation method, prefabricated product and application thereof

    CN114702720A

  • Continuous process for making polyetherimide foam materials and articles made therefrom

    CN101952096A

  • PE (Poly Ethylene) foaming material and preparation method thereof

    CN107141564A

  • Polymer microcellular foaming material with bimodal pore structure, and preparation method thereof

    CN108997666A